Fabricated composite floor slab construction method

By using magnesium phosphate grouting material at the joints of the overlapping floor, the rapid reactivity and bonding properties are used to solve the cracking problem of the overlapping floor joints, and the rapid assembly and stability of the overlapping floor are achieved, which significantly improves the The service function and life of prefabricated concrete structures.

CN119083643APending Publication Date: 2024-12-06CHONGQING CONSTR ENG NEW BUILDING MATERIALS +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411304236.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The cracking of the joints of the overlapping floor slabs during the construction service seriously affects the use function and comfort of prefabricated buildings, and existing expansion agents and organic joint fillers are difficult to completely solve this problem.

Method used

Magnesium phosphate grout material is used as the caulking material for the overlapping floor joints, and its rapid reactivity, strong bonding performance and good flexibility can avoid cracking of the floor. The specific ratio includes sintered magnesium sand, soluble phosphate, Retarder, natural river sand, glass fiber powder, polydimethylsiloxane and sodium polyacrylate produce struvite crystals through acid-base reaction, improving bond strength and crack resistance.

Benefits of technology

The interface bonding strength and deformation coordination between the overlapping floor slabs and magnesium phosphate grouting material are significantly improved, and cracking is prevented, and the rapid assembly and construction of the overlapping floor slabs are realized, which enhances the stability and service life of the prefabricated concrete structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an assembly type composite floor slab construction method, which comprises the following steps of: during floor slab construction, firstly completing horizontal paving and splicing of prefabricated slabs on a support beam, and then completing concrete pouring of a cast-in-place layer above the prefabricated slabs after a formwork is erected on the lower surfaces of the spliced prefabricated slabs, and is characterized in that after the prefabricated slabs are spliced and the formwork is erected on the lower surfaces, the prefabricated slabs are paved on the lower surfaces of the prefabricated slabs; before the concrete is cast in place, a magnesium phosphate grouting material is poured in the abutted seam, and the magnesium phosphate grouting material contains a magnesium phosphate cementing material. According to the invention, the deformation coordination of the interface bonding strength between the magnesium phosphate grouting material and the concrete composite floor slab can be obviously improved, the rapid splicing construction of the composite floor slab is realized, the floor slab is prevented from cracking, and a new technical approach and technical guarantee are provided for the effective utilization of the magnesium phosphate grouting material in the field of fabricated concrete structure construction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building floor slab construction, and in particular to a method for constructing an assembled composite floor slab. Background Art

[0002] The development of prefabricated buildings is an important way to achieve sustainable development of my country's construction industry. Common prefabricated building systems are divided into prefabricated concrete structures, prefabricated steel structures and prefabricated wooden structures according to the type of structural materials. Due to the great pressure of anti-corrosion and fire prevention during the service of steel and wooden structures, prefabricated buildings are currently mainly prefabricated concrete structures. Composite floor slabs are assembled integral floor slabs composed of prefabricated panels and cast-in-place reinforced concrete layers. During the construction of composite floor slabs, the lower prefabricated panels can be spliced ​​first, and then a cast-in-place layer can be poured on the lower surface of the spliced ​​prefabricated panels after formwork is supported. The cast-in-place layer is fixed as a whole through the steel bars reserved on the upper surface of the prefabricated panels to complete the floor slab construction.

[0003] This type of composite floor is the most commonly used and largest-volume building component in prefabricated concrete structures. However, the cracking problem of the joints of composite floor seriously affects the use function of prefabricated buildings. Although the cracking of the joints of composite floor will not have a significant impact on the safety of prefabricated concrete structures, it seriously affects the living comfort, resulting in a reduction in the use function of prefabricated concrete structures, which restricts the large-scale promotion and application of prefabricated concrete structures.

[0004] In order to suppress and eliminate the joints of composite floor slabs, it is usually used to pour the joints with cement-based grouting material mixed with expansion agent after the prefabricated panels are spliced. However, the expansion agent is difficult to fully hydrate and produce expansion deformation in an environment without water curing, resulting in cracks in the joints of composite floor slabs after pouring cement-based grouting material. Moreover, as the service life of prefabricated buildings increases, the problem of cracks in the joints of composite floor slabs will gradually increase, and it is difficult to repair.

[0005] In addition, there is also a method of injecting flexible organic materials such as polyurethane foam into the joints of the composite floor slabs in the prior art. Although this method can improve the deformation performance of the joints of the composite floor slabs, the organic sealant is easy to age. The organic sealant will accelerate the aging after long-term contact with the alkaline environment of concrete. In addition, the organic sealant has poor compatibility with the concrete poured on the upper part of the composite floor slab, which will cause the concrete on the upper part of the composite floor slab to crack easily.

[0006] Therefore, the use of expansive cement-based grouting materials or organic sealants still cannot completely solve the problem of cracking in the joints of composite floor slabs. Therefore, how to design a solution that can better solve the problem of cracking in the joints of assembled composite floor slabs is still a problem to be studied by those skilled in the art. Summary of the invention

[0007] In view of the above-mentioned deficiencies in the prior art, the technical problem to be solved by the present invention is: how to provide a method for constructing an assembled composite floor slab that can better avoid the problem of cracking of the floor slab during the service life of the building.

[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0009] A method for constructing an assembled composite floor slab, during floor slab construction, firstly completing the horizontal paving and splicing of precast panels on support beams, and then completing the pouring of concrete for the cast-in-place layer above the precast panels after the lower surfaces of the spliced ​​precast panels are formworked. The method is characterized in that after the precast panels are spliced ​​and the lower surfaces are formworked, and before the concrete is cast-in-place, firstly pouring magnesium phosphate grouting material in the joints, the magnesium phosphate grouting material containing magnesium phosphate cementitious material.

[0010] The magnesium phosphate cementitious material is a hydraulic inorganic cementitious material that quickly generates strength based on the acid-base reaction of metal oxides and soluble phosphates or phosphoric acid. The material is first used to cast the joints, and its rapid reaction performance can be used to ensure good early strength. At the same time, its strong bonding performance can be used to ensure the reliability of the bonding between prefabricated panels and between the prefabricated panels and the cast-in-place concrete layer above, so as to better avoid the occurrence of floor cracks.

[0011] Preferably, the magnesium phosphate cementitious material refers to a cementitious material having a 28d compressive strength greater than 85 MPa and a flexural strength greater than 15 MPa, so as to better improve the interfacial bonding strength between the composite floor slab and the magnesium phosphate cementitious material.

[0012] Preferably, the composition of the magnesium phosphate grouting material includes the following materials in proportion by mass: 100 parts of sintered magnesia, 20-50 parts of soluble phosphate, 5-10 parts of retarder, 50-100 parts of natural river sand, 0.5-2 parts of glass fiber powder, 10-50 parts of mineral admixture, 0.1-0.5 parts of polydimethylsiloxane, 0.5-1.5 parts of polymer latex powder, 0.05-0.1 parts of hydroxypropyl methylcellulose ether, 0.05-0.1 parts of sodium polyacrylate and 20-40 parts of water.

[0013] The magnesium phosphate grouting material with the above specific proportion is made by uniformly mixing soluble phosphate and sintered magnesia with boric acid and sodium alginate retarder, natural river sand, glass fiber powder, mineral admixture and thickening and water-retaining components (polymer latex powder, hydroxypropyl methylcellulose ether), adding water and quickly stirring into a slurry with good fluidity, and then adding flexible polymer (polydimethylsiloxane) and water-absorbing and swelling components (sodium polyacrylate) and stirring together to form a grouting material, and immediately pouring it into the joints of concrete composite floor slabs. This can achieve a good anti-cracking effect at the joints.

[0014] Specifically, the magnesium phosphate grouting material with the above-mentioned proportion quickly generates strength based on the acid-base reaction of sintered magnesia and soluble phosphate. During the reaction process, the main product generated is struvite crystals (magnesium ammonium phosphate hexahydrate). The magnesium phosphate grouting material with the above-mentioned proportion has the characteristics of simple composition, high bonding strength, good flexibility, excellent crack resistance, strong water retention, good environmental stability and easy preparation. At the same time, it has high early compressive strength, bonding strength and good elastic deformation performance, and is suitable for the rapid pouring construction of composite floor slab joints.

[0015] As a preferred embodiment, in the above material ratio, the sintered magnesia sand used has a specific surface area of ​​160~300 m 2 / kg, the calcination temperature is not less than 1500℃, and the MgO content is not less than 82%.

[0016] Sintered magnesia is the alkaline component of magnesium phosphate cementitious materials. The sintered magnesia with the above parameters can ensure that the magnesium phosphate grouting material has a better bonding effect, and can also avoid the slow hydration of sintered magnesia in the later stage, which leads to a decrease in the volume stability of the magnesium phosphate grouting material.

[0017] Preferably, in the above material ratio, the soluble phosphate uses industrial grade potassium dihydrogen phosphate and / or ammonium dihydrogen phosphate, with a purity of not less than 98%.

[0018] Soluble phosphate is the acidic component in magnesium phosphate grouting material. The soluble phosphate of the above material can quickly dissolve and ionize hydrogen ions when it meets water. The pH value of the solution is 3~5, which is moderately acidic, which helps to improve the bonding strength of magnesium phosphate grouting material.

[0019] Preferably, in the above material ratio, the retarder is industrial-grade boric acid and sodium alginate, so that the setting and hardening time and fluidity of the magnesium phosphate grouting material can be better regulated.

[0020] Preferably, in the above material ratio, the mineral admixture is kaolin and / or fly ash; wherein the mass ratio of kaolin or fly ash is 10% to 50% of the sintered magnesia, and the specific surface area of ​​fly ash and kaolin should be not less than 500m 2 / kg.

[0021] This is because the role of the admixture is to improve the fluidity of the magnesium phosphate grouting material and enhance the cohesiveness of the grouting material. The use of admixtures defined by the above parameters can achieve better results.

[0022] Preferably, in the above material ratio, natural river sand preferably uses natural medium sand with a mud content of less than 1.0%, which can better control the fluidity and filling performance of magnesium phosphate grouting material.

[0023] Preferably, in the above material ratio, the glass fiber powder is made of continuous glass fiber raw filaments that are chopped, ground and screened, and the fiber length range is less than 0.3 mm, which is suitable for use as joints. It can be used as a filling and reinforcing material to improve the crack resistance of magnesium phosphate grouting materials.

[0024] In the above material ratio, hydroxypropyl methylcellulose ether (viscosity unit 4000 mPa·s) and polymer latex powder are used together as thickeners.

[0025] Among the above material ratios, an appropriate proportion of polydimethylsiloxane is innovatively used as a flexible polymer and combined with other materials, which can increase the flexibility of the grouting material and exert its defoaming function, improve the compression deformation performance of the magnesium phosphate grouting material and its deformation coordination with the concrete composite floor slab, and prevent bonding failure and cracking between the magnesium phosphate grouting material and the composite floor slab.

[0026] In the above material ratio, an appropriate proportion of sodium polyacrylate is innovatively used as a water-absorbing and swelling component. Sodium polyacrylate has strong water absorption and expands in volume after absorbing water, which can greatly improve the volume stability of magnesium phosphate grouting material after solidification and hardening, prevent the volume shrinkage of magnesium phosphate grouting material, and thus effectively prevent the composite floor slab from cracking.

[0027] Furthermore, the pouring process of the magnesium phosphate grouting material comprises the following steps:

[0028] a. At the construction site, according to the corresponding proportion, the soluble phosphate and sintered magnesia sand in the raw materials are mixed with the retarder, natural river sand, glass fiber powder, mineral admixture, polymer latex powder as a thickening and water-retaining component, and hydroxypropyl methylcellulose ether, and then added to the mortar mixer and stirred slowly and evenly (preferably, the stirring time of the mixer is 60-90 seconds, the speed of the mixer is greater than 1600 r / min, and the output power is 2-3kW), and then the mixing water of the corresponding proportion is added and stirred quickly (a high-speed mixer can be used for stirring time of 120-180 seconds) to complete the mixing of the first part of the materials;

[0029] b. After the first part of the materials are mixed, the corresponding second part of the materials are added according to the required proportion before pouring. The second part of the materials includes polydimethylsiloxane as a flexible polymer and sodium polyacrylate as a water-absorbing and swelling component. The magnesium phosphate grouting material is prepared by high-speed stirring (a high-speed mixer can be used for stirring for 120-180 seconds);

[0030] c. Pour the prepared magnesium phosphate grouting material into the joints of the prefabricated parts. After it has initially set, cover it with a plastic film (0.1 mm thick) and maintain it for at least 1 day. After the hydration reaction is completed, pour the upper cast-in-place concrete layer.

[0031] In the present invention, the principle of phosphate grouting material is: using the acid-base reaction of sintered magnesia sand and soluble phosphate to quickly form strength, using flexible polymer (polydimethylsiloxane) to improve the compression elastic deformation performance of magnesium phosphate grouting material, and using water-absorbing swelling component (sodium polyacrylate) to make magnesium phosphate grouting material produce volume expansion to inhibit the shrinkage deformation of the hardened body. The polydimethylsiloxane used in the scheme is an organic elastomer material, which is non-toxic and tasteless, has good flexibility, stretchability, biocompatibility, chemical inertness, good weather resistance and thermal stability, and has defoaming ability. In the present invention, the flexibility and compressibility of magnesium phosphate grouting material can be significantly improved, and bubbles in the slurry of magnesium phosphate grouting material can also be eliminated, and the density of magnesium phosphate grouting material can be improved. The sodium polyacrylate used in the scheme has strong wettability and is a polymer compound with both hydrophilic and hydrophobic groups. It can slowly dissolve in water to form an extremely viscous transparent liquid, and has good dispersibility. Sodium polyacrylate also has strong water absorption. In the slurry containing magnesium hydroxide generated by the hydration of magnesium oxide, a component material of magnesium phosphate cementitious material, sodium polyacrylate can exert its strong water absorption characteristics to form a precipitate whose volume expands dozens of times, thereby significantly improving the volume expansion characteristics of the magnesium phosphate grouting material during the coagulation and hardening process, and making the magnesium phosphate grouting material in a slightly expanded state during the coagulation and hardening process, thereby significantly improving the crack resistance of the magnesium phosphate grouting material and its interface bonding strength with the concrete composite floor.

[0032] Therefore, in the above steps, the materials are divided into two parts. The first part of the materials is mixed and stirred evenly, and then the second part of the materials is added before pouring. This can better ensure the timeliness of the flexible polymer and the water-absorbing and swelling components, and at the same time avoid the influence of this part of the materials on the stirring and mixing of the first part of the materials, thereby ensuring the smoothness of the overall pouring construction process.

[0033] The above steps are simple to operate. The present invention is used to process the joints of composite floor slabs. It is verified by experiments that the 2h positive tensile bonding strength between the magnesium phosphate grouting material of the present invention and the concrete composite floor slab can reach more than 2.0MPa, the elastic compression deformation at the age of 28d reaches more than 3%, and the drying shrinkage value at the age of 28d is reduced to 0.01%, thereby ensuring that the magnesium phosphate grouting material and the concrete composite floor slab have good bonding performance and deformation coordination.

[0034] The advantages of the present invention are as follows: (1) The magnesium phosphate grouting material has high early strength and good bonding performance, which can significantly speed up the assembly construction speed of the composite floor slab. (2) By improving the compression elastic deformation performance of the magnesium phosphate grouting material, the deformation coordination between the magnesium phosphate grouting material and the concrete composite floor slab can be significantly improved, and the bonding failure between the grouting material and the composite floor slab can be prevented. (3) By improving the early expansion performance of the magnesium phosphate grouting material, its volume stability is significantly improved, and the shrinkage and cracking of the magnesium phosphate grouting material is effectively prevented.

[0035] In summary, the present invention can significantly improve the deformation coordination of the interface bonding strength between the magnesium phosphate grouting material and the concrete composite floor slab, realize the rapid assembly construction of the composite floor slab, avoid the cracking of the floor slab, and provide a new technical approach and technical guarantee for the effective use of magnesium phosphate grouting materials in the field of prefabricated concrete structure construction. DETAILED DESCRIPTION

[0036] The present invention is further described in detail below in conjunction with specific implementation modes.

[0037] Best practice:

[0038] A method for constructing an assembled composite floor slab, during the floor slab construction, the horizontal paving and splicing of precast panels are first completed on the support beams, and then after the lower surface of the spliced ​​precast panels are supported by formwork, the concrete pouring of the cast-in-place layer is completed above the precast panels. The method is characterized in that after the precast panels are spliced ​​and the lower surface formwork is completed, before the concrete is poured in-situ, magnesium phosphate grouting material is first poured in the joints, and the magnesium phosphate grouting material contains magnesium phosphate cementitious material.

[0039] During implementation, the precast panels described in the above scheme are reinforced concrete precast components, which are manufactured in an assembled concrete component production enterprise, then transported to the construction site for hoisting in place, and laid flat on the support beam as the bottom support layer of the composite floor. The joint refers to the gap between two adjacent precast panels. Among them, the magnesium phosphate cementitious material refers to a cementitious material with a 28d compressive strength greater than 85MPa and a flexural strength greater than 15MPa. This can better improve the interface bonding strength between the composite floor and the magnesium phosphate cementitious material.

[0040] Among them, the composition of the magnesium phosphate grouting material includes the following materials in proportion by mass: 100 parts of sintered magnesia, 20-50 parts of soluble phosphate, 5-10 parts of retarder, 50-100 parts of natural river sand, 0.5-2 parts of glass fiber powder, 10-50 parts of mineral admixture, 0.1-0.5 parts of polydimethylsiloxane, 0.5-1.5 parts of polymer latex powder, 0.05-0.1 parts of hydroxypropyl methylcellulose ether, 0.05-0.1 parts of sodium polyacrylate and 20-40 parts of water.

[0041] The magnesium phosphate grouting material with the above specific proportion is made by uniformly mixing soluble phosphate and sintered magnesia with boric acid and sodium alginate retarder, natural river sand, glass fiber powder, mineral admixture and thickening and water-retaining components (polymer latex powder, hydroxypropyl methylcellulose ether), adding water and quickly stirring into a slurry with good fluidity, and then adding flexible polymer (polydimethylsiloxane) and water-absorbing and swelling components (sodium polyacrylate) and stirring together to form a grouting material, and immediately pouring it into the joints of concrete composite floor slabs. This can achieve a good anti-cracking effect at the joints.

[0042] Specifically, the magnesium phosphate grouting material with the above-mentioned proportion quickly generates strength based on the acid-base reaction of sintered magnesia and soluble phosphate. During the reaction process, the main product generated is struvite crystals (magnesium ammonium phosphate hexahydrate). The magnesium phosphate grouting material with the above-mentioned proportion has the characteristics of simple composition, high bonding strength, good flexibility, excellent crack resistance, strong water retention, good environmental stability and easy preparation. At the same time, it has high early compressive strength, bonding strength and good elastic deformation performance, and is suitable for the rapid pouring construction of composite floor slab joints.

[0043] Among them, the sintered magnesia used in the above material ratio has a specific surface area of ​​160~300 m 2 / kg, the calcination temperature is not less than 1500℃, and the MgO content is not less than 82%.

[0044] Sintered magnesia is the alkaline component of magnesium phosphate cementitious materials. The sintered magnesia with the above parameters can ensure that the magnesium phosphate grouting material has a better bonding effect, and can also avoid the slow hydration of sintered magnesia in the later stage, which leads to a decrease in the volume stability of the magnesium phosphate grouting material.

[0045] Among them, in the above material ratio, the soluble phosphate uses industrial grade potassium dihydrogen phosphate and / or ammonium dihydrogen phosphate, and the purity is not less than 98%.

[0046] Soluble phosphate is the acidic component in magnesium phosphate grouting material. The soluble phosphate of the above material can quickly dissolve and ionize hydrogen ions when it meets water. The pH value of the solution is 3~5, which is moderately acidic, which helps to improve the bonding strength of magnesium phosphate grouting material.

[0047] Among them, in the above material ratio, the retarder adopts industrial grade boric acid and sodium alginate, which can better control the setting and hardening time and fluidity of magnesium phosphate grouting material.

[0048] Among them, in the above material ratio, the mineral admixtures are kaolin and / or fly ash; the mass ratio of kaolin or fly ash is 10% to 50% of the sintered magnesia, and the specific surface area of ​​fly ash and kaolin should not be less than 500 m 2 / kg.

[0049] This is because the role of the admixture is to improve the fluidity of the magnesium phosphate grouting material and enhance the cohesiveness of the grouting material. The use of admixtures defined by the above parameters can achieve better results.

[0050] Among them, in the above material ratio, natural river sand is preferably natural medium sand with a mud content of less than 1.0%, which can better control the fluidity and filling performance of magnesium phosphate grouting material.

[0051] Among them, in the above material ratio, the glass fiber powder is made of continuous glass fiber raw filaments that are chopped, ground and screened, and the fiber length range is less than 0.3mm, which is suitable for use as joints. It can be used as a filling and reinforcing material to improve the crack resistance of magnesium phosphate grouting materials.

[0052] In the above material ratio, hydroxypropyl methylcellulose ether (viscosity unit 4000 mPa·s) and polymer latex powder are used together as thickeners.

[0053] Among the above material ratios, an appropriate proportion of polydimethylsiloxane is innovatively used as a flexible polymer and combined with other materials, which can increase the flexibility of the grouting material and exert its defoaming function, improve the compression deformation performance of the magnesium phosphate grouting material and its deformation coordination with the concrete composite floor slab, and prevent bonding failure and cracking between the magnesium phosphate grouting material and the composite floor slab.

[0054] In the above material ratio, an appropriate proportion of sodium polyacrylate is innovatively used as a water-absorbing and swelling component. Sodium polyacrylate has strong water absorption and expands in volume after absorbing water, which can greatly improve the volume stability of magnesium phosphate grouting material after solidification and hardening, prevent the volume shrinkage of magnesium phosphate grouting material, and thus effectively prevent the composite floor slab from cracking.

[0055] During implementation, the pouring process of the magnesium phosphate grouting material includes the following steps:

[0056] a. At the construction site, according to the corresponding proportion, the soluble phosphate and sintered magnesia sand in the raw materials are mixed with the retarder, natural river sand, glass fiber powder, mineral admixture, polymer latex powder as a thickening and water-retaining component, and hydroxypropyl methylcellulose ether, and then added to the mortar mixer and stirred slowly and evenly (preferably, the stirring time of the mixer is 60-90 seconds, the speed of the mixer is greater than 1600 r / min, and the output power is 2-3kW), and then the mixing water of the corresponding proportion is added and stirred quickly (a high-speed mixer can be used for stirring time of 120-180 seconds) to complete the mixing of the first part of the materials;

[0057] b. After the first part of the materials are mixed, the corresponding second part of the materials are added according to the required proportion before pouring. The second part of the materials includes polydimethylsiloxane as a flexible polymer and sodium polyacrylate as a water-absorbing and swelling component. The magnesium phosphate grouting material is prepared by high-speed stirring (a high-speed mixer can be used for stirring for 120-180 seconds);

[0058] c. Pour the prepared magnesium phosphate grouting material into the joints of the prefabricated parts. After it has initially set, cover it with a plastic film (0.1 mm thick) and maintain it for at least 1 day. After the hydration reaction is completed, pour the upper cast-in-place concrete layer.

[0059] In addition, during implementation, the specific mass ratio of sintered magnesia, soluble phosphate, retarder, mineral admixture, natural river sand, glass fiber powder, polydimethylsiloxane, polymer latex powder, hydroxypropyl methylcellulose ether, sodium polyacrylate and water can be adjusted within the above-mentioned ratio range according to the design requirements of the bonding strength of the composite floor slab, and the bonding effect can be specifically tested to select a more optimal specific ratio.

[0060] Specifically, the mass ratio (mass ratio) of the magnesium phosphate grouting material at room temperature can be adjusted according to the strength grade of the composite floor concrete. Based on the above specific implementation scheme, the applicant selects different specific parameters and adopts three groups of test examples to verify the effect. The specific table is as follows:

[0061]

[0062] Note: M—sintered magnesia; P—soluble phosphate; B—boric acid; AS—sodium alginate; NS—natural river sand; glass fiber powder—BF; FA—fly ash; JG—polydimethylsiloxane; JX—sodium polyacrylate; VAE—polymer latex powder; HPMC—hydroxypropyl methylcellulose ether.

[0063] Test example 1. Each step in this test example is the same as the above-mentioned specific implementation method, but the specific parameter values ​​are as follows: When the composite floor slab concrete strength grade is C50 or above, the magnesium phosphate grouting material in this embodiment adopts the following materials in parts by weight: 100 parts of sintered magnesia sand, 50 parts of soluble phosphate, 2 parts of retarder boric acid, 2 parts of retarder sodium alginate, 100 parts of natural river sand, 2 parts of glass fiber powder, 20 parts of fly ash, 1.5 parts of polymer latex powder, 0.05 parts of hydroxypropyl methylcellulose ether, 1.0 parts of polydimethylsiloxane, 1.5 parts of sodium polyacrylate, and 40 parts of mixing water.

[0064] Test Example 2. All steps in this test example are the same as those in the above-mentioned specific implementation method, but the specific parameter values ​​are as follows: when the strength grade of the composite floor concrete is C35~C45, the magnesium phosphate grouting material in this embodiment adopts the following materials in parts by mass: 100 parts of sintered magnesia sand, 30 parts of soluble phosphate, 3 parts of retarder boric acid, 4 parts of retarder sodium alginate, 75 parts of natural river sand, 1 part of glass fiber powder, 30 parts of fly ash, 1.0 part of polymer latex powder, 0.08 parts of hydroxypropyl methylcellulose ether, 0.75 parts of polydimethylsiloxane, 0.5 parts of sodium polyacrylate, and 30 parts of mixing water.

[0065] Test Example 3, each step in the test example is the same as the above-mentioned specific implementation method, but the specific parameter values ​​are as follows: when the strength grade of the composite floor concrete is C20~C30, the phosphate interface agent in this embodiment adopts the following materials in parts by weight: 100 parts of sintered magnesia, 20 parts of soluble phosphate, 4 parts of retarder boric acid, 6 parts of retarder sodium alginate, 50 parts of natural river sand, 0.5 parts of glass fiber powder, 50 parts of fly ash, 0.5 parts of polymer latex powder, 0.05 parts of hydroxypropyl methylcellulose ether, 0.5 parts of polydimethylsiloxane, 1.0 parts of sodium polyacrylate, and 20 parts of mixing water.

[0066] In the above three test cases, the interface bond strength between magnesium phosphate grouting material and concrete was tested by positive tensile bond test. Cut 100 mm × 100 mm × 50 mm concrete. Pour magnesium phosphate grouting material on the concrete surface according to the above sequence to form a 100 mm × 100 mm × 100 mm splitting tensile strength test specimen. After pouring, the specimen was placed in a curing box with the same ambient temperature. Referring to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the splitting tensile strength test method was used to test the interface bond strength of the specimens formed after pouring magnesium phosphate grouting material at 2h and 28d. Magnesium phosphate grouting was used to cast and form a 100 mm × 100 mm × 300 mm prism specimen, which was placed in a curing room at a temperature of 20±2℃ and a relative humidity of 55%±5% and cured to 28d. The axial pressure mechanical properties and elastic compression deformation were tested. The magnesium phosphate grouting material was used to cast a 25 mm × 25 mm × 280 mm prism specimen, which was placed in a curing room at a temperature of 20 ± 2°C and a relative humidity of 55% ± 5% to test the drying shrinkage value of the magnesium phosphate grouting material at 28 days. The test results of the three test cases are shown in the table below.

[0067]

[0068] In contrast, when cement-based grouting material is used, the cement-based grouting material and concrete interface bonding strength, 2h is 0MPa, and 28d bonding strength is only 0.5MPa. And the 2h bonding strength of magnesium phosphate grouting material and concrete is greater than 2.1MPa, and the 28d bonding strength is greater than 3.5MPa, so it can be seen that the interface bonding strength between magnesium phosphate grouting material and concrete composite floor is enhanced by this method, and its interface bonding strength can meet the requirement of removing support after 2h of construction completion, and there is no interface bonding failure situation between magnesium phosphate grouting material and concrete in addition. This illustrates that phosphoric acid prepared using the inventive method, Grouting material, its interface bonding strength with concrete composite floor is significantly improved, and bonding is more firm, and the rapid construction of concrete composite floor can be realized.

[0069] Therefore, the method is simple to operate. The present invention is used to process the joints of composite floor slabs. It is verified by experiments that the 2h positive tensile bonding strength between the magnesium phosphate grouting material of the present invention and the concrete composite floor slab can reach more than 2.0MPa, the elastic compression deformation at the age of 28d reaches more than 3%, and the drying shrinkage value at the age of 28d is reduced to 0.01%, thereby ensuring that the magnesium phosphate grouting material and the concrete composite floor slab have good bonding performance and deformation coordination.

Claims

1. A method for constructing an assembled composite floor slab, wherein during the construction of the floor slab, the horizontal paving and splicing of the prefabricated panels are first completed on the support beams, and then the concrete pouring of the cast-in-place layer is completed above the prefabricated panels after the lower surfaces of the spliced ​​prefabricated panels are supported by formwork, wherein: After the prefabricated panels are spliced ​​and the lower surface formwork is completed, before the concrete is poured in situ, a magnesium phosphate grouting material is poured in the joints, wherein the magnesium phosphate grouting material contains a magnesium phosphate cementitious material.

2. The method for constructing an assembled composite floor slab according to claim 1, characterized in that: The composition of the magnesium phosphate grouting material includes the following materials in proportion by mass: 100 parts of sintered magnesia, 20-50 parts of soluble phosphate, 5-10 parts of retarder, 50-100 parts of natural river sand, 0.5-2 parts of glass fiber powder, 10-50 parts of mineral admixture, 0.1-0.5 parts of polydimethylsiloxane, 0.5-1.5 parts of polymer latex powder, 0.05-0.1 parts of hydroxypropyl methylcellulose ether, 0.05-0.1 parts of sodium polyacrylate and 20-40 parts of water.

3. The method for constructing an assembled composite floor slab according to claim 2, characterized in that: In the above material ratio, the sintered magnesia used has a specific surface area of ​​160~300 m 2 / kg, the calcination temperature is not less than 1500℃, and the MgO content is not less than 82%.

4. The method for constructing an assembled composite floor slab according to claim 2, wherein: In the above material ratio, the soluble phosphate uses industrial grade potassium dihydrogen phosphate and / or ammonium dihydrogen phosphate, and the purity is not less than 98%.

5. The method for constructing an assembled composite floor slab according to claim 2, characterized in that: In the above material ratio, the retarder is industrial grade boric acid and sodium alginate.

6. The method for constructing an assembled composite floor slab according to claim 2, characterized in that: In the above material ratio, the mineral admixtures are kaolin and / or fly ash; the mass ratio of kaolin or fly ash is 10% to 50% of the sintered magnesia, and the specific surface area of ​​fly ash and kaolin should not be less than 500 m 2 / kg.

7. The method for constructing an assembled composite floor slab according to claim 2, characterized in that: In the above material ratio, natural river sand is preferably natural medium sand with a mud content of less than 1.0%.

8. The method for constructing an assembled composite floor slab according to claim 2, characterized in that: In the above material ratio, the glass fiber powder is made of continuous glass fiber raw yarn that is chopped, ground and screened, and the fiber length range is less than 0.3mm.

9. The method for constructing an assembled composite floor slab according to claim 2, characterized in that: The pouring process of the magnesium phosphate grouting material comprises the following steps: a. At the construction site, according to the corresponding proportion, the soluble phosphate and sintered magnesia sand in the raw materials are mixed with the retarder, natural river sand, glass fiber powder, mineral admixture, polymer latex powder as a thickening and water-retaining component, and hydroxypropyl methylcellulose ether, and added into the mortar mixer to slowly stir evenly, and then the corresponding proportion of mixing water is added to quickly stir to complete the mixing of the first part of the materials; b. After the first part of the materials are mixed, the corresponding second part of the materials are added according to the required proportion before pouring. The second part of the materials includes polydimethylsiloxane as a flexible polymer and sodium polyacrylate as a water-absorbing and swelling component, and the magnesium phosphate grouting material is prepared by high-speed stirring; c. Pour the prepared magnesium phosphate grouting material into the joints of prefabricated parts. After it has initially set, cover it with plastic film and maintain it for at least 1 day. After the hydration reaction is completed, pour the upper cast-in-place concrete layer.

10. The method for constructing an assembled composite floor slab according to claim 9, characterized in that: During stirring in step a, before adding the mixing water, the stirring time is 60-90 seconds using a stirrer, the stirring speed of the stirrer is greater than 1600 r / min, and the output power is 2-3 kW; after adding the mixing water, the stirring time is 120-180 seconds using a high-speed stirrer.