New method for reducing baking energy of iron powder

By using a dehydration device and an axial fan to assist in dehydration during the iron powder baking process, and further drying is achieved by using the hot air flow of the drying device and the waste heat of the second dragon twisting mechanism, the reduction of moisture content in iron powder baking is solved. and the problem of high cost has achieved a significant reduction in the moisture content and cost reduction of iron powder.

CN119085275APending Publication Date: 2024-12-06PANZHIHUA GANGCHENG GROUP

Patent Information

Application Number
CN202411454373.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing iron powder baking technology, the moisture content of wet concentrate is reduced and the efficiency is low and the baking cost is high, resulting in operational risks and high energy consumption during the iron powder baking process.

Method used

The dehydration device is used for preliminary dehydration, and the airflow formed by the axial flow fan is assisted in the dehydration, and then it is transported to the drying device through the first dragon twisting mechanism, and the hot airflow of the drying device is used to assist in the dehydration of the material, and the second dragon twisting mechanism is used to utilize itself. The waste heat is further dried to reduce the moisture content and baking cost of the iron powder.

Benefits of technology

The moisture content of iron powder has been significantly reduced to about 0.1%, and the baking cost has been reduced to 45-50 yuan/ton, which has significantly reduced the moisture content and baking cost of iron powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119085275A_ABST
    Figure CN119085275A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of iron powder baking, in particular to a novel method for reducing iron powder baking energy. Comprising the following steps: (1) grinding and washing an iron-containing material to obtain wet concentrate; (2) conveying the wet concentrate into a dehydration device for dehydration; (3) the dehydrated materials are conveyed to a drying device through a first auger mechanism to be dried; the dried hot air flow is introduced into a first auger mechanism to assist in material dehydration, and the air flow discharged from the first auger mechanism is introduced to a discharge port of a dehydration device to assist in dehydration through an axial flow fan; and (4) the dried iron powder is discharged from a discharging port of the drying device and conveyed into a storage device through a second auger mechanism. By adopting the new method provided by the invention to bake the iron powder, the moisture content of the baked iron powder is reduced to about 0.1%, the baking cost is reduced to 45-50 yuan / ton, and the moisture content of the iron powder and the comprehensive cost of baking the iron powder are greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron powder baking, in particular to a new method for reducing the energy of iron powder baking. Background Art

[0002] After the iron-containing material is ground by a ball mill, washed by a magnetic separator and a classifier, a semi-finished iron powder is obtained, which is called wet concentrate. The moisture content of the wet concentrate fluctuates between 18-20%. In the existing iron powder production technology, the wet concentrate enters the drying drum in two different ways. Currently, a single-drum drying drum is generally used, that is, the wet concentrate enters from the inlet of the drying drum. After the baking is completed, the dry iron powder is discharged from the outlet of the drying drum. The size of the inlet end of the drying drum is the same as that of the outlet end, and it is installed at an inclination of 3-5°. The conventional choice of drying drum is φ1200-1500mm×9000-12000mm. The appropriate drying drum model can be selected according to the output of iron powder.

[0003] There are two ways for wet concentrate to enter the drying drum:

[0004] 1. Use iron troughs to hold the concentrate. During the holding process, vibrate and dehydrate. After dehydration, turn the wet concentrate to the baking platform and use a feeding disc to feed the material into the drying drum. The feeding disc is mainly for uniform feeding to ensure the stability of the feeding process. The moisture content of the wet concentrate entering the drying drum is reduced to 12-15%. This method can reduce the moisture content of the wet concentrate by 5-8 percentage points, but it requires frequent lifting of the iron trough, which is labor-intensive for operators and poses certain safety risks.

[0005] Second, use a dehydration disc for simple dehydration. This method effectively connects the front-end hydrometallurgy with the subsequent baking, reduces the lifting link, and reduces the labor intensity of operators. However, when this method is used to process wet concentrate, the dehydration disc can only reduce the moisture content by 2-3 percentage points, resulting in a significant increase in subsequent baking costs.

[0006] When wet concentrate is dried with a drying drum, anthracite, organic sintering rods, electricity, gas and other energy media can be used to generate heat to bake the material. In order to reduce the moisture content of the iron powder product, the temperature of the iron powder product after drying is generally controlled at 70-90℃, resulting in the baking cost being maintained at 80-100 yuan / ton of dry iron powder.

[0007] Therefore, a new method for baking iron powder which can reduce the moisture content of iron powder and reduce the cost is proposed. Summary of the invention

[0008] The purpose of the present invention is to provide a new method for reducing the energy required for baking iron powder, which can reduce the moisture content in the iron powder after baking and significantly reduce the baking cost.

[0009] The present invention provides a new method for reducing the energy of iron powder baking, comprising the following steps:

[0010] (1) grinding the iron-containing material with a ball mill, washing with a magnetic separator and a separator to obtain a wet concentrate;

[0011] (2) transporting the wet concentrate to a dehydration device for dehydration;

[0012] (3) The dehydrated material is transported to the drying device for drying through the first auger mechanism; the dried hot air flow is introduced into the first auger mechanism through the air inlet to assist in dehydrating the material, and then discharged from the air outlet of the first auger mechanism, and the air flow discharged from the air outlet is guided to the discharge port of the dehydration device by an axial flow fan to assist in dehydrating the material; wherein the flow direction of the hot air flow inside the first auger mechanism is opposite to the transportation direction of the material;

[0013] (4) The dried iron powder is discharged from the discharge port of the drying device and transported to the storage device through the second auger mechanism.

[0014] Furthermore, the particle size distribution of the wet concentrate in step (1) includes: +40 mesh 7-10%; 40-60 mesh 10-12%; 60-80 mesh 14-16%; 80-100 mesh 16-18%; -100 mesh 45-50%;

[0015] The wet concentrate has a metallic iron content of 88-90%, a total iron content of 90-92% and a moisture content of 18-20%.

[0016] Furthermore, the dehydration device in step (2) adopts a disc dehydrator, and 15-20 threaded steel bars with a diameter of 10 mm and a length of 300 mm are arranged on the surface of the dehydration disc of the disc dehydrator, and the threaded steel bars are evenly distributed along the center of the dehydration disc.

[0017] Furthermore, in step (3), the air inlet is provided on one side of the discharge port of the first auger mechanism, and the air outlet is provided on one side of the feed port of the first auger mechanism; the axial flow fan is provided on one side of the air outlet, and the air outlet of the axial flow fan faces the discharge port of the dehydration device.

[0018] Furthermore, the first auger mechanism is tilted, and the tilt angle is not less than 5-10 degrees; the first auger mechanism includes a box body, a spiral auger is arranged inside the box body, a feed port is arranged at the top of one end of the box body, and a discharge port is arranged at the bottom of one end of the box body, and the position of the discharge port is higher than the position of the feed port.

[0019] Furthermore, 3-5 air inlet holes and air outlet holes are respectively provided at the top of both ends of the box body, and the diameters of the air inlet holes and the air outlet holes are 30-50 mm; and a drainage outlet is provided at one end of the box body close to the feed port.

[0020] Furthermore, the drying device in step (3) includes a drying cylinder, a combustion chamber and a driving device for driving the drying cylinder to rotate, the drying cylinder includes an inner cylinder and an outer cylinder, a cavity is provided between the outer cylinder and the inner cylinder; the heat source outlet of the combustion chamber is connected to the heat source inlet of the inner cylinder, the feed port of the inner cylinder is connected to the discharge port of the first auger mechanism; and a discharge port is provided at one end of the outer cylinder close to the heat source inlet.

[0021] Furthermore, the diameters of both ends of the inner cylinder and the outer cylinder are different, the end with a smaller diameter of the inner cylinder is connected to the end with a larger diameter of the outer cylinder, the length of the outer cylinder is greater than the length of the inner cylinder, the end with a larger diameter of the inner cylinder is completely open, and the material is discharged from the end with a larger diameter of the inner cylinder into the outer cylinder.

[0022] Furthermore, the interior of the inner cylinder is divided into a low-temperature preheating zone, a medium-temperature transition zone, and a high-temperature baking zone in sequence from the end with a smaller diameter to the end with a larger diameter; the inner cylinder is provided with 3-5 rotating blades in the low-temperature preheating zone; a water vapor collection device is provided in the medium-temperature transition zone, and the water vapor collection device discharges the water vapor inside the inner cylinder to the outside of the drying cylinder.

[0023] Furthermore, the area of ​​the outer cylinder near the end with a larger diameter is a waste heat storage area, and the area at the other end is a high-temperature baking area. The high-temperature baking area of ​​the outer cylinder is connected to the high-temperature baking area of ​​the inner cylinder, and the heat is pumped into the first auger mechanism in the waste heat storage area by means of negative pressure extraction; the drying device adopts low-temperature baking, and the temperature of the baked iron powder is controlled at 40-50°C, maintaining a small amount of moisture while carrying a small amount of waste heat. The residual moisture is baked through the process of turning the material by the second auger mechanism using its own waste heat.

[0024] In summary, compared with the prior art, the present invention has the following advantages:

[0025] The technical solution provided by the present invention dehydrates the wet concentrate through a dehydration device, and at the same time uses the flowing airflow formed by the axial flow fan toward the discharge port of the dehydration device to strengthen auxiliary dehydration, and then transports it to the inside of the drying device through the first auger mechanism for drying. The hot air flow after drying is led to the first auger mechanism to assist the material in dehydration, and the airflow discharged after cooling is aimed at the discharge port of the dehydration device to assist the material in dehydration. The iron powder product baked from the drying device is transported to the storage device through the second auger mechanism, and the iron powder is dried by its own heat during transportation. The above method is used to bake the iron powder, and the moisture content of the baked iron powder is reduced to about 0.1%, and the baking cost is 45-50 yuan / ton of iron powder, which greatly reduces the moisture content of the iron powder and the comprehensive cost of baking the iron powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 It is a layout diagram of the dehydration disc in an embodiment of the present invention;

[0028] Figure 2 It is a layout diagram of the first auger mechanism in an embodiment of the present invention;

[0029] Figure 3 Schematic diagram of the layout of the drying device in the embodiment of the present invention.

[0030] Description of reference numerals: 1-sorter; 2-disc dehydrator; 201-rebar; 3-first auger mechanism; 301-air inlet; 302-air outlet; 303-drain outlet; 4-axial flow fan; 5-drying cylinder; 501-inner cylinder; 502-outer cylinder; 503-rotating blades; 504-water vapor collection device; 505-water vapor discharge pipeline; 506-waste heat recovery device; 507-heat introduction pipeline; 508-induced draft fan; 6-combustion chamber;

[0031] in Figure 1 , Figure 2 and Figure 3 The solid arrows in the figure represent the material direction, and the dotted arrows represent the airflow direction. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0034] In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined. In addition, the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0035] Example

[0036] A new method for reducing iron powder baking energy, the specific steps are as follows:

[0037] (1) The iron-containing material is ground by a ball mill, and then washed by a magnetic separator and a separator 1 to obtain a wet concentrate. The particle size distribution and chemical indexes of the wet concentrate are shown in Tables 1 and 2 respectively:

[0038] Table 1 Particle size distribution of wet concentrate

[0039] Particle size distribution +40 mesh 40-60 mesh 60-80 mesh 80-100 mesh -100 mesh % 8.24 11.07 15.32 17.06 48.31

[0040] Table 2 Chemical indicators of wet concentrate

[0041] Components MFe TFe Moisture content content% 88.67 90.27 18.78

[0042] (2) transporting the wet concentrate to a dehydration device for dehydration;

[0043] (3) The dehydrated material is transported to the drying device for drying through the first auger mechanism 3; the hot air flow after drying is introduced into the first auger mechanism 3 through the air inlet 301 to assist in dehydrating the material, and then discharged from the air outlet 302 of the first auger mechanism 3, and the air flow discharged from the air outlet 302 is guided to the discharge port of the dehydration device by the axial flow fan 4 to take away the moisture in the dehydrated material; wherein the flow direction of the hot air flow inside the first auger mechanism 3 is opposite to the transportation direction of the material;

[0044] (4) The dried iron powder is discharged from the discharge port of the drying device, screened by the screen device, and finally transported to the storage device through the second auger mechanism.

[0045] Among them, the dehydration device in step (2) adopts a vibrating disc dehydrator 2. To improve the dehydration efficiency, the vibration frequency is set to vibrate for 1-2 minutes every 8-10 minutes; the dehydration disc of the disc dehydrator 2 is tilted, the tilt angle is 3-5°, and the diameter of the dehydration disc is 1500-2000mm; preferably, the dehydration disc has a tilt angle of 3° and a diameter of 1500mm. Figure 1 As shown, 20 threaded steel bars 201 are welded on the side of the dehydration disc, and the size of the threaded steel bars 201 is φ10×300mm, and the threaded steel bars 201 are evenly distributed along the center of the dehydration disc. The multiple threaded steel bars 201 can filter water better, and the diameter and length of the threaded steel bars 201 can be adjusted appropriately as needed.

[0046] In step (3), the material dehydrated by the disc dehydrator 2 is transported to the drying device by the first auger mechanism 3. The first auger mechanism 3 is tilted, and the tilt angle in this embodiment is 25°. The first auger mechanism 3 adopts a conventional screw conveyor in the art, including a box body, a spiral auger is arranged inside the box body, a feed port is arranged at the top of one end of the box body, and a discharge port is arranged at the bottom of the other end. The height of the feed port is lower than the height of the discharge port. When the spiral auger rotates to transport the material, the water in the material flows from the discharge end to the feed end.

[0047] like Figure 2As shown, three air inlet holes 301 and air outlet holes 302 with a diameter of 30 mm are respectively arranged at both ends of the top of the box; the air inlet hole 301 is arranged 10-30 mm above the projection position of the discharge port, and the air outlet hole 302 is arranged 10-30 mm above the feed port. A drainage port 303 is arranged 10-30 mm from the top of the side wall of the box near the feed port, and the water formed inside the box is discharged through the drainage port 303. The drainage port 303 is connected with a hose to smoothly discharge the water of the first auger mechanism 3. Except for the feed port, the discharge port, the air inlet hole 301, the air outlet hole 302 and the drainage port 303, the other parts of the box are completely closed.

[0048] The drying device in step (3) includes a drying drum 5, a combustion chamber 6 and a driving device for driving the drying drum 5 to rotate. The drying device uses anthracite, organic sintered rods, electricity, gas and other energy sources to provide heat. Figure 3 As shown, the drying cylinder 5 includes an inner cylinder 501 and an outer cylinder 502, wherein one end of the inner cylinder 501 is provided with a feed port and a heat source inlet, the heat source inlet is connected to the combustion chamber 6, and the feed port is connected to the discharge port of the first auger mechanism 3. During the rotation of the inner cylinder 501, the material gradually contacts the hot air flow, and both the material and the hot air flow gradually move toward the outlet of the inner cylinder 501. The driving device therein adopts a conventional driving device in the art, and under the action of the driving device, the inner cylinder 501 and the outer cylinder 502 rotate in opposite directions, and when a person stands facing the end of the feed port of the inner cylinder 501, the inner cylinder 501 and the outer cylinder 502 rotate clockwise and counterclockwise respectively.

[0049] Both the inner cylinder 501 and the outer cylinder 502 have a central axis, and the central axis is kept horizontal. The inner cylinder and the outer cylinder can be the same size at both ends, but it is better to use a "big end and small end" cylinder, that is, the diameters of the two ends of the inner cylinder 501 and the outer cylinder 502 are different. During the installation of the drying cylinder 5, while ensuring that the central axis of the drying cylinder 5 is in a horizontal position, the cylinder body of the drying cylinder 5 has an inclination angle of 3-5°. The end with a smaller diameter of the inner cylinder 501 is provided with a feed port and a heat source inlet, and the end with a larger diameter is completely open, and the rest of the parts are all closed. The material moves from the "small end" to the "big end" as the inner cylinder 501 rotates, comes out from the "big end" end, and enters the cavity between the inner cylinder 501 and the outer cylinder 502. The length of the inner cylinder 501 is 500-1000mm shorter than that of the outer cylinder 502. The "big head and small head" of the inner cylinder 501 and the outer cylinder 502 are installed upside down. The "small head" of the inner cylinder 501 and the "big head" of the outer cylinder 502 are roughly flush, and the "big head" of the inner cylinder 501 and the "small head" of the outer cylinder 502 differ by 500-1000mm. The discharge port of the drying cylinder 5 is located at the end with a larger diameter of the outer cylinder 502, and is located at the same end as the feed port. The "small head" end of the outer cylinder 502 reserves the position of the water vapor discharge pipe 505, and the "big head" end reserves the position of the discharge port and the heat guide pipe 507, and the rest is fully closed. The "big head" end of the inner cylinder 501 and the "small head" of the outer cylinder 502 are connected with a position of 80-120mm to facilitate the passage of materials.

[0050] The length of the drying cylinder 5 is generally controlled to be 10-12 meters. The internal space of the inner cylinder 501 from the "small head" end to 5-6 meters is a low-temperature preheating zone, the area from 5-6 meters to 8-9 meters is a medium-temperature transition zone, and the area from 8-9 meters to the "big head end" is a high-temperature baking zone; the area from the "big head" end to 7-8 meters of the outer cylinder 502 is a waste heat storage area, and the area from 7-8 meters to the "small head" end of the outer cylinder 502 is a high-temperature baking zone; the high-temperature baking zone of the inner cylinder 501 is connected to the high-temperature baking zone of the outer cylinder 502.

[0051] In the low-temperature preheating zone, the material is the material brought in by the first auger mechanism 3, which has a high moisture content, and some of the material will inevitably stick together. In order to avoid material sticking and improve the preheating efficiency, in the low-temperature preheating zone, 3-5 rotating blades 503 are set in the upper half arc of the inner cylinder 501 based on the central axis of the inner cylinder 501. When the inner cylinder 501 rotates, the material falls, and the internal rotating blades 503 are used to break up the material to avoid clumping. When designing and making, the rotating blades 503 are based on the cross-section of the inner cylinder of the drying cylinder and are evenly distributed. The rotating blades 503 can rotate by themselves, but cannot rotate with the inner cylinder 501. A motor and a rotating shaft can be set to drive the rotating blades 503 to rotate. The number, width, length and other parameters of the rotating blades 503 need to ensure that in the low-temperature preheating zone, when the inner cylinder 501 rotates, the material that falls can be completely broken up.

[0052] A water vapor collecting device 504 is provided in the medium temperature transition zone, and the water vapor collecting device 504 is connected to the water vapor exhaust pipe 505. The water vapor collecting device uses a relatively simple method such as vacuuming to draw the water vapor in the medium temperature transition zone from the inner cylinder 501 to the outside of the drying cylinder 5, so as to prevent the water vapor from entering the high temperature baking zone and affecting the baking.

[0053] The material entering the waste heat storage area has been dried, and a large amount of waste heat is stored in this area. The heat in this area is led out to the inside of the first auger mechanism 3 by extracting negative pressure. A waste heat recovery device 506 can be installed in this area. The waste heat recovery device 506 is connected to the heat introduction pipe 507. The heat introduction pipe 507 is equipped with an induced draft fan 508 to collect the waste heat and introduce it into the first auger mechanism 3 through the heat introduction pipe 507 and the induced draft fan 508. After baking, the remaining heat in the waste heat storage area of ​​the outer cylinder 502 is drawn by the heat introduction pipe 507, and enters the inside of the first auger mechanism 3 through the air inlet 301 in the form of hot air flow, and is discharged through the air outlet 302 after cooling; the material of the first auger mechanism 3 moves from the feed port to the discharge port, and the hot air flow moves from the discharge port to the feed port. The moving directions of the material and the hot air flow are just opposite. The heat can be used to assist the material in the first auger mechanism 3 to effectively dehydrate.

[0054] A 2.2-kilowatt axial flow fan 4 is installed on one side of the air outlet 302 of the first auger mechanism 3. The air outlet of the axial flow fan 4 faces the discharge port of the disc dehydrator 2. The temperature of the airflow discharged from the first auger mechanism 3 is reduced. The axial flow fan 4 is used to form a flowing airflow and align it with the discharge port of the disc dehydrator 2. The moisture on the surface of the material is taken away by air circulation, which can better assist dehydration.

[0055] In this embodiment, the diameter of the "small end" of the outer cylinder 502 is 1500mm and the length is 12 meters. Taking the center line of the drying cylinder as the reference, the cylinder has an inclination angle of 3° in the horizontal direction; the diameter of the "big end" of the inner cylinder 501 is 1300mm and the length is 11 meters. Taking the center line of the drying cylinder as the reference, the cylinder has an inclination angle of 3° in the horizontal direction; the end of the "big end" and the "small end" of the inner cylinder 501 differ by 1 meter, and the rotation speeds of the inner cylinder 501 and the outer cylinder 502 are both 6 rpm. The area from the "small end" of the inner cylinder 501 to 6 meters is a low-temperature preheating zone, the area from 6 to 9 meters is a medium-temperature transition zone, and the area from 9 meters to the "big end" is a high-temperature baking zone; the area from the "big end" to 7 meters of the outer cylinder 502 is a waste heat storage area, and the area from 7 meters to the "small end" is a high-temperature baking zone. 3-5 rotating blades 503 are arranged in the area of ​​3-5 meters of the inner cylinder 501. A water vapor collecting device 504 is arranged at 7-8 meters of the inner cylinder 501, and the outlet of the water vapor collecting device 504 is connected to the water vapor exhaust pipe 505.

[0056] During the drying in step (3), the material enters the inner cylinder 501 from the feed port and is baked at low temperature. The heat source of the combustion chamber 6 enters the inner cylinder 501 through the heat source inlet. During the rotation of the inner cylinder 501 and the outer cylinder 502, the material passes through the low-temperature preheating zone and the medium-temperature transition zone inside the inner cylinder 501 and enters the high-temperature baking zone and then enters the high-temperature baking zone of the outer cylinder 502. Finally, the material passes through the waste heat storage zone of the outer cylinder 502 and is discharged from the discharge port. The temperature of the iron powder after baking is controlled at 40-50°C, and the moisture content of the iron powder is 0.2-0.3%. The waste heat recovery device 506 in the waste heat storage zone recovers the heat and introduces it into the first auger mechanism 3 through the heat introduction pipe 507 and the induced draft fan 508 through the air inlet 301 to assist in dehydration of the material. The cooled airflow is discharged from the air outlet 302, and the airflow discharged from the air outlet 302 is led out to the discharge port of the disc dehydrator 2 by the axial flow fan 4 to take away the moisture in the dehydrated material. The drying cylinder 5 adopts a low-temperature baking mode to control the temperature of the iron powder after baking at 40-50°C. The air flow temperature in the waste heat storage area fluctuates at 40-50°C, that is, the air flow temperature entering the first auger mechanism 3 fluctuates at 40-50°C, and the air flow temperature from the first auger mechanism 3 to the discharge port of the disc dehydrator 2 fluctuates at 30-35°C. This temperature has a good auxiliary disc dehydration effect. The temperature of the iron powder after screening the finished iron powder fluctuates at 30-40°C when it is transported to the storage device by the second auger mechanism.

[0057] The dried material in step (4) is discharged from the discharge port of the outer cylinder 502, and is screened by a screen device to obtain iron powder, and the proportion of iron powder under the 40-mesh screen is controlled to be ≥95%, and finally transported to the storage device through the second auger mechanism. When the second auger mechanism transports the iron powder, the waste heat of the iron powder itself is used to dry the iron powder again during the process of the auger blade turning the iron powder, so that the final moisture content of the iron powder is controlled to be about 0.1%. The second auger mechanism can be a conventional screw conveyor in the field.

[0058] The moisture content of the wet concentrate formed after grinding and washing fluctuates between 18-20%. After dehydration through the dehydration disc, the moisture content is reduced to 13-15%. After the first auger mechanism and hot air flow assisted dehydration, the moisture content is reduced to 8-9%. The moisture content of the material can be reduced to 4-5% in the low-temperature preheating zone of the inner drum of the drying drum, and the moisture content can be reduced to 1.0-1.2% in the medium-temperature transition zone. The moisture content of the iron powder after baking is reduced to 0.2-0.3%. Finally, it is transported by the second auger mechanism and dried again using the heat of the iron powder itself, so that the final moisture content of the iron powder is controlled at about 0.1%. At the same time, the comprehensive cost of baking the iron powder is reduced to 45-50 yuan / ton of iron powder.

[0059] The new method for reducing the energy of iron powder baking provided by the present invention utilizes flowing airflow to assist the disc dehydrator in dehydration, and uniformly welding threaded steel on the surface of the dehydration disc can enhance the water filtering effect; the drying cylinder is designed as an outer cylinder sleeve inner cylinder mode, and both the outer cylinder and the inner cylinder adopt a "large and small head" mode, and the material enters from the inner cylinder and is discharged into the outer cylinder, and is discharged from the discharge end of the outer cylinder, so as to achieve the purpose of rationally utilizing the waste heat resources; rotating blades are arranged in the low-temperature preheating zone at the front end of the inner cylinder to prevent material agglomeration, and a water vapor collection device is arranged in the medium-temperature transition zone to extract water vapor to avoid water vapor The heat in the waste heat storage area in the outer cylinder is pumped to the first auger mechanism by means of negative pressure to assist in dehydration, and the cooled exhaust airflow is passed through the axial flow fan to assist in dehydrating the material at the discharge port of the disc dehydrator; the drying cylinder adopts a low-temperature baking mode to reduce the baking temperature, and adopts the second auger mechanism to transport the material, and through the process of turning the material by the second auger mechanism, the residual heat is used to bake the residual moisture; the new method provided by the present invention greatly reduces the moisture content of iron powder and the comprehensive cost of baking iron powder.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A new method for reducing iron powder baking energy, characterized in that: The following steps are involved: (1) grinding the iron-containing material with a ball mill, washing with a magnetic separator and a separator to obtain a wet concentrate; (2) transporting the wet concentrate to a dehydration device for dehydration; (3) The dehydrated material is transported to the drying device for drying through the first auger mechanism; the dried hot air flow is introduced into the first auger mechanism through the air inlet to assist in dehydrating the material, and then discharged from the air outlet of the first auger mechanism, and the air flow discharged from the air outlet is guided to the discharge port of the dehydration device by an axial flow fan to assist in dehydrating the material; wherein the flow direction of the hot air flow inside the first auger mechanism is opposite to the transportation direction of the material; (4) The dried iron powder is discharged from the discharge port of the drying device and transported to the storage device through the second auger mechanism.

2. The new method for reducing iron powder baking energy according to claim 1 is characterized in that: The particle size distribution of the wet concentrate in step (1) includes: +40 mesh 7-10%; 40-60 mesh 10-12%; 60-80 mesh 14-16%; 80-100 mesh 16-18%; -100 mesh 45-50%; The wet concentrate has a metallic iron content of 88-90%, a total iron content of 90-92% and a moisture content of 18-20%.

3. The new method for reducing iron powder baking energy according to claim 1 is characterized in that: The dehydration device in step (2) adopts a disc dehydrator, and 15-20 threaded steel bars with a diameter of 10 mm and a length of 300 mm are arranged on the surface of the dehydration disc of the disc dehydrator, and the threaded steel bars are evenly distributed along the center of the dehydration disc.

4. The new method for reducing iron powder baking energy according to claim 1 is characterized in that: In step (3), the air inlet is provided on one side of the discharge port of the first auger mechanism, and the air outlet is provided on one side of the feed port of the first auger mechanism; the axial flow fan is provided on one side of the air outlet, and the air outlet of the axial flow fan faces the discharge port of the dehydration device.

5. The new method for reducing iron powder baking energy according to claim 4 is characterized in that: The first auger mechanism is tilted, and the tilt angle is not less than 5-10 degrees; the first auger mechanism includes a box body, a spiral auger is arranged inside the box body, a feed port is arranged at the top of one end of the box body, and a discharge port is arranged at the bottom of one end of the box body, and the position of the discharge port is higher than the position of the feed port.

6. The new method for reducing iron powder baking energy according to claim 5 is characterized in that: The tops of both ends of the box body are respectively provided with 3-5 air inlet holes and air outlet holes, and the diameters of the air inlet holes and the air outlet holes are 30-50 mm; a drainage outlet is provided at one end of the box body close to the feed port.

7. The new method for reducing iron powder baking energy according to claim 4 is characterized in that: The drying device in step (3) includes a drying cylinder, a combustion chamber and a driving device for driving the drying cylinder to rotate, the drying cylinder includes an inner cylinder and an outer cylinder, a cavity is provided between the outer cylinder and the inner cylinder; the heat source outlet of the combustion chamber is connected to the heat source inlet of the inner cylinder, the feed port of the inner cylinder is connected to the discharge port of the first auger mechanism; the outer cylinder is provided with a discharge port at one end close to the heat source inlet.

8. The new method for reducing iron powder baking energy according to claim 7 is characterized in that: The diameters of both ends of the inner cylinder and the outer cylinder are different. The end with a smaller diameter of the inner cylinder is connected to the end with a larger diameter of the outer cylinder. The length of the outer cylinder is greater than the length of the inner cylinder. The end with a larger diameter of the inner cylinder is completely open, and the material is discharged from the end with a larger diameter of the inner cylinder into the outer cylinder.

9. The new method for reducing iron powder baking energy according to claim 8 is characterized in that: The interior of the inner cylinder is divided into a low-temperature preheating zone, a medium-temperature transition zone, and a high-temperature baking zone in sequence from the end with a smaller diameter to the end with a larger diameter; the inner cylinder is provided with 3-5 rotating blades in the low-temperature preheating zone; a water vapor collecting device is provided in the medium-temperature transition zone, and the water vapor collecting device discharges the water vapor inside the inner cylinder to the outside of the drying cylinder.

10. The new method for reducing iron powder baking energy according to claim 9, characterized in that: The area of ​​the outer cylinder near the end with a larger diameter is a waste heat storage area, and the area at the other end is a high-temperature baking area. The high-temperature baking area of ​​the outer cylinder is connected to the high-temperature baking area of ​​the inner cylinder, and the heat is pumped into the first auger mechanism in the waste heat storage area by means of negative pressure extraction; the drying device adopts low-temperature baking, and the temperature of the baked iron powder is controlled at 40-50°C, maintaining a small amount of moisture and carrying a small amount of waste heat. The residual moisture is baked by the second auger mechanism through the process of turning the material.

Citation Information

Patent Citations

  • Method for industrially producing iron powder by utilizing steelmaking sludge coarse particles

    CN118437748A

  • Sleeve type rotary drying apparatus

    CN2036650U

  • Energy-saving lithium battery raw material drying device

    CN209689323U

  • Multipurpose gathering combustion type rotary furnace

    CN209801494U

  • Drying device for bulk drug processing

    CN220793760U

Cited By

  • Ternary precursor powder drying device

    CN120333089A