Method for detecting amorphous oxide film in anode foil

By using an etching liquid composed of chromium trioxide and phosphoric acid to etch the anode foil, we can detect whether there are depressions on the surface of the anode foil, which solves the problem of cumbersome and high cost in traditional methods, and realizes the amorphous quality in the anode foil Fast, low-cost detection and thickness measurement of oxide films.

CN119086545APending Publication Date: 2024-12-06XINJIANG JOINWORLD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411190064.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional methods are used to detect the amorphous oxide film in the anode foil with cumbersome thickness and high cost, requiring high-precision cutting equipment, and the equipment is expensive, making it difficult to achieve fast and low-cost detection.

Method used

The anode foil is etched by etching liquid composed of chromium trioxide and phosphoric acid. By observing whether there are depressions on the surface morphology map, the existence and thickness of the amorphous oxide film is judged, avoiding slice processing and high-precision cutting. Use of the equipment.

Benefits of technology

The rapid and low-cost detection of amorphous oxide films in the anode foil is achieved, which reduces production costs and can be adjusted into processes in a timely manner to reach the preset thickness range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086545A_ABST
    Figure CN119086545A_ABST
Patent Text Reader

Abstract

The invention relates to a method for detecting an amorphous oxide film in an anode foil, which comprises the following steps of: performing etching treatment on the anode foil by using an etching solution to obtain a pretreated anode foil; the etching liquid comprises chromium trioxide and phosphoric acid; then carrying out a morphology test on the surface of the pretreated anode foil to obtain a surface morphology graph of the pretreated anode foil; and determining whether the amorphous oxide film exists in the anode foil or not according to the condition that whether pits exist in the surface morphology graph of the pretreated anode foil or not. According to the method, the anode foil is soaked in the etching solution with specific components, so that the amorphous oxide film in the anode foil can be soaked away, the pit is left, and the thickness value of the amorphous oxide film can be obtained according to the width of the pit. The method is simple to operate and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of testing and analysis, and in particular to a method for detecting an amorphous oxide film in an anode foil. Background Art

[0002] Aluminum electrolytic capacitors are widely used in consumer electronics, communication products, computers and peripheral products, instruments and meters, automation control, automotive industry, optoelectronic products, high-speed railways, aviation and military equipment, and anode foil is an important material for the preparation of aluminum electrolytic capacitors. In the manufacturing process of anode foil, tunnel holes are formed on the surface of aluminum foil through steps such as alkaline corrosion or acid corrosion, and the retained aluminum forms the tunnel hole wall. Then, the aluminum is oxidized through methods such as anodization to form a dense crystalline oxide film on the surface of the tunnel hole wall. This crystalline oxide film has a high dielectric constant and good insulation properties, and can store a large amount of charge, thereby giving the electrolytic capacitor a higher capacitance value.

[0003] In the process of forming the oxide film of the anode foil, in order to improve the quality of the oxide film and reduce the loss and leakage current of the anode foil after being prepared into a capacitor, a multi-stage formation process is usually adopted to form an amorphous oxide film on the inner layer of the crystalline oxide film, or to form an oxide film structure in which the crystalline oxide film and the amorphous oxide film alternate with each other in the direction from the inside to the outside of the tunnel hole wall. The amorphous oxide film can effectively reduce the leakage current and loss of the anode foil, so that the anode foil formed by this method can be used in fields that require the anode foil for capacitors to have low capacity, low leakage, low loss and low equivalent series resistance (ESR), such as spot welding machines; and the amorphous oxide film can improve the fast charge and discharge resistance of the anode foil. Based on the fact that the amorphous oxide film has an important influence on the fast charge and discharge resistance of the anode foil and the reduction of the loss and leakage current of the anode foil, it is necessary to timely know whether the amorphous oxide film in the anode foil in the formation process is formed and the thickness of the amorphous oxide film.

[0004] The traditional method for detecting the thickness of amorphous oxide films is to slice the anode foil, and then use a scanning electron microscope or a transmission electron microscope to observe the crystalline and amorphous thicknesses in the oxide film under high magnification conditions. However, during the slicing process, the accuracy of the sample after slicing is required to be high, and the sample needs to be cut to a thickness of about 1 micron, so the accuracy of the cutting equipment is also required to be high; and the slicing process requires a sharp cutter, and even ion light speed is required for cutting. In addition, in order to obtain a sample with a smooth surface, the sample needs to be frozen with liquid nitrogen before slicing. Therefore, the traditional slicing method has a cumbersome process, and the equipment accuracy requirements are also high. The equipment is expensive, and the production cost increases. Summary of the invention

[0005] Based on this, it is necessary to provide a method for detecting amorphous oxide film in anode foil which is simple to operate and low in cost.

[0006] In a first aspect, the present application provides a method for detecting an amorphous oxide film in an anode foil, the detection method comprising the following steps:

[0007] The anode foil is etched by an etching solution to obtain a pretreated anode foil; the etching solution comprises chromium trioxide and phosphoric acid;

[0008] Then, a morphology test is performed on the surface of the pretreated anode foil to obtain a surface morphology map of the pretreated anode foil;

[0009] Whether the anode foil has an amorphous oxide film is determined based on whether there are depression pits in the surface morphology of the pre-treated anode foil.

[0010] In the above method, an etching solution of a specific component is used to perform a first immersion treatment on the anode foil to obtain a pre-treated anode foil, and then a morphology test is performed on the surface of the pre-treated anode foil to obtain a surface morphology map of the pre-treated anode foil, and whether the anode foil contains an amorphous oxide film is determined based on the sunken pits in the surface morphology map. Among them, in the anode foil, compared with the crystalline oxide film, the amorphous oxide film has the characteristics of lower density, higher porosity and lower hardness. The amorphous oxide film is more easily separated from the original position by the action of chromium trioxide and phosphoric acid solution and etched away. From the surface of the pre-treated anode foil, it can be observed that the etched amorphous oxide film will leave a sunken pit at the original position. From the surface morphology map of the pre-treated anode foil, it can be observed whether there is a sunken pit, and it can be determined that the amorphous oxide film is contained in the anode foil; and then the anode foil formation process can be adjusted in time.

[0011] The above method does not require slicing of the anode foil, nor does it require the use of high-precision and expensive cutting equipment, which can reduce production costs to a certain extent.

[0012] In some embodiments, if there are depressions in the surface topography of the pre-treated anode foil, the thickness of the amorphous oxide film is obtained according to the width of the depressions in the surface topography of the pre-treated anode foil.

[0013] In some embodiments, the anode foil comprises tunnel holes extending in a thickness direction, and a surface topography of the pre-treated anode foil comprises concave pits arranged around the tunnel holes.

[0014] In some embodiments, the hole wall surface of the tunnel hole in the anode foil is an amorphous oxide film, and the etching process is controlled to etch a portion of the amorphous oxide film on the hole wall surface of the tunnel hole to form the concave pit.

[0015] In some embodiments, the hole wall of the tunnel hole in the anode foil is provided with stacked crystalline oxide film and amorphous oxide film in sequence from the surface to the inside, and the etching process etches the amorphous oxide film in the hole wall of the tunnel hole to form the depression pit in the area of ​​the amorphous oxide film.

[0016] In some embodiments, the shape of the depression is one or more of a ring shape, an arc shape, a quasi-arc shape, and a quasi-ring shape.

[0017] In some embodiments, the etching solution further comprises water, and the mass ratio of the chromium trioxide, the phosphoric acid and the water in the etching solution is 1:(3-4):(450-550); and / or,

[0018] The etching treatment conditions include: an etching temperature of 80° C. to 95° C.; and / or an etching time of 5 min to 15 min.

[0019] In some embodiments, before the anode foil is immersed in the etching solution, the step of grinding and polishing the surface of the anode foil is also included;

[0020] The steps of grinding and polishing include:

[0021] The surface of the anode foil is ground flat with sandpaper, and then polished with a polishing liquid;

[0022] The mesh number of the sandpaper is 600 mesh to 2000 mesh;

[0023] The average particle size of the abrasive in the polishing liquid is 3 μm to 9 μm.

[0024] In some embodiments, when sandpaper is used to grind the surface of the anode foil, at least two sandpapers with different mesh sizes are used in order from small to large to grind the surface of the anode foil; and / or,

[0025] When polishing the surface of the anode foil with the polishing liquid, at least two polishing liquids with different average abrasive particle sizes are used in order from large to small to polish the surface of the anode foil.

[0026] In some embodiments, before the step of grinding and polishing the surface of the anode foil, the step of embedding the anode foil in a resin matrix is ​​also included. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are merely embodiments of the present application, and ordinary technicians in this field can obtain other drawings based on the disclosed drawings without paying any creative work.

[0028] Figure 1 This is a SEM image of a cross section of a tunnel hole on the surface of an anode foil.

[0029] Figure 2 This is a SEM image of a cross section of an anode foil.

[0030] Figure 3 This is a SEM image of Example 1 of the present application obtained at a magnification of 2000 times.

[0031] Figure 4 This is the SEM picture of Example 1 of the present application obtained at a magnification of 10,000 times.

[0032] Figure 5 This is the SEM image of Example 2 of the present application obtained at a magnification of 2000 times.

[0033] Figure 6 This is the SEM image of Example 2 of the present application obtained at a magnification of 20,000 times.

[0034] Figure 7 This is the SEM image of Example 3 of the present application obtained at a magnification of 20,000 times.

[0035] Figure 8 This is the SEM image of Example 4 of the present application obtained at a magnification of 20,000 times.

[0036] Fig. 9 This is the SEM image of Example 5 of the present application obtained at a magnification of 20,000 times.

[0037] Fig.10 This is the SEM image of Example 6 of the present application obtained at a magnification of 20,000 times.

[0038] Fig.11 This is the SEM image of Example 7 of the present application obtained at a magnification of 20,000 times.

[0039] Fig.12 This is the SEM picture of Comparative Example 1 of the present application obtained at a magnification of 2000 times. DETAILED DESCRIPTION

[0040] In order to facilitate the understanding of the present invention, the present invention is described more comprehensively below. And preferred embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0042] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0043] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0044] See also Figure 1 and Figure 2 During the preparation process, the anode foil is treated with corrosion to form a tunnel hole extending along the thickness direction of the aluminum foil on the surface of the aluminum foil; from the cross-section of the anode foil, the aluminum column structure retained after corrosion forms the hole wall of the tunnel hole; see Figure 1On the cross section of the aluminum column, it can be observed that the tunnel holes present individual cylindrical tunnel holes 1-3, serially connected tunnel holes 1-1, and clustered connected tunnel holes 1-2. These tunnel holes can significantly increase the specific surface area of ​​the anode foil, thereby increasing the capacitance of the capacitor. Further, through the anodizing process, the aluminum on the wall of the tunnel hole can be oxidized, thereby forming a crystalline oxide film on the surface of the wall of the tunnel hole. This crystalline oxide film has a high dielectric constant and good insulation properties, and can store a large amount of charge, thereby giving the electrolytic capacitor a higher capacitance value. In order to further reduce the leakage current and loss of the anode foil, the crystallinity of the oxide film can be controlled by improving the multi-stage anodizing process, and an oxide film structure of amorphous oxide film and crystalline oxide film can be formed from the inside to the outside of the wall of the tunnel hole, or an oxide film structure of crystalline oxide film and amorphous oxide film can be obtained from the inside to the outside. The film alternates multiple times.

[0045] The traditional method for detecting amorphous oxide film in anode foil is to slice the anode foil. This method has very high requirements on sample accuracy and equipment accuracy. The slicing equipment is expensive, which increases the detection cost. Based on this, the present application provides a method for detecting amorphous oxide film in anode foil as shown below.

[0046] In one embodiment of the present application, a method for detecting an amorphous oxide film in an anode foil is provided, comprising the following steps S10 to S30.

[0047] S10, etching the anode foil with an etching solution to obtain a pretreated anode foil; the etching solution includes chromium trioxide and phosphoric acid;

[0048] S20, then performing a morphology test on the surface of the pretreated anode foil to obtain a surface morphology map of the pretreated anode foil;

[0049] S30, determining whether the anode foil has an amorphous oxide film according to whether there are depression pits in the surface morphology image of the pre-treated anode foil.

[0050] Specifically, if there are depression pits in the surface morphology of the pre-treated anode foil, it is determined that the anode foil has an amorphous oxide film. If there are no depression pits in the surface morphology of the pre-treated anode foil, it is determined that the anode foil has no amorphous oxide film.

[0051] In the above method, an etching solution of a specific component is used to perform a first immersion treatment on the anode foil to obtain a pretreated anode foil, and then a morphology test is performed on the surface of the pretreated anode foil to obtain a surface morphology map of the pretreated anode foil. Whether the anode foil contains an amorphous oxide film is determined based on the sunken pits in the surface morphology map. Among them, in the anode foil, compared with the crystalline oxide film, the amorphous oxide film has the characteristics of lower density, higher porosity and lower hardness. The amorphous oxide film is more easily separated from the original position by the action of chromium trioxide and phosphoric acid solution and etched away. From the surface morphology map of the pretreated anode foil, it can be observed that the etched amorphous oxide film leaves a sunken pit at the original position. Therefore, by observing whether there is a sunken pit from the surface morphology map of the pretreated anode foil, it can be determined whether the anode foil contains an amorphous oxide film. Then, the anode foil formation process can be adjusted in time.

[0052] The above method does not require slicing of the anode foil, nor does it require the use of high-precision and expensive cutting equipment, which can reduce production costs to a certain extent.

[0053] The etching treatment refers to the step of immersing the anode foil in an etching solution.

[0054] In some embodiments, if there is a concave pit in the surface topography of the pre-treated anode foil, the thickness value of the amorphous oxide film is obtained according to the width of the concave pit in the surface topography of the pre-treated anode foil. The thickness of the amorphous oxide film is obtained according to the width of the concave pit, and the anode foil forming process can be adjusted in time according to the thickness value, so that the thickness of the amorphous oxide film reaches a preset thickness range.

[0055] In some embodiments, the method for obtaining the thickness value of the amorphous oxide film according to the width of the depression pit in the surface topography of the pre-treated anode foil includes:

[0056] In the process of forming an amorphous oxide film on the surface of the anode foil, in the same time period and in the same tank, the oxide film thickness formed at different positions on the surface of the anode foil is the same, and the thickness of the amorphous oxide film formed is also the same. In the same morphology diagram, the width of a depression pit at one position can be measured as the thickness value of the amorphous oxide film in the anode foil. Alternatively, in the same morphology diagram, the average value of the width of depression pits at at least 3 different positions is measured as the thickness value of the amorphous oxide film in the anode foil. Furthermore, when taking the thickness of depression pits at different positions, the thickness values ​​of depression pits of different shapes can be taken.

[0057] In some embodiments, the anode foil comprises tunnel holes extending in the thickness direction, and the depressions are arranged around the tunnel holes.

[0058] In some embodiments, the hole wall surface of the tunnel hole in the anode foil is an amorphous oxide film, and the etching process is controlled to etch a portion of the amorphous oxide film on the hole wall surface of the tunnel hole to form a concave pit. It can be understood that when the etching process is controlled to etch a portion of the amorphous oxide film on the hole wall surface of the tunnel hole, the amorphous oxide film on the hole wall surface is not completely eroded and an observable concave pit is left, which can prevent the amorphous oxide film on the hole wall surface from being completely etched without a concave pit, resulting in a misjudgment when determining whether there is an amorphous oxide film.

[0059] In some embodiments, the hole wall of the tunnel hole in the anode foil is provided with a stacked crystalline oxide film and an amorphous oxide film in sequence from the surface to the inside, and the etching process etches the amorphous oxide film on the hole wall surface of the tunnel hole to form a concave pit in the area of ​​the amorphous oxide film. It can be understood that the hole wall from the surface to the inside refers to the direction from the hole wall surface to the inner layer of the hole wall, that is, the direction gradually away from the tunnel hole.

[0060] In some embodiments, the shape of the above-mentioned concave pit is one or more of a circular ring shape, an arc shape, a quasi-circular ring shape and a quasi-circular arc shape.

[0061] In some embodiments, the etching solution further includes water, and the mass ratio of chromium trioxide, phosphoric acid and water in the etching solution is 1: (3-4): (450-550). As an example, the mass ratio of chromium trioxide, phosphoric acid and water in the etching solution can be 1: 3.3: 500. By controlling the proportion of each component in the etching solution, the amorphous oxide film can be corroded and dissolved from the anode foil, while the crystalline oxide film is not dissolved.

[0062] The etching treatment refers to the step of immersing the anode foil in an etching solution.

[0063] In some embodiments, the immersion temperature of the above-mentioned etching treatment is 80° C. to 95° C. As an example, the immersion temperature of the first immersion treatment can be 80° C., 81° C., 82° C., 83° C., 84° C., 85° C., 86° C., 87° C., 88° C., 89° C., 90° C., 91° C., 92° C., 93° C., 94° C. or 95° C. Controlling the immersion temperature can make the amorphous oxide film react quickly with the etching solution, thereby reducing the time cost of detection.

[0064] In some embodiments, the immersion time of the etching treatment is 5 minutes to 15 minutes. As an example, the immersion time of the first immersion treatment can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes. Controlling the immersion time can allow the amorphous oxide film and the etching solution to have enough reaction time to leave a concave pit while preventing the amorphous film from being completely etched away.

[0065] In some embodiments, the amorphous oxide film is an amorphous aluminum oxide film.

[0066] In some embodiments, the surface of the anode foil further includes a crystalline oxide film.

[0067] In some embodiments, the crystalline oxide film is a crystalline aluminum oxide film.

[0068] In some embodiments, the thickness of the amorphous oxide film in the anode foil is 50 nm to 600 nm.

[0069] In some embodiments, the morphology test of the surface of the pre-treated anode foil may be performed by observation using a scanning electron microscope or a transmission electron microscope.

[0070] In some embodiments, before the anode foil is immersed in the etching solution, the step of grinding and polishing the surface of the anode foil is also included.

[0071] The steps of grinding and polishing include:

[0072] The surface of the anode foil is ground flat with sandpaper and then polished with polishing liquid;

[0073] The mesh number of sandpaper is 600~2000;

[0074] The average particle size of the abrasive in the polishing liquid is 3μm~9μm.

[0075] As an example, the mesh number of the sandpaper may be 600 mesh, 800 mesh, 900 mesh, 1000 mesh, 1100 mesh, 1200 mesh, 1500 mesh, 1800 mesh or 2000 mesh. Further, the mesh number of the sandpaper may be a range value consisting of any two of the above point values ​​as end values.

[0076] As an example, the average particle size of the abrasive in the polishing liquid is 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm or 9 μm. Furthermore, the average particle size of the abrasive in the polishing liquid can be a range value consisting of any two of the above point values ​​as end values. The surface of the anode foil is first ground with sandpaper, and then polished with a polishing liquid, so that a smooth anode foil can be obtained, and the concave pits left after the amorphous oxide film in the anode foil reacts with the etching solution are easier to observe.

[0077] In some embodiments, when sandpaper is used to grind the surface of the anode foil, at least two sandpapers with different mesh sizes are used in order from small to large to grind the surface of the anode foil.

[0078] The flattening treatment refers to the use of sandpaper to rub the surface of the anode foil to make the surface of the anode foil flat, wherein flatness means that the surface of the anode foil is flat when observed by naked eyes without depressions and protrusions.

[0079] As an example, when sandpapers with 600 mesh, 1000 mesh and 2000 mesh are used to grind the surface of the anode foil, the order of grinding is: first grind the surface of the anode foil with 600 mesh sandpaper, then grind the surface of the anode foil with 1000 mesh sandpaper, and finally grind the surface of the anode foil with 2000 mesh sandpaper. The surface of the anode foil can be further smoothed by using at least two sandpapers with different meshes in order from small to large.

[0080] In some embodiments, each time the surface of the anode foil is smoothed using sandpaper, the single smoothing time is 1 min to 3 min.

[0081] In some embodiments, when sandpaper is used to grind the surface of the anode foil, water is used to rinse the surface while grinding.

[0082] In some embodiments, the sandpaper is selected from at least one of metallographic sandpaper and water-abrasive sandpaper.

[0083] In some embodiments, when polishing the surface of the anode foil with a polishing liquid, at least two polishing liquids with different average abrasive particle sizes are used in order from large to small to polish the surface of the anode foil.

[0084] As an example, when the surface of the anode foil is polished using two polishing liquids with different average particle sizes of abrasives of 9 μm and 3 μm respectively, the surface of the anode foil is first polished using the polishing liquid with an average particle size of abrasives of 9 μm, and then the surface of the anode foil is polished using the polishing liquid with an average particle size of abrasives of 3 μm.

[0085] In some embodiments, the polishing liquid is at least one of a diamond polishing liquid, a silicon dioxide polishing liquid, and a silicon carbide polishing liquid.

[0086] In some embodiments, when the surface of the anode foil is polished with a polishing liquid, the polishing liquid should be used in conjunction with a polishing cloth. As an example, a short-neck polishing cloth is attached to a mechanical polishing disc (the mechanical polishing disc rotates at 300 rpm), and then a 9μm polishing liquid is added to the polishing cloth, and the surface of the anode foil is polished for 1min to 3min, and then a 3μm polishing liquid is added, and the surface of the anode foil is polished for 1min to 3min, until the surface of the sample is smooth and has no obvious scratches.

[0087] In some embodiments, when the surface of the anode foil is polished, the surface of the anode foil needs to be polished off by 10 μm to 12 μm. Polishing off the surface thickness of the anode foil by 10 μm to 12 μm can make it easier to observe the cross section of the tunnel holes in the anode foil and more accurately observe whether there are pits left by the amorphous film.

[0088] In some embodiments, before the step of polishing the surface of the anode foil, the step of embedding the anode foil in a resin matrix is ​​also included.

[0089] In some embodiments, the method of embedding the anode foil in the resin matrix comprises the following steps:

[0090] Provide anode foil samples, aluminum sheets, sample making molds, and resin embedding liquid to be tested.

[0091] According to the size of the sample making mold, the anode foil sample and the aluminum sheet to be tested are trimmed and sampled, and the anode foil sample to be tested is pasted and fixed on the aluminum sheet to obtain a fixed sample to be tested.

[0092] Place the fixed sample to be tested parallel to the bottom of the sample preparation mold.

[0093] Pour the resin embedding liquid into the sample preparation mold and solidify it.

[0094] In some embodiments, the resin embedding solution includes epoxy resin, dibutyl phthalate and ethylenediamine.

[0095] In some embodiments, the volume ratio of epoxy resin, dibutyl phthalate and ethylenediamine in the resin embedding solution is 10: (1-2): (0.5-1.5).

[0096] In some embodiments, after the anode foil is etched with an etchant, the pre-treated anode foil is soaked in water at 30° C. to 40° C. The pre-treated anode foil is soaked in water to remove the etchant on the surface of the anode foil, thereby preventing the residual etchant components from further corroding the amorphous oxide film.

[0097] In some embodiments, the immersion treatment is to immerse the pretreated anode foil in water at least twice, and the time of each immersion treatment is 0.5h to 2h.

[0098] In some embodiments, the soaking treatment is to soak the pretreated anode foil in water for 5 to 8 times.

[0099] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0100] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.

[0101] Example 1

[0102] This embodiment tests the 560vf anode foil, and the steps are as follows:

[0103] Anode foil embedded in resin:

[0104] (1) Take samples of the anode foil to be tested, with a sampling size of approximately 1.5 cm*1.5 cm.

[0105] (2) According to the size of the sample preparation mold, the sample of the anode foil is fixed: the anode foil is pasted on the aluminum foil to fix it, and a fixed sample to be tested is obtained; the fixed sample to be tested is placed parallel to the bottom of the sample preparation mold.

[0106] (3) Prepare a liquid according to the ratio of epoxy resin: dibutyl phthalate: ethylenediamine = 10:1.5:1 (volume ratio) to obtain a resin mixed solution. Gently stir the solution during the preparation process to prevent the generation of a large number of bubbles.

[0107] (4) Slowly pour the prepared resin mixed solution into the sample preparation mold to minimize the generation of bubbles. Then let the mold stand at 20°C for 24 hours until the resin mixed solution is completely solidified. Then take it out and obtain the embedded anode foil sample.

[0108] (5) The surface of the mounted anode foil sample was ground and polished: first, the surface of the anode foil was mechanically ground for 2 min using 600-mesh, 1000-mesh, and 2000-mesh metallographic sandpapers respectively (water should be added automatically to rinse the sandpaper during the grinding process); then, a short-neck polishing cloth was attached to a mechanical polishing disc (the mechanical polishing disc speed was 300 rpm), and 9 μm polishing liquid was added to the polishing cloth, and the surface of the anode foil was polished for 2 min, and then 3 μm polishing liquid was added to the polishing cloth, and the surface of the anode foil was polished for 2 min. The surface of the sample was smooth without obvious scratches.

[0109] Anode foil soaking steps:

[0110] (1) The polished anode foil sample is placed in an etching solution for the first immersion treatment. The ratio of the etching solution is chromium trioxide: 85% phosphoric acid by mass: water = 1:3.3:500 (weight ratio); wherein the immersion temperature is maintained at 90°C and the immersion time is 10 min. During the immersion process, the polished surface faces upward and the surface of the anode foil is completely immersed in the etching solution.

[0111] (2) After the first immersion treatment is completed, place the sample on its side in pure water at 30℃~40℃ for immersion. Replace the pure water every 60 minutes and replace it 5-8 times to clean the immersion liquid on the surface of the sample.

[0112] (3) Take the sample out of the pure water, let it dry at room temperature, and then observe the cross section under an electron microscope.

[0113] Anode foil electron microscopy steps:

[0114] (1) The cleaned sample is placed in an ion sputtering device for gold spraying to make the surface of the anode foil conductive.

[0115] (2) The embedded samples were observed using a German Zeiss EV050 SEM.

[0116] (3) Observe samples at different magnifications: 2000x, 10000x, and 20000x.

[0117] (4) When observing the sample under a scanning electron microscope, it is necessary to first observe at a small magnification. After seeing a single or multiple holes, use a high magnification to take pictures and read the thickness of the amorphous oxide film.

[0118] See also Figure 3 and Figure 4 , Figure 3 This is the SEM picture of Example 1 obtained at a magnification of 2000 times. Figure 4 This is a SEM picture of Example 1 obtained at a magnification of 10,000 times. Figure 4 There is a depression pit set in the tunnel hole at the position 4-1 in the figure. This depression pit is a depression pit left by the amorphous oxide film, and the width of the depression pit Pa2=495.8nm, which means that the 560vf anode foil tested in this embodiment contains an amorphous oxide film, and the thickness of the amorphous oxide film is 495.8nm. Figure 4 There are irregular holes and pits at the 4-2 position in the figure. The pits here are uneven defects left after grinding and polishing. Figure 4 It can be seen that the tunnel hole contains particles, which may be resin particles filled in the tunnel hole; the distance between the resin particles and one side wall of the tunnel hole is Pa1=882.0nm.

[0119] Example 2

[0120] The test conditions used in this embodiment are basically the same as those in Embodiment 1, except that the test is conducted on a 590vf anode foil in this embodiment.

[0121] See also Figure 5 and Figure 6 , Figure 5 This is the SEM picture of Example 2 obtained at a magnification of 2000 times. Figure 6 This is a SEM picture obtained at a magnification of 20,000 times in Example 2. From the picture, it can be seen that there is an obvious annular depression pit on the tunnel hole wall, and the thickness of the depression pit is Pa1=619.7nm; that is, the 590vf anode foil tested in this example contains an amorphous oxide film, and the amorphous oxide film is arranged on the hole wall surface of the tunnel hole, and the thickness of the amorphous oxide film is 619.7nm.

[0122] Example 3

[0123] The test conditions used in this embodiment are basically the same as those in Embodiment 1, except that this embodiment tests 600vf anode foil.

[0124] See also Figure 7 , Figure 7 This is a SEM picture obtained at a magnification of 20,000 times in Example 3. From the picture, it can be seen that there is an obvious annular depression pit on the tunnel hole wall, and the thickness of the depression pit is Pa1=781.6nm; that is, the 700vf anode foil tested in this embodiment contains an amorphous oxide film, and the amorphous oxide film is arranged on the hole wall surface of the tunnel hole, and the thickness of the amorphous oxide film is 781.6nm.

[0125] Example 4

[0126] The test conditions used in this embodiment are basically the same as those in Embodiment 1, except that the test is conducted on a 670vf anode foil in this embodiment.

[0127] See also Figure 8 , Figure 8 This is the SEM picture of Example 4 obtained at a magnification of 20,000 times. From the figure, it can be seen that there are annular hole walls and annular depressions from the hole wall surface to the inside of the tunnel hole, and the thickness of the annular hole wall is Pa2 = 591.8nm, and the thickness of the annular depression is Pa1 = 110.0nm. That is, the 670vf anode foil tested in this embodiment contains an amorphous oxide film, and in the direction from the hole wall surface to the inside of the tunnel hole, there are crystalline oxide film, amorphous oxide film and crystalline oxide film respectively, among which the thickness of the amorphous oxide film is 110.0nm.

[0128] Example 5

[0129] The test conditions used in this embodiment are basically the same as those in Embodiment 1, except that the test is conducted on 800 VF anode foil in this embodiment.

[0130] See also Fig. 9 , Fig. 9 This is the SEM picture obtained at a magnification of 20,000 times in Example 5. From the figure, it can be seen that there are hole walls and annular depressions from the hole wall surface to the inside of the tunnel hole, and the thickness of the annular hole wall is Pa2 = 932.4nm, and the thickness of the annular depression is Pa1 = 212.2nm. That is, it can be seen from the figure that the 800vf anode foil tested in this embodiment contains an amorphous oxide film, and in the direction from the hole wall surface to the inside of the tunnel hole, there are crystalline oxide film, amorphous oxide film and crystalline oxide film respectively, and the thickness of the amorphous oxide film is 212.2nm.

[0131] Example 6

[0132] The test conditions used in this embodiment are basically the same as those in Embodiment 1, except that this embodiment tests 600vf anode foil.

[0133] See also Fig.10 , Fig.10 This is the SEM picture obtained at a magnification of 20,000 times in Example 6. From the figure, it can be seen that from the surface of the tunnel wall to the inside, there are the first hole wall, the first concave pit, the second hole wall, and the second concave pit in sequence; among which, the thickness of the first hole wall is Pa3 = 139.7nm, the thickness of the first concave pit is Pa4 = 111.6nm, the thickness of the second hole wall is Pa2 = 212.1nm, and the thickness of the second concave pit is Pa1 = 217.2nm; among which, the distance from the surface of the tunnel hole wall to the side wall of the second concave pit away from the tunnel hole is Pa5 = 666.7nm. That is to say, the 600vf anode foil tested in this embodiment contains an amorphous oxide film, and in the direction from the hole wall surface to the inside of the tunnel hole, there are crystalline oxide film, amorphous oxide film, crystalline oxide film, amorphous oxide film and crystalline oxide film respectively; and the thickness of the amorphous oxide film closer to the tunnel hole is 139.7nm, and the thickness of the amorphous oxide film farther from the tunnel hole is 217.2nm.

[0134] Example 7

[0135] The test conditions used in this embodiment are basically the same as those in Embodiment 1, except that this embodiment tests the anode foil 560vf without a specially prepared amorphous oxide film.

[0136] See also Fig.11 , Fig.11This is a SEM picture obtained at a magnification of 20,000 times in Example 7. It can be seen from the figure that there is no concave pit arranged around the tunnel hole in the direction from the hole wall to the inside, that is, it can be determined that the 560vf anode foil tested in this example does not contain a specially prepared amorphous oxide film.

[0137] Comparative Example 1

[0138] The steps of this comparative example are basically the same as those of Example 1, except that the etching solution is not used to immerse the anode foil sample to be tested in this comparative example.

[0139] This embodiment tests the 560vf anode foil, and the steps are as follows:

[0140] Anode foil inlay steps:

[0141] (1) Take samples of the anode foil to be tested, with a sampling size of approximately 1.5 cm*1.5 cm.

[0142] (2) According to the size of the sample preparation mold, the sample of the anode foil is fixed: the anode foil is pasted on the aluminum foil to fix it, and a fixed sample to be tested is obtained; the fixed sample to be tested is placed parallel to the bottom of the sample preparation mold.

[0143] (3) Prepare a liquid according to the ratio of epoxy resin: dibutyl phthalate: ethylenediamine = 10:1.5:1 (volume ratio) to obtain a resin mixed solution. Gently stir the solution during the preparation process to prevent the generation of a large number of bubbles.

[0144] (4) Slowly pour the prepared resin mixed solution into the sample preparation mold to minimize the generation of bubbles. Then let the mold stand at 20°C for 24 hours until the resin mixed solution is completely solidified. Then take it out and obtain the embedded anode foil sample.

[0145] (5) Grind and polish the surface of the mounted anode foil sample: first, use 600 mesh, 1000 mesh, and 2000 mesh metallographic sandpaper to grind the surface of the anode foil for 2 minutes respectively (during the grinding process, water should be added automatically to rinse the sandpaper); then attach a short-neck polishing cloth to a mechanical polishing disc (the speed of the mechanical polishing disc is 300 rpm), first add 9μm polishing liquid to the polishing cloth, and polish the surface of the anode foil for 2 minutes, then add 3μm polishing liquid, and polish the surface of the anode foil for 2 minutes.

[0146] Anode foil electron microscopy steps:

[0147] (1) The polished sample is placed in an ion sputtering device for gold spraying to make the surface of the anode foil conductive.

[0148] (2) The embedded samples were observed using a German Zeiss EV050 SEM.

[0149] (3) Observe samples at different magnifications: 2000x, 10000x, and 20000x.

[0150] (4) When observing the sample under a scanning electron microscope, it is necessary to first observe at a small magnification. After seeing a single or multiple holes, use a high magnification to take pictures and read the thickness of the amorphous oxide film.

[0151] See also Fig.12 , Fig.12 This is the SEM picture of comparative example 1 obtained at a magnification of 2000 times. It can be seen from the figure that there are no sunken pits arranged around the tunnel hole in the direction from the hole wall to the inside, which means that the surface of the anode foil of this embodiment is not immersed, and it is impossible to observe whether there is an amorphous oxide film in the oxide film.

[0152] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0153] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A method for detecting an amorphous oxide film in an anode foil, characterized in that: The detection method comprises the following steps: The anode foil is etched by an etching solution to obtain a pretreated anode foil; the etching solution comprises chromium trioxide and phosphoric acid; Then, a morphology test is performed on the surface of the pretreated anode foil to obtain a surface morphology map of the pretreated anode foil; Whether the anode foil has an amorphous oxide film is determined based on whether there are depression pits in the surface morphology of the pre-treated anode foil.

2. The detection method according to claim 1, characterized in that If there are concave pits in the surface topography of the pre-treated anode foil, the thickness value of the amorphous oxide film is obtained according to the width of the concave pits in the surface topography of the pre-treated anode foil.

3. The detection method according to claim 2, characterized in that The anode foil comprises tunnel holes extending in a thickness direction, and a surface topography of the pre-treated anode foil comprises concave pits arranged around the tunnel holes.

4. The detection method according to claim 3, characterized in that The hole wall surface of the tunnel hole in the anode foil is an amorphous oxide film, and the etching process is controlled to etch part of the amorphous oxide film on the hole wall surface of the tunnel hole to form the concave pit.

5. The detection method according to claim 3, characterized in that: The hole wall of the tunnel hole in the anode foil is provided with a stacked crystalline oxide film and an amorphous oxide film in sequence from the surface to the inside, and the etching process etches the amorphous oxide film in the hole wall of the tunnel hole to form the concave pit in the area of ​​the amorphous oxide film.

6. The detection method according to any one of claims 1 to 5, characterized in that The shape of the concave pit is one or more of a circular ring, an arc, a quasi-arc shape and a quasi-circular ring shape.

7. The detection method according to any one of claims 1 to 5, characterized in that The etching solution also includes water, and the mass ratio of the chromium trioxide, the phosphoric acid and the water in the etching solution is 1: (3-4): (450-550); and / or, The etching treatment conditions include: an etching temperature of 80° C. to 95° C.; and / or an etching time of 5 min to 15 min.

8. The detection method according to any one of claims 1 to 5, characterized in that Before the anode foil is soaked in the etching solution, the method further includes the step of grinding and polishing the surface of the anode foil; The steps of grinding and polishing include: The surface of the anode foil is ground flat with sandpaper, and then polished with a polishing liquid; The mesh number of the sandpaper is 600 mesh to 2000 mesh; The average particle size of the abrasive in the polishing liquid is 3 μm to 9 μm.

9. The detection method according to claim 8, characterized in that When sandpaper is used to grind the surface of the anode foil, at least two sandpapers with different mesh sizes are used in order from small to large to grind the surface of the anode foil; and / or, When polishing the surface of the anode foil with the polishing liquid, at least two polishing liquids with different average abrasive particle sizes are used in order from large to small to polish the surface of the anode foil.

10. The detection method according to claim 8, characterized in that: Before the step of grinding and polishing the surface of the anode foil, the method further includes the step of embedding the anode foil in a resin matrix.