Preparation method of moisture absorption and sweat releasing knitted fabric

The method of using sodium dodecyl sulfate and sodium carbonate to open cotton yarn pores, combined with additional treatments, enhances the moisture-wicking and perspiration-removal performance of cotton fabrics by improving porosity and maintaining structural integrity, addressing the issues of slow moisture conduction and storage in pure cotton fabrics.

CN119083167APending Publication Date: 2024-12-06ZHEJIANG SIRIS TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411071834.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Pure cotton fabrics exhibit poor moisture-wicking performance and moisture-heat exchange under hot and humid conditions, leading to discomfort due to slow moisture conduction and storage, which affects the moisture and heat exchange between the human body and the environment.

Method used

A method involving constant-temperature steaming with sodium dodecyl sulfate and sodium carbonate to open cotton yarn pores, followed by treatments with BASF Lufibrol MSD, BASF Kieralon F-MFB, glacial acetic acid, a waterproofing agent, and a cross-linking agent to enhance porosity and form a stable waterproof structure on the cotton yarn.

Benefits of technology

The method significantly improves the moisture-wicking and perspiration-removal performance of cotton fabrics by enhancing porosity and maintaining pore structure integrity, resulting in faster moisture absorption and evaporation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of fabrics, and particularly relates to a preparation method of a moisture-absorbing and sweat-releasing knitted fabric, which comprises the following steps: homogenizing pores of cotton yarns in a manner of matching cooking with a dispersing agent, pre-treating the inner and outer surfaces of the cotton yarns in a manner of matching pre-boiling-off and acidification, and reacting with a waterproof agent and a cross-linking agent to achieve modification treatment of the cotton yarns, so that the moisture-absorbing and sweat-releasing knitted fabric is obtained. Finally, the cotton yarn is woven, scoured, bleached, dyed and shaped, and the moisture-absorbing and sweat-releasing knitted fabric is obtained. The problems that an existing fabric is poor in moisture removal performance and unsmooth in moisture and heat exchange are solved, constant-temperature cooking of lauryl sodium sulfate and sodium carbonate is used in cooperation with cooking pretreatment, monofilament pores of cotton yarn are effectively opened, the porosity of the cotton yarn is greatly improved, and therefore the pore structure of the fabric is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabrics, and in particular relates to a method for preparing a moisture absorbing and perspiration wicking knitted fabric. Background Art

[0002] Pure cotton fabrics are comfortable and natural fibers are environmentally friendly, which is in line with the concept of green development. However, under hot and humid conditions, due to the fiber's moisture absorption, expansion and deformation, and the moisture storage itself, the moisture conduction and release speed of pure cotton fabrics is slow, which greatly reduces the moisture absorption and perspiration function of pure cotton fabrics, affects the moisture and heat exchange between human skin and the outside world, and makes the human body feel stuffy. Therefore, the market is in urgent need of a knitted fabric with excellent moisture absorption and perspiration effect. Summary of the invention

[0003] In view of the problems in the prior art, the present invention provides a method for preparing a moisture-absorbing and perspiration-wicking knitted fabric, which solves the problems of poor moisture-wicking performance and poor moisture-heat exchange of the prior fabric. The pores of the cotton yarn monofilaments are effectively opened by constant-temperature steaming of sodium dodecyl sulfate and sodium carbonate in combination with a pre-steaming treatment, thereby greatly improving the porosity of the cotton yarn and thus improving the pore structure of the fabric.

[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0005] A method for preparing a moisture wicking knitted fabric comprises the following steps:

[0006] Step 1, adding cotton yarn to water and boiling for 20-30 minutes, then adding sodium dodecyl sulfate and sodium carbonate and keeping warm for 2-4 hours, filtering and rinsing with hot water for 2-3 times, and drying to obtain pore-dispersed cotton yarn, wherein the bath ratio of the boiling is 1-10, the boiling temperature is 40-60°C, the concentration of the sodium dodecyl sulfate in water is 1-3g / L, the amount of sodium carbonate added is 30-100g / L, the insulation temperature is 90-100°C, the hot water rinsing temperature is 50-70°C; the drying temperature is 100-110°C; in this step, the cotton yarn is completely opened by boiling to promote the expansion of the gap in the cotton yarn, and the cotton yarn is completely opened by the insulation treatment of sodium dodecyl sulfate and sodium carbonate, thereby softening the cotton yarn;

[0007] Step 2, putting cotton yarn into water, and then sequentially adding BASF Lufibrol MSD and BASF Kieralon F-MFB, stirring at a constant temperature for 0.5-1h, cooling to 50°C, draining and drying to obtain pre-scour cotton yarn; the bath ratio of the cotton yarn in water is 1-10, the addition amount of BASF Kieralon F-MFB is 1% of the mass of the cotton yarn, and the addition amount of BASF Lufibrol MSD is 2% of the mass of the cotton yarn;

[0008] Step 3, putting the pre-scouring cotton yarn into water, and adding glacial acetic acid for pickling, and obtaining acidified cotton yarn after rinsing, wherein the bath ratio of the cotton yarn in water is 1-10, the amount of the glacial acetic acid added is 0.3-0.4 g / L, the pickling time is 20-30 min, and the temperature is 50-60° C.; the rinsing is cold water rinsing, and the rinsing temperature is 25-30° C.; this step uses a constant temperature pickling method to directly act glacial acetic acid on the cotton yarn with uniform pore dispersion, thereby achieving excellent surface acidification;

[0009] Step 4, putting the acidified cotton yarn into water, adjusting the pH to 4-5, then adding the waterproofing agent and stirring evenly, after constant temperature circulation for 20-40 minutes, adding the cross-linking agent to react for 10-20 minutes, draining, taking the yarn, and drying; the bath ratio of the acidified cotton yarn in water is 1-10, the pH adjusting agent is acetic acid solution, and the concentration of the acetic acid solution is 0.4-0.6g / L, the waterproofing agent is Smart Repel Hydro CMD, and the amount of the waterproofing agent is 5-7% of the mass of the acidified cotton yarn, the temperature of the constant temperature circulation is 75-80°C, and the cross-linking agent is Phobol XAN, the addition amount is 1% of the cotton yarn mass, the temperature is 80-85°C; in this step, the cotton yarn is placed in a dyeing tank, and an acidic environment is provided by adjusting the pH, and the constant temperature circulation cooking of the waterproofing agent is combined to form a waterproof treatment of the acidified cotton yarn, and the acidified active groups on the surface of the acidified cotton yarn itself can improve the fixation of the waterproofing agent on the surface of the cotton yarn, and the effect of the cross-linking agent on the waterproofing agent is combined to form a stable three-proof system on the surface of the cotton yarn;

[0010] Step 5, weaving the cotton yarn obtained in the above steps at room temperature to obtain a woven fabric, and scouring and bleaching the fabric, then wet-dyeing the scouring and bleaching fabric, and shaping to obtain a moisture-absorbing and perspiration-wicking knitted fabric, scouring and washing is to put the fabric into a scouring and bleaching liquid for a half-bleaching process, the temperature of the half-bleaching process is 100-110°C, the bath ratio is 1-10, the concentration of the scouring agent CSP-T07 in the scouring and bleaching liquid is 2g / L, the concentration of hydrogen peroxide is 5g / L, and the concentration of the chelating agent MAG-L is 3g / L, the shaping is to immerse the fabric at a temperature of 40-50°C and a vehicle speed of 30-50m / min, and then dry and shape it at a temperature of 150-160°C, and the immersion solution contains a fluffy silicone softener TF-4981 with a concentration of 25-35g / L.

[0011] It can be seen from the above description that the present invention has the following advantages:

[0012] 1. The present invention solves the problems of poor moisture removal performance and poor heat and moisture exchange of existing fabrics. The constant temperature cooking of sodium dodecyl sulfate and sodium carbonate is used in combination with pre-cooking treatment to effectively open the pores of the cotton yarn monofilaments, greatly improve the porosity of the cotton yarn, and thus improve the pore structure of the fabric.

[0013] 2. The present invention performs waterproofing treatment on the basis of opening the cotton yarn, and combines the waterproofing agent and the cross-linking agent in a cooking and acidic environment to form an in-situ bond on the surface of the cotton yarn, thereby reducing the decrease in porosity caused by the self-shrinkage of the cotton yarn. DETAILED DESCRIPTION

[0014] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.

[0015] Example 1

[0016] A method for preparing a moisture wicking knitted fabric comprises the following steps:

[0017] Step 1, adding cotton yarn to water and boiling for 20 minutes, then adding sodium dodecyl sulfate and sodium carbonate and keeping warm for 2 hours, filtering and rinsing with hot water twice, and drying to obtain pore-dispersed cotton yarn, wherein the bath ratio of the boiling is 1, the boiling temperature is 40°C, the concentration of the sodium dodecyl sulfate in water is 1g / L, the amount of sodium carbonate added is 30g / L, the insulation temperature is 90°C, the temperature of the hot water rinsing is 50°C; and the temperature of the drying is 100°C;

[0018] Step 2, putting cotton yarn into water, and then sequentially adding BASF Lufibrol MSD and BASF Kieralon F-MFB, stirring at a constant temperature for 0.5h, cooling to 50°C, draining and drying to obtain pre-scour cotton yarn; the bath ratio of the cotton yarn in water is 1, the amount of BASF Kieralon F-MFB added is 1% of the mass of the cotton yarn, and the amount of BASF Lufibrol MSD added is 2% of the mass of the cotton yarn;

[0019] Step 3, putting the pre-scouring cotton yarn into water, and adding glacial acetic acid for pickling, and obtaining acidified cotton yarn after rinsing, wherein the bath ratio of the cotton yarn in water is 1, the amount of the glacial acetic acid added is 0.3 g / L, the pickling time is 20 min, and the temperature is 50° C.; the rinsing is cold water rinsing, and the rinsing temperature is 25° C.;

[0020] Step 4, putting the acidified cotton yarn into water, adjusting the pH to 4, then adding the waterproofing agent and stirring evenly, subjecting to constant temperature circulation for 20 minutes, adding the cross-linking agent to react for 10 minutes, draining the liquid, taking the yarn, and drying; the bath ratio of the acidified cotton yarn in water is 1, the pH adjusting agent is an acetic acid solution, and the concentration of the acetic acid solution is 0.4g / L, the waterproofing agent is SmartRepel Hydro CMD, and the amount of the waterproofing agent is 5% of the mass of the acidified cotton yarn, the temperature of the constant temperature circulation is 75°C, the cross-linking agent is Phobol XAN, the amount added is 1% of the mass of the cotton yarn, and the temperature is 80°C;

[0021] Step 5, weaving the cotton yarn obtained in the above steps at room temperature to obtain a woven fabric, and scouring and bleaching the fabric, then wet-dyeing the scouring and bleaching fabric, and shaping to obtain a moisture-absorbing and perspiration-wicking knitted fabric, scouring and washing is to put the fabric into a scouring and bleaching liquid for a half-bleaching process, the temperature of the half-bleaching process is 100°C, the bath ratio is 1, the concentration of the scouring agent CSP-T07 in the scouring liquid is 2g / L, the concentration of hydrogen peroxide is 5g / L, and the concentration of the chelating agent MAG-L is 3g / L, the shaping is to immerse the fabric at a temperature of 40°C and a vehicle speed of 30m / min, and then dry and shape it at a temperature of 150°C, and the immersion solution contains a fluffy silicone softener TF-4981 at a concentration of 25g / L.

[0022] Example 2

[0023] A method for preparing a moisture wicking knitted fabric comprises the following steps:

[0024] Step 1, adding cotton yarn to water and boiling for 30 minutes, then adding sodium dodecyl sulfate and sodium carbonate and keeping warm for 4 hours, filtering and rinsing with hot water for 3 times, and drying to obtain pore-dispersed cotton yarn, wherein the bath ratio of the boiling is 10, the boiling temperature is 60°C, the concentration of sodium dodecyl sulfate in water is 3g / L, the amount of sodium carbonate added is 100g / L, the insulation temperature is 100°C, the temperature of the hot water rinsing is 70°C; and the temperature of the drying is 110°C;

[0025] Step 2, putting cotton yarn into water, and then sequentially adding BASF Lufibrol MSD and BASF Kieralon F-MFB, stirring at a constant temperature for 1 hour, cooling to 50° C., draining and drying, to obtain pre-scour cotton yarn; the bath ratio of the cotton yarn in water is 10, the addition amount of BASF Kieralon F-MFB is 1% of the mass of the cotton yarn, and the addition amount of BASF Lufibrol MSD is 2% of the mass of the cotton yarn;

[0026] Step 3, putting the pre-scouring cotton yarn into water, and adding glacial acetic acid for pickling, and obtaining acidified cotton yarn after rinsing, wherein the bath ratio of the cotton yarn in water is 10, the amount of the glacial acetic acid added is 0.4 g / L, the pickling time is 30 min, and the temperature is 60° C.; the rinsing is cold water rinsing, and the rinsing temperature is 30° C.;

[0027] Step 4, putting the acidified cotton yarn into water, adjusting the pH to 5, then adding the waterproofing agent and stirring evenly, after constant temperature circulation for 40 minutes, adding the cross-linking agent to react for 20 minutes, draining, taking the yarn, and drying; the bath ratio of the acidified cotton yarn in water is 10, the pH regulator is acetic acid solution, and the concentration of the acetic acid solution is 0.6g / L, the waterproofing agent is SmartRepel Hydro CMD, and the amount of the waterproofing agent is 7% of the mass of the acidified cotton yarn, the temperature of the constant temperature circulation is 80°C, the cross-linking agent is Phobol XAN, the amount added is 1% of the mass of the cotton yarn, and the temperature is 85°C;

[0028] Step 5, weaving the cotton yarn obtained in the above steps at room temperature to obtain a woven fabric, and scouring and bleaching the fabric, then wet-dyeing the scouring and bleaching fabric, and shaping to obtain a moisture-absorbing and perspiration-wicking knitted fabric, scouring and washing is to put the fabric into a scouring and bleaching liquid for a half-bleaching process, the temperature of the half-bleaching process is 110°C, the bath ratio is 10, the concentration of the scouring agent CSP-T07 in the scouring liquid is 2g / L, the concentration of hydrogen peroxide is 5g / L, and the concentration of the chelating agent MAG-L is 3g / L, the shaping is to immerse the fabric at a temperature of 50°C and a vehicle speed of 50m / min, and then dry and shape it at a temperature of 160°C, and the immersion solution contains a fluffy silicone softener TF-4981 at a concentration of 35g / L.

[0029] Example 3

[0030] A method for preparing a moisture wicking knitted fabric comprises the following steps:

[0031] Step 1, adding cotton yarn to water and boiling for 25 minutes, then adding sodium dodecyl sulfate and sodium carbonate and keeping warm for 3 hours, filtering and rinsing with hot water for 3 times, and drying to obtain pore-dispersed cotton yarn, wherein the bath ratio of the boiling is 5, the boiling temperature is 50°C, the concentration of the sodium dodecyl sulfate in water is 2g / L, the amount of sodium carbonate added is 60g / L, the insulation temperature is 95°C, the temperature of the hot water rinsing is 60°C; and the temperature of the drying is 105°C;

[0032] Step 2, putting cotton yarn into water, and then sequentially adding BASF Lufibrol MSD and BASF Kieralon F-MFB, stirring at a constant temperature for 1 hour, cooling to 50° C., draining and drying to obtain pre-scour cotton yarn; the bath ratio of the cotton yarn in water is 5, the addition amount of BASF Kieralon F-MFB is 1% of the mass of the cotton yarn, and the addition amount of BASF Lufibrol MSD is 2% of the mass of the cotton yarn;

[0033] Step 3, putting the pre-scouring cotton yarn into water, and adding glacial acetic acid for pickling, and obtaining acidified cotton yarn after rinsing, wherein the bath ratio of the cotton yarn in water is 5, the amount of the glacial acetic acid added is 0.4 g / L, the pickling time is 25 min, and the temperature is 55° C.; the rinsing is cold water rinsing, and the rinsing temperature is 30° C.;

[0034] Step 4, putting the acidified cotton yarn into water, adjusting the pH to 4, then adding the waterproofing agent and stirring evenly, subjecting to constant temperature circulation for 30 minutes, adding the cross-linking agent to react for 15 minutes, draining the liquid, taking the yarn, and drying; the bath ratio of the acidified cotton yarn in water is 5, the pH regulator is an acetic acid solution, and the concentration of the acetic acid solution is 0.5g / L, the waterproofing agent is SmartRepel Hydro CMD, and the amount of the waterproofing agent is 6% of the mass of the acidified cotton yarn, the temperature of the constant temperature circulation is 78°C, the cross-linking agent is Phobol XAN, the amount added is 1% of the mass of the cotton yarn, and the temperature is 80°C;

[0035] Step 5, weaving the cotton yarn obtained in the above steps at room temperature to obtain a woven fabric, and scouring and bleaching the fabric, then wet-dyeing the scouring and bleaching fabric, and shaping to obtain a moisture-absorbing and perspiration-wicking knitted fabric, scouring and washing is to put the fabric into a scouring and bleaching liquid for a half-bleaching process, the temperature of the half-bleaching process is 105°C, the bath ratio is 5, the concentration of the scouring agent CSP-T07 in the scouring liquid is 2g / L, the concentration of hydrogen peroxide is 5g / L, and the concentration of the chelating agent MAG-L is 3g / L, the shaping is to immerse the fabric at a temperature of 45°C and a vehicle speed of 40m / min, and then dry and shape it at a temperature of 155°C, and the immersion solution contains a fluffy silicone softener TF-4981 at a concentration of 30g / L.

[0036] Comparative Example 1

[0037] A method for preparing a moisture wicking knitted fabric comprises the following steps:

[0038] Step 1, putting cotton yarn into water, and then sequentially adding BASF Lufibrol MSD, BASF Kieralon F-MFB and sodium carbonate, stirring at a constant temperature for 1 hour, cooling to 50° C., draining and drying to obtain pre-scour cotton yarn; the bath ratio of the cotton yarn in water is 5, the addition amount of the BASF Kieralon F-MFB is 1% of the mass of the cotton yarn, the addition amount of the BASF Lufibrol MSD is 2% of the mass of the cotton yarn; the addition amount of the sodium carbonate is 60 g / L;

[0039] Step 2, putting the pre-scouring cotton yarn into water, and adding glacial acetic acid for pickling, and obtaining acidified cotton yarn after rinsing, wherein the bath ratio of the cotton yarn in water is 5, the amount of the glacial acetic acid added is 0.4 g / L, the pickling time is 25 min, and the temperature is 55° C.; the rinsing is cold water rinsing, and the rinsing temperature is 30° C.;

[0040] Step 3, putting the acidified cotton yarn into water, adjusting the pH to 4, then adding the waterproofing agent and stirring evenly, subjecting to constant temperature circulation for 30 minutes, adding the cross-linking agent to react for 15 minutes, draining the liquid, taking the yarn, and drying; the bath ratio of the acidified cotton yarn in water is 5, the pH regulator is an acetic acid solution, and the concentration of the acetic acid solution is 0.5g / L, the waterproofing agent is SmartRepel Hydro CMD, and the amount of the waterproofing agent is 6% of the mass of the acidified cotton yarn, the temperature of the constant temperature circulation is 78°C, the cross-linking agent is Phobol XAN, the amount added is 1% of the mass of the cotton yarn, and the temperature is 80°C;

[0041] Step 4, weaving the cotton yarn obtained in the above steps at room temperature to obtain a woven fabric, and scouring and bleaching the fabric, then wet-dyeing the scouring and bleaching fabric, and shaping to obtain a moisture-absorbing and perspiration-wicking knitted fabric, scouring and washing is to put the fabric into a scouring and bleaching liquid for a half-bleaching process, the temperature of the half-bleaching process is 105°C, the bath ratio is 5, the concentration of the scouring agent CSP-T07 in the scouring liquid is 2g / L, the concentration of hydrogen peroxide is 5g / L, and the concentration of the chelating agent MAG-L is 3g / L, the shaping is to immerse the fabric at a temperature of 45°C and a vehicle speed of 40m / min, and then dry and shape it at a temperature of 155°C, and the immersion solution contains a fluffy silicone softener TF-4981 with a concentration of 30g / L.

[0042] Comparative Example 2

[0043] Comparative Example 2 uses commercially available ordinary cotton yarn textile fabric.

[0044] Performance Testing

[0045] The fabrics prepared in Examples 1-3, the fabrics prepared in Comparative Example 1, and Comparative Example 2 were used as test samples for drying test. The fabrics were washed at a constant temperature according to the washing method of AATCC143, and then dried under the same lighting environment after washing. The results are as follows:

[0046] Basic drying time Complete drying time Example 1 27min 43min Example 2 22min 39min Example 3 25min 42min Comparative Example 1 32min 49min Comparative Example 2 83min -

[0047] Through the comparison of the above data, the drying methods of Examples 1-3 have good drying properties, and combined with the hygroscopicity of the cotton yarn itself, they show excellent moisture absorption and perspiration removal effects. Although Comparative Example 1 is slightly worse than Examples 1-3, it is far better than Comparative Example 2, showing a certain moisture absorption and perspiration removal effect. It also shows that the dispersed pores of the cotton yarn can effectively enhance its moisture absorption and perspiration removal effect.

[0048] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for preparing a moisture wicking knitted fabric, characterized in that: The steps include: Step 1, adding cotton yarn to water and boiling for 20-30 minutes, then adding sodium dodecyl sulfate and sodium carbonate and keeping warm for 2-4 hours, filtering and rinsing with hot water for 2-3 times, and drying to obtain pore-dispersed cotton yarn; Step 2, putting cotton yarn into water, and then sequentially adding BASF Lufibrol MSD and BASF Kieralon F-MFB, stirring at a constant temperature for 0.5-1h, cooling to 50°C, draining and drying, to obtain pre-scouring cotton yarn; Step 3, putting the pre-scoured cotton yarn into water, adding glacial acetic acid for pickling, and obtaining acidified cotton yarn after rinsing; Step 4, putting the acidified cotton yarn into water, adjusting the pH to 4-5, then adding the waterproofing agent and stirring evenly, circulating at a constant temperature for 20-40 minutes, adding the cross-linking agent to react for 10-20 minutes, draining the liquid, taking the yarn, and drying; Step 5, weaving the cotton yarn obtained in the above steps at room temperature to obtain a woven fabric, scouring and bleaching the fabric, and then wet-dyeing the scouring and bleaching fabric to obtain a moisture-absorbing and perspiration-wicking knitted fabric.

2. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The bath ratio of the cooking in step 1 is 1-10, the cooking temperature is 40-60° C., the concentration of the sodium dodecyl sulfate in water is 1-3 g / L, the amount of sodium carbonate added is 30-100 g / L, and the insulation temperature is 90-100° C.

3. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The temperature of the hot water rinsing in step 1 is 50-70°C; the temperature of the drying is 100-110°C.

4. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The bath ratio of the cotton yarn in water in step 2 is 1-10, the added amount of BASF Kieralon F-MFB is 1% of the mass of the cotton yarn, and the added amount of BASF Lufibrol MSD is 2% of the mass of the cotton yarn.

5. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The bath ratio of the cotton yarn in water in step 3 is 1-10, the amount of glacial acetic acid added is 0.3-0.4 g / L, the pickling time is 20-30 min, the temperature is 50-60° C.; the rinsing is cold water rinsing, and the rinsing temperature is 25-30° C.

6. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The bath ratio of the acidified cotton yarn in water in step 4 is 1-10, the pH regulator is acetic acid solution, and the concentration of the acetic acid solution is 0.4-0.6 g / L.

7. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The waterproofing agent in step 4 is Smart Repel Hydro CMD, a fluorine-free waterproofing agent from Argo. The amount of the waterproofing agent added is 5-7% of the mass of the acidified cotton yarn, and the temperature of the constant temperature cycle is 75-80°C.

8. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The crosslinking agent in step 4 is Phobol XAN, the added amount is 1% of the mass of the cotton yarn, and the temperature is 80-85°C.

9. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The scouring in step 5 is to put the fabric into the scouring liquid for a half-bleaching process, the temperature of the half-bleaching process is 100-110°C, the bath ratio is 1-10, and the concentration of the scouring agent CSP-T07, the concentration of the hydrogen peroxide is 5g / L, and the concentration of the chelating agent MAG-L is 3g / L in the scouring liquid.

10. The method for preparing the moisture wicking knitted fabric according to claim 1, characterized in that: The shaping in step 5 is to immerse and roll the fabric at a temperature of 40-50°C and a speed of 30-50m / min, and then dry and shape it at a temperature of 150-160°C. The immersion solution contains a fluffy silicone softener TF-4981 at a concentration of 25-35g / L.