Method for preparing flame-retardant polyamide fiber, flame-retardant polyamide fiber and aviation carpet containing flame-retardant polyamide fiber

By grafting Si(OH)3 groups on the surface of nylon fibers and building a three-dimensional silicon oxide network structure, the problem of fire spread caused by molten drips during combustion of nylon fibers is solved, and its flame retardant performance is significantly improved.

CN119083173APending Publication Date: 2024-12-06BEIJING AVIATION CRAFT CARPET CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411425509.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Modified drips during combustion can easily cause fire to spread, and the prior art is difficult to effectively improve its flame retardant ability.

Method used

Si(OH)3 groups are grafted on the surface of nylon fibers and condensation reaction with compound I to construct a three-dimensional silicon oxide network structure to enhance its flame retardant properties.

Benefits of technology

It effectively inhibits the flow and migration of melted droplets of nylon fiber, significantly improves its flame retardant performance, and reduces the risk of fire spread.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a method for preparing a flame-retardant polyamide fiber. The method comprises the following steps: obtaining a polyamide fiber grafted with a Si (OH) 3 group on the surface; preparing a compound I; and putting the polyamide fiber with the Si (OH) 3 group grafted on the surface into a second organic solution containing a compound I to prepare the flame-retardant polyamide fiber with a three-dimensional silicon oxide network structure constructed on the surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of fiber materials, and in particular to a method for preparing flame-retardant nylon fiber, the flame-retardant nylon fiber and an aviation carpet containing the same. Background Art

[0002] Nylon fiber is the earliest synthetic fiber to be industrially produced in the world. Although it is not considered a flammable fiber (limiting oxygen index LOI = 22-24), the presence of molten drippings when it burns can easily cause the spread of fire, which is very unfavorable for firefighting and disaster relief. Silicone has the characteristics of being halogen-free, environmentally friendly, and having excellent thermal stability, and has a flexible and easily controllable molecular skeleton. It is considered to be a halogen-free, anti-melt droplet type condensed phase flame retardant material with good development prospects; after being heated, the silicon element can form a stable silicon-containing carbonized layer, which is heat-insulating and oxygen-isolating, promotes the carbonization of the matrix material, and inhibits the flow and migration of the melt. Therefore, there is an urgent need for a method of combining silicone and nylon fiber to improve the flame retardancy of nylon fiber. Summary of the invention

[0003] The present invention provides a method for preparing flame-retardant nylon fiber, flame-retardant nylon fiber and aviation carpet containing the same. The present invention constructs a three-dimensional silicon oxide network structure on the surface of the nylon fiber body by grafting Si(OH)3 groups on the nylon fiber body and then performing a condensation reaction between the Si(OH)3 groups and compound I.

[0004] According to a first aspect of an embodiment of the present disclosure, there is provided a method for preparing a flame retardant nylon fiber, the method comprising the following steps:

[0005] Step 1: preparing a first mixed solution, wherein the first mixed solution is a tetrahydrofuran solution containing potassium tert-butoxide and / or a crown ether compound;

[0006] Step 2: providing a nylon fiber body, placing the nylon fiber body in the first mixed solution, stirring under the condition of isolating oxygen, and then adding 3-glycidyloxypropyltrimethoxysilane to form a second mixed solution, keeping isolating oxygen, stirring at 50° C.-70° C. for 2-5 hours, to obtain a nylon fiber with Si(OH)3 groups grafted on the surface;

[0007] Step 3: Preparation of compound I having the following formula I

[0008]

[0009] wherein R1 and R2 are each independently selected from hydrogen, deuterium, a halogen atom, a hydroxyl group, a nitro group, a cyano group, an amino group, a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C1-C5 alkoxy group, a substituted or unsubstituted C3-6 cycloalkyl group, a substituted or unsubstituted C6-C10 aryl group, a substituted or unsubstituted 3-6 membered heterocyclyl group or a substituted or unsubstituted 5-10 membered heteroaryl group; R3, R4, R5 and R6 are each independently selected from a C1-C5 alkyl group;

[0010] Step 4: dissolving the compound I in a second organic solution, and then placing the nylon fiber with Si(OH)3 groups grafted on the surface prepared in step 2 in the second organic solution, stirring at 60°C-80°C for 1.5-3h to obtain the flame-retardant nylon fiber.

[0011] In one aspect of the embodiments of the present disclosure, in the second mixed solution, the concentration of 3-glycidyloxypropyltrimethoxysilane is a mmol / mL, and 0.8≤a≤1.2.

[0012] In one aspect of the embodiments of the present disclosure, in the second organic solution, the concentration of the compound I is b mmol / mL, 0.6≤b≤1.5.

[0013] In one aspect of the disclosed embodiment, 0.8≤a×b≤1.4.

[0014] In one aspect of the disclosed embodiments, R1 and R2 are selected from the same substituent, and R3, R4, R5 and R6 are selected from the same substituent.

[0015] In one aspect of the embodiments of the present disclosure, the compound I is selected from the following compounds I-1 to I-4:

[0016]

[0017] In one aspect of the embodiments of the present disclosure, the material of the nylon fiber body is selected from nylon 6.

[0018] In one aspect of the embodiments of the present disclosure, the second organic solution is selected from toluene.

[0019] According to a second aspect of an embodiment of the present disclosure, a flame retardant nylon fiber is provided. The flame retardant nylon fiber is prepared by the aforementioned method.

[0020] According to a third aspect of an embodiment of the present disclosure, there is provided an aviation carpet, wherein the aviation carpet comprises the aforementioned flame-retardant nylon fiber.

[0021] The technical solution provided by the embodiments of the present disclosure may have the following beneficial effects:

[0022] It can be seen from the above embodiments that the present invention constructs a three-dimensional silicon oxide network structure on the surface of the nylon fiber body by grafting Si(OH)3 groups on the nylon fiber body and then reacting the Si(OH)3 groups with compound I through a condensation reaction, thereby further effectively enhancing the inhibitory effect of silicone on the occurrence of molten droplets in the nylon fiber.

[0023] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present disclosure and, together with the description, serve to explain the principles of the present disclosure.

[0025] Figure 1 It is a schematic diagram of the reaction principle of step 2 in the preparation method of the present disclosure according to an exemplary embodiment.

[0026] Figure 2 It is a schematic diagram of the reaction principle of step 4 in the preparation method of the present disclosure according to an exemplary embodiment. DETAILED DESCRIPTION

[0027] The terms used in this disclosure are for the purpose of describing specific embodiments only and are not intended to limit the disclosure. The singular forms of "a", "said" and "the" used in this disclosure and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0028] It should be understood that although the terms first, second, third, etc. may be used in the present disclosure to describe various information, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other.

[0029] In the present disclosure, the 3-glycidyloxypropyltrimethoxysilane used in the present disclosure, namely, the silane coupling agent Kh560, is also γ-glycidyloxypropyltrimethoxysilane.

[0030] The present disclosure provides a method for preparing a flame retardant nylon fiber, which comprises the following steps 1-6:

[0031] In some embodiments of the present disclosure, step 1 includes: preparing a first mixed solution, the first mixed solution is a tetrahydrofuran solution containing potassium tert-butoxide and / or a crown ether compound; in step 1, the role of potassium tert-butoxide (t-BuOK) is to activate the nitrogen element in the amide on the surface of the nylon fiber, which is helpful for its alkylation; the role of the crown ether compound is to act as a phase transfer catalyst. In some embodiments of the present disclosure, the crown ether compound can be selected from dicyclohexyl-18-crown-6.

[0032] In some embodiments of the present disclosure, the first mixed solution is a tetrahydrofuran solution containing potassium tert-butoxide and dicyclohexyl-18-crown-6; wherein the concentration of potassium tert-butoxide is selected from 0.05-0.15 mmol / mL, and the concentration of dicyclohexyl-18-crown-6 is selected from 0.005-0.015 mmol / mL.

[0033] In some embodiments of the present disclosure, step 2 includes: providing a nylon fiber body, placing the nylon fiber body in the aforementioned first mixed solution, stirring under the condition of isolating oxygen, and then adding 3-glycidyloxypropyltrimethoxysilane to form a second mixed solution, in which the concentration of 3-glycidyloxypropyltrimethoxysilane is a mmol / mL, 0.8≤a≤1.2; keeping the reaction system isolated from oxygen, stirring at 55°C for 3h, and obtaining a nylon fiber with Si(OH)3 groups grafted on the surface; the reaction schematic diagram is as shown in Figure 1 shown; from Figure 1 It can be seen that after step 2, the surface of the nylon fiber is grafted with -CH2CHO- segments, and the side of the -CH2CHO- segments contains -O-(CH2)3-Si(OH)3.

[0034] In some embodiments of the present disclosure, step 3 comprises: preparing a compound I having a structure of the following formula I

[0035]

[0036] wherein R1 and R2 are each independently selected from hydrogen, deuterium, a halogen atom, a hydroxyl group, a nitro group, a cyano group, an amino group, a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C1-C5 alkoxy group, a substituted or unsubstituted C3-6 cycloalkyl group, a substituted or unsubstituted C6-C10 aryl group, a substituted or unsubstituted 3-6 membered heterocyclyl group or a substituted or unsubstituted 5-10 membered heteroaryl group; and R3, R4, R5 and R6 are each independently selected from a C1-C5 alkyl group.

[0037] In some embodiments of the present disclosure, Compound 1 can be prepared by the following steps:

[0038] Weigh a certain amount of toluene and metal Na, heat to 100 ° C under nitrogen protection, and disperse the metal sodium into fine particles under rapid stirring; drip a dichlorosilane / toluene solution equimolar to the metal Na through a constant pressure dropping funnel, and continue stirring the reaction for 12 hours. After that, the reaction mixture is cooled to below 0 ° C, and under rapid stirring, a toluene solution containing a reaction raw material containing an aniline structure (such as but not limited to aniline, p-toluidine, m-toluidine, etc.) is slowly dripped through a constant pressure dropping funnel. After reacting for a period of time at this temperature, it is gradually warmed to room temperature to further complete the dechlorination reaction, and the by-products of sodium chloride and amine chloride are precipitated. Then at room temperature, continue stirring in the air for 1 hour, filter and remove the reaction by-products, and obtain compound I.

[0039] In some embodiments of the present disclosure, step 4 comprises: dissolving compound I in a second organic solution, and then placing the nylon fiber with Si(OH)3 groups grafted on the surface prepared in step 2 in the second organic solution, and stirring at 70°C for 1.5-3h to obtain the flame-retardant nylon fiber. The reaction diagram is as follows Figure 2 shown; from Figure 2 It can be seen that after the condensation reaction in step 4, since the side of the -CH2CHO- segment contains a Si(OH)3 group, it can dehydrate and condense with the Si-OH at position 1 of compound I to form Si-O-Si, and each Si-OH at the other three positions of compound I can dehydrate and condense with the Si(OH)3 group on the same amide segment to form Si-O-Si, thereby forming an interwoven silicon oxide structure.

[0040] The present disclosure is further described below by way of specific examples. The various chemical reagents used in the examples of the present disclosure are obtained through conventional commercial channels unless otherwise specified. Unless otherwise specified, the contents described below are all weight contents. Unless otherwise specified, it is understood that the process is carried out at room temperature.

[0041] Embodiment 1:

[0042] Embodiment 1 comprises the following steps:

[0043] Surface grafting:

[0044] Cut nylon 6 into 8cm×8cm samples, dissolve potassium tert-butoxide (561mg, 5mmol) and dicyclohexyl-18-crown-6 (186mg, 0.5mmol) in 50mL of THF, place the nylon 6 sample in the above solution, stir under oxygen-free conditions, then add 3-glycidyloxypropyltrimethoxysilane (11.8g, 50mmol, 11mL) using a syringe, keep the reaction system isolated from oxygen, stir at 55°C for 3h, and obtain nylon fibers with Si(OH)3 groups grafted on the surface.

[0045] Preparation of compound I-1:

[0046]

[0047] Weigh a certain amount of toluene and metal Na, heat to 100 ° C under nitrogen protection, and disperse the metal sodium into fine particles under rapid stirring; drip a dichlorosilane / toluene solution containing an equal mole of metal Na through a constant pressure dropping funnel, and continue stirring and reacting for 12 hours. After that, the reaction mixture is cooled to below 0 ° C, and a toluene solution containing aniline is slowly dripped through a constant pressure dropping funnel under rapid stirring. After reacting at this temperature for a period of time, it is gradually heated to room temperature to further complete the dechlorination reaction, and the by-products of sodium chloride and amine chloride are precipitated. Then continue stirring in the air for 1 hour at room temperature, remove the reaction by-products by suction filtration, and obtain compound I-1.

[0048] Condensation reaction:

[0049] A certain amount of the prepared compound I-1 was dissolved in 30 mL of toluene to obtain a 1 mmol / L toluene solution, the nylon fiber with Si(OH)3 groups grafted on the surface prepared above was placed in a second organic solution, dibutyltin dilaurate (DBTL) was added, and stirred at 70°C for 2 hours; the sample of Example 1 was obtained.

[0050] Embodiment 2:

[0051] Embodiment 2 comprises the following steps:

[0052] Surface grafting:

[0053] Cut nylon 6 into 8cm×8cm samples, dissolve potassium tert-butoxide (561mg, 5mmol) and dicyclohexyl-18-crown-6 (186mg, 0.5mmol) in 50mL of THF, place the nylon 6 sample in the above solution, stir under oxygen-free conditions, then add 3-glycidyloxypropyltrimethoxysilane (11.8g, 50mmol, 11mL) using a syringe, keep the reaction system isolated from oxygen, stir at 55°C for 3h, and obtain nylon fibers with Si(OH)3 groups grafted on the surface.

[0054] Preparation of compound I-2:

[0055]

[0056] Weigh a certain amount of toluene and metal Na, heat to 100 ° C under nitrogen protection, and disperse the metal sodium into fine particles under rapid stirring; drip a dichlorosilane / toluene solution dissolved in an equal mole of metal Na through a constant pressure dropping funnel, and continue stirring the reaction for 12 hours. After that, the reaction mixture is cooled to below 0 ° C, and a toluene solution dissolved in m-methylaniline is slowly dripped through a constant pressure dropping funnel under rapid stirring. After reacting at this temperature for a period of time, it is gradually heated to room temperature to further complete the dechlorination reaction, and the by-products of sodium chloride and amine chloride are precipitated. Then continue stirring in the air for 1 hour at room temperature, remove the reaction by-products by suction filtration, and obtain compound I-2.

[0057] Condensation reaction:

[0058] A certain amount of the prepared compound I-2 was dissolved in 30 mL of toluene to obtain a 1 mmol / L toluene solution, the nylon fiber with Si(OH)3 groups grafted on the surface prepared above was placed in a second organic solution, dibutyltin dilaurate (DBTL) was added, and stirred at 70°C for 2 hours; the sample of Example 2 was obtained.

[0059] Embodiment 3:

[0060] Embodiment 3 comprises the following steps:

[0061] Surface grafting:

[0062] Cut nylon 6 into 8cm×8cm samples, dissolve potassium tert-butoxide (561mg, 5mmol) and dicyclohexyl-18-crown-6 (186mg, 0.5mmol) in 50mL of THF, place the nylon 6 sample in the above solution, stir under oxygen-free conditions, then add 3-glycidyloxypropyltrimethoxysilane (11.8g, 50mmol, 11mL) using a syringe, keep the reaction system isolated from oxygen, stir at 55°C for 3h, and obtain nylon fibers with Si(OH)3 groups grafted on the surface.

[0063] Preparation of compound I-3:

[0064]

[0065] Weigh a certain amount of toluene and metal Na, heat to 100 ° C under nitrogen protection, and disperse the metal sodium into fine particles under rapid stirring; drip a dichlorosilane / toluene solution dissolved in an equal mole of metal Na through a constant pressure dropping funnel, and continue stirring the reaction for 12 hours. After that, the reaction mixture is cooled to below 0 ° C, and a toluene solution dissolved in p-methylaniline is slowly dripped through a constant pressure dropping funnel under rapid stirring. After reacting at this temperature for a period of time, it is gradually heated to room temperature to further complete the dechlorination reaction, and the by-products of sodium chloride and amine chloride are precipitated. Then continue stirring in the air for 1 hour at room temperature, remove the reaction by-products by suction filtration, and obtain compound I-3.

[0066] Condensation reaction:

[0067] A certain amount of the prepared compound I-3 was dissolved in 30 mL of toluene to obtain a 1 mmol / L toluene solution, the nylon fiber with Si(OH)3 groups grafted on the surface prepared above was placed in a second organic solution, dibutyltin dilaurate (DBTL) was added, and stirred at 70°C for 2 hours; the sample of Example 3 was obtained.

[0068] Embodiment 4:

[0069] Embodiment 4 comprises the following steps:

[0070] Surface grafting:

[0071] Cut nylon 6 into 8cm×8cm samples, dissolve potassium tert-butoxide (561mg, 5mmol) and dicyclohexyl-18-crown-6 (186mg, 0.5mmol) in 50mL of THF, place the nylon 6 sample in the above solution, stir under oxygen-free conditions, then add 3-glycidyloxypropyltrimethoxysilane (11.8g, 50mmol, 11mL) using a syringe, keep the reaction system isolated from oxygen, stir at 55°C for 3h, and obtain nylon fibers with Si(OH)3 groups grafted on the surface.

[0072] Preparation of compound I-4:

[0073]

[0074] Weigh a certain amount of toluene and metal Na, heat to 100 ° C under nitrogen protection, disperse the metal sodium into fine particles under rapid stirring; drip a dichlorosilane / toluene solution dissolved in an equal mole of metal Na through a constant pressure dropping funnel, and continue stirring the reaction for 12 hours. After that, the reaction mixture is cooled to below 0 ° C, and a toluene solution dissolved in p-methylaniline is slowly dripped through a constant pressure dropping funnel under rapid stirring. After reacting at this temperature for a period of time, it is gradually heated to room temperature to further complete the dechlorination reaction, and the by-products of sodium chloride and amine chloride are precipitated. Then continue stirring in the air for 1 hour at room temperature, remove the reaction by-products by suction filtration, and obtain compound I-4.

[0075] Condensation reaction:

[0076] A certain amount of the prepared compound I-3 was dissolved in 30 mL of toluene to obtain a 1 mmol / L toluene solution, the nylon fiber with Si(OH)3 groups grafted on the surface prepared above was placed in a second organic solution, dibutyltin dilaurate (DBTL) was added, and stirred at 70°C for 2 hours; the sample of Example 4 was obtained.

[0077] Comparative Example 1:

[0078] Comparative Example 1 is a sample of nylon 6 cut into 8 cm×8 cm.

[0079] Comparative Example 2:

[0080] Comparative Example 2 comprises the following steps:

[0081] Surface grafting:

[0082] Cut nylon 6 into 8cm×8cm samples, dissolve potassium tert-butoxide (561mg, 5mmol) and dicyclohexyl-18-crown-6 (186mg, 0.5mmol) in 50mL of THF, place the nylon 6 sample in the above solution, stir under oxygen-free conditions, then add 3-glycidyloxypropyltrimethoxysilane (11.8g, 50mmol, 11mL) using a syringe, keep the reaction system isolated from oxygen, stir at 55°C for 3h, and obtain the nylon fiber with Si(OH)3 groups grafted on the surface of comparative example 2.

[0083] Flame retardant performance test:

[0084] According to GB / T20462009, the samples of Examples 1-4 and Comparative Examples 1-2 were tested using an oxygen index tester; according to GB / T2048-2009, the samples of Examples 1-4 and Comparative Examples 1-2 were tested using a vertical combustion instrument. The test results are shown in Table 1 below:

[0085] Table 1

[0086] Example Limiting oxygen index Vertical burning level Example 1 30.5 V-1 Example 2 32.8 V-0 Example 3 31.2 V-0 Example 4 29.5 V-1 Comparative Example 1 24.2 V-2 Comparative Example 2 27.6 V-2

[0087] Embodiment 5:

[0088] The steps of Example 5 are the same as those of Example 2, except that the amount of 3-glycidyloxypropyltrimethoxysilane added in Example 5 is 25 mmol.

[0089] Embodiment 6:

[0090] The steps of Example 6 are the same as those of Example 2, except that the amount of 3-glycidyloxypropyltrimethoxysilane added in Example 6 is 75 mmol.

[0091] Embodiment 7:

[0092] The steps of Example 7 are the same as those of Example 2, except that, in Example 7, a toluene solution having a concentration of 0.5 mmol / L of compound I-2 is used in the condensation reaction step.

[0093] Embodiment 8:

[0094] The steps of Example 8 are the same as those of Example 2, except that, in Example 7, a toluene solution of compound I-2 having a concentration of 2 mmol / L is used in the condensation reaction step.

[0095] Flame retardant performance test:

[0096] According to GB / T2046-2009, the samples of Examples 5-8 were tested using an oxygen index tester; according to GB / T2048-2009, the samples of Examples 5-8 were tested using a vertical combustion instrument. The test results are shown in Table 2 below:

[0097] Table 2

[0098] Example Limiting oxygen index Vertical burning level Example 2 32.8 V-0 Example 5 28.6 V-1 Example 6 29.7 V-1 Example 7 28.2 V-1 Example 8 29.3 V-1

[0099] It can be seen from Table 2 that both the concentration of 3-glycidyloxypropyltrimethoxysilane in the second mixed solution and the concentration of compound I in the second organic solution should be in an appropriate range. If the values ​​of both are too small, a cross-linked network structure cannot be formed well; if the values ​​of both are too large, a self-condensation reaction will occur in the condensation reaction, and a cross-linked network structure cannot be formed well.

[0100] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the disclosure disclosed herein. The present disclosure is intended to cover any variations, uses or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The description and examples are intended to be exemplary only.

Claims

1. A method for preparing flame-retardant nylon fiber, characterized in that: The method comprises the following steps: Step 1: preparing a first mixed solution, wherein the first mixed solution is a tetrahydrofuran solution containing potassium tert-butoxide and / or a crown ether compound; Step 2: providing a nylon fiber body, placing the nylon fiber body in the first mixed solution, stirring under the condition of isolating oxygen, and then adding 3-glycidyloxypropyltrimethoxysilane to form a second mixed solution, keeping isolating oxygen, stirring at 50° C.-70° C. for 2-5 hours, to obtain a nylon fiber with Si(OH)3 groups grafted on the surface; Step 3: Preparation of compound I having the following formula I wherein R1 and R2 are each independently selected from hydrogen, deuterium, a halogen atom, a hydroxyl group, a nitro group, a cyano group, an amino group, a substituted or unsubstituted C1-C5 alkyl group, a substituted or unsubstituted C1-C5 alkoxy group, a substituted or unsubstituted C3-6 cycloalkyl group, a substituted or unsubstituted C6-C10 aryl group, a substituted or unsubstituted 3-6 membered heterocyclyl group or a substituted or unsubstituted 5-10 membered heteroaryl group; R3, R4, R5 and R6 are each independently selected from a C1-C5 alkyl group; Step 4: dissolving the compound I in a second organic solution, and then placing the nylon fiber with Si(OH)3 groups grafted on the surface prepared in step 2 in the second organic solution, stirring at 60°C-80°C for 1.5-3h to obtain the flame-retardant nylon fiber.

2. The method according to claim 1, characterized in that In the second mixed solution, the concentration of 3-glycidyloxypropyltrimethoxysilane is a mmol / mL, and 0.8≤a≤1.

2.

3. The method according to claim 1, characterized in that: In the second organic solution, the concentration of the compound I is b mmol / mL, 0.6≤b≤1.

5.

4. The method according to claim 2 or 3, characterized in that: 0.8≤a×b≤1.

4.

5. The method according to claim 1, characterized in that R1 and R2 are selected from the same substituent, and R3, R4, R5 and R6 are selected from the same substituent.

6. The method according to claim 5, characterized in that The compound I is selected from the following compounds I-1 to I-4:

7. The method according to claim 1, characterized in that The material of the nylon fiber body is selected from nylon 6.

8. A flame retardant nylon fiber, characterized in that: The flame retardant nylon fiber is prepared by the method according to any one of claims 1 to 7.

9. An aviation carpet, characterized in that: The aviation carpet comprises the flame-retardant nylon fiber according to claim 8.