Bismuth oxyiodide / carbon nitride composite material, preparation method and application thereof, self-energized electrochemical sensor and application thereof

By using the p-n heterojunction structure of bismuth oxide/carbon nitride composite in traditional electrochemical sensors, the photoelectric conversion efficiency is improved, and the traditional detection method is solved with high cost, complex operation and external power supply required, and the problem of the traditional detection method is achieved. High sensitivity detection and self-powering function of heavy metal ions.

CN119086673APending Publication Date: 2024-12-06NORTHEAST GASOLINEEUM UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411187550.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional heavy metal ion detection methods have the limitations of high cost, complex operation, long time consumption and external power supply, and the photoelectric conversion efficiency of traditional electrochemical sensors is low.

Method used

The p-n heterojunction structure is prepared by hydrothermal reaction by using bismuth iodide/carbon nitride composite material as the photoelectric anode, and used for self-energized electrochemical sensors, and combined with photocatalytic fuel cells to achieve self-powered power function.

Benefits of technology

It improves the photoelectric conversion efficiency, realizes high sensitivity detection of Cd2+ (limited to 0.033μM), has excellent selectivity, stability and self-powering capabilities, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086673A_ABST
    Figure CN119086673A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of heavy metal ion detection, and particularly relates to a bismuth oxyiodide / carbon nitride composite material, a preparation method and application thereof, a self-energized electrochemical sensor and application thereof. In the invention, the p-n heterojunction between the BiOI and the CN not only retains the structural characteristics of the BiOI and the CN, but also has a larger specific surface area, so that the BiOI / CN heterojunction has more active sites; meanwhile, due to the formation of the heterojunction, the transmission path of electrons is changed, the separation and migration efficiency of photon-generated carriers is improved, and the photoelectric property is excellent. According to the test result of the embodiment, the detection limit of the BiOI / CN-34%-based p-n heterojunction sensor to Cd < 2 + > is as low as 0.033 mu M (the signal-to-noise ratio (S / N = 3)), and meanwhile, the BiOI / CN-34%-based p-n heterojunction sensor has excellent selectivity, stability, repeatability and certain self-powered capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of heavy metal ion detection, and specifically relates to a bismuth iodide oxide / carbon nitride composite material and a preparation method and application thereof, a self-powered electrochemical sensor and application thereof. Background Art

[0002] Traditional heavy metal ion detection methods mainly include ultraviolet spectroscopy, flame atomic absorption spectroscopy, atomic absorption spectroscopy, inductively coupled plasma atomic emission spectroscopy and inductively coupled plasma mass spectrometry, but these methods have disadvantages such as high cost, complex operation, time-consuming, and the need for support from professional technicians.

[0003] Electrochemical sensors have the advantages of low cost, simple operation, high sensitivity and fast response speed, but traditional electrochemical sensors still have the limitation of requiring an external power supply. The new photocatalytic fuel cell self-powered electrochemical sensor platform combines electrochemical sensing technology with photocatalytic fuel cells. It not only has the advantages of electrochemical sensors, but also can convert energy in the environment to achieve its own energy supply. It does not require an external power supply or bias voltage, and has the advantage of energy saving. Self-powered electrochemical sensors mainly include photoelectrodes and electrolytes. The performance of the photoelectrode material determines the performance of the self-powered electrochemical sensor, but the current photoelectric conversion efficiency of the photoelectrode needs to be further improved. Summary of the invention

[0004] The purpose of the present invention is to provide a bismuth iodide / carbon nitride composite material and its preparation method and application, a self-powered electrochemical sensor and its application. The present invention provides a photoanode prepared from the bismuth iodide / carbon nitride composite material, which has excellent photoelectric conversion efficiency when applied to a self-powered electrochemical sensor.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a bismuth oxyiodide / carbon nitride composite material, comprising a bismuth oxyiodide matrix and carbon nitride supported on the surface of the bismuth oxyiodide matrix;

[0007] A pn heterojunction structure is formed between the bismuth oxyiodide matrix and the carbon nitride.

[0008] Preferably, the mass of the carbon nitride is 10-60% of the mass of the bismuth oxyiodide matrix.

[0009] The present invention also provides a method for preparing the bismuth oxyiodide / carbon nitride composite material described in the above technical solution, comprising the following steps:

[0010] Bismuth salt, iodine salt, ethylene glycol, polyvinyl pyrrolidone and carbon nitride are mixed and subjected to hydrothermal reaction to obtain the bismuth oxyiodide / carbon nitride composite material.

[0011] Preferably, the bismuth salt comprises bismuth nitrate; the iodine salt comprises potassium iodide; the molar ratio of the bismuth salt to the iodine salt is 1.0 to 1.1:1;

[0012] The dosage ratio of the bismuth salt to ethylene glycol is 1.0-1.1 mol: 70-90 mL;

[0013] The usage ratio of polyvinyl pyrrolidone to ethylene glycol is 0.15-0.25 g:70-90 mL.

[0014] Preferably, the mixing comprises:

[0015] The bismuth salt and the iodine salt are dispersed in ethylene glycol, and then polyvinyl pyrrolidone is added to stir and dissolve to obtain a mixed solution; the carbon nitride is added to the mixed solution to perform ultrasonic dispersion.

[0016] Preferably, the temperature of the hydrothermal reaction is 140-180° C., and the time is 12-16 hours.

[0017] The present invention also provides the use of the bismuth oxyiodide / carbon nitride composite material described in the above technical solution or the bismuth oxyiodide / carbon nitride composite material prepared by the preparation method described in the above technical solution as an electrode material in a self-powered electrochemical sensor.

[0018] The present invention also provides a self-powered electrochemical sensor, comprising a photoanode, a cathode and an electrolyte, wherein the electrode material on the photoanode is the bismuth oxyiodide / carbon nitride composite material described in the above technical scheme or the bismuth oxyiodide / carbon nitride composite material prepared by the preparation method described in the above technical scheme.

[0019] Preferably, the cathode comprises carbon paper and a cathode material loaded on the carbon paper; the cathode material comprises iron phthalocyanine; and the electrolyte is a nitric acid solution.

[0020] The present invention also provides the self-powered electrochemical sensor described in the above technical solution for detecting Cd 2+ Application in.

[0021] The present invention provides a bismuth iodide / carbon nitride composite material, comprising a bismuth iodide matrix and carbon nitride loaded on the surface of the bismuth iodide matrix; a pn heterojunction structure is formed between the bismuth iodide matrix and the carbon nitride. In the present invention, the pn heterojunction between BiOI / CN not only retains the structural characteristics of BiOI and CN, but also has a larger specific surface area, so that it has more active sites; at the same time, the formation of the heterojunction changes the transmission path of electrons, improves the separation and migration efficiency of photogenerated carriers, and has excellent photoelectric properties. According to the test results of the embodiment, the pn heterojunction sensor based on BiOI / CN-34% has a good performance on Cd 2+ The detection limit is as low as 0.033 μM (signal-to-noise ratio (S / N=3)), and it has excellent selectivity, stability, repeatability and a certain self-powered capability.

[0022] The present invention also provides a method for preparing the bismuth oxyiodide / carbon nitride composite material described in the above technical solution, comprising the following steps: mixing bismuth salt, iodide salt, ethylene glycol, polyvinyl pyrrolidone and carbon nitride, and performing a hydrothermal reaction to obtain the bismuth oxyiodide / carbon nitride composite material. The present invention adopts a one-step hydrothermal method to react BiOI with gC 3 N 4 (CN) coupling, and further constructed a photocatalytic self-powered electrochemical sensor based on BiOI / CN pn heterojunction photoanode, and used it to detect Cd 2+ This method simplifies the preparation process and avoids the complicated and cumbersome two-step process required by most heterojunction preparation schemes. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a SEM image of the bismuth oxyiodide / carbon nitride composite material obtained in Example 1;

[0024] Figure 2 The XRD patterns of the bismuth oxyiodide / carbon nitride composite material and bismuth oxyiodide and carbon nitride obtained in Example 1;

[0025] Figure 3 The BET diagrams of the bismuth oxyiodide / carbon nitride composite material and bismuth oxyiodide and carbon nitride obtained in Example 1;

[0026] Figure 4 The self-powered electrochemical sensor obtained in Example 1 is 2+ The test results of the detection performance;

[0027] Figure 5 The self-powered electrochemical sensor obtained in Example 1 is 2+ Selective test results;

[0028] Figure 6The self-powered electrochemical sensor obtained in Example 1 is 2+ Test results of stability of OCPT response;

[0029] Figure 7 Self-powered electrochemical sensor for Cd 2+ Repeatability test results of the assay;

[0030] Figure 8 The test result of hydrogen peroxide production of BiOI / CN-34% obtained in Example 1;

[0031] Fig. 9 The self-powered electrochemical sensor obtained in Comparative Example 2 is 2+ The test results of the detection performance;

[0032] Fig.10 Schematic diagram of the process for preparing BiOI / CN-34% in Example 1;

[0033] Fig.11 These are the transient photocurrent test results of five electrode materials: BiOI, CN, BiOI / CN-11%, BiOI / CN-34%, and BiOI / CN-56%. DETAILED DESCRIPTION

[0034] The present invention provides a bismuth oxyiodide / carbon nitride composite material, comprising a bismuth oxyiodide matrix and carbon nitride supported on the surface of the bismuth oxyiodide matrix;

[0035] A pn heterojunction structure is formed between the bismuth oxyiodide matrix and the carbon nitride.

[0036] In the present invention, the mass of the carbon nitride is preferably 10 to 60% of the mass of the bismuth oxyiodide matrix, more preferably 11 to 56%, and even more preferably 34 to 35%.

[0037] The present invention also provides a method for preparing the bismuth oxyiodide / carbon nitride composite material described in the above technical solution, comprising the following steps:

[0038] Bismuth salt, iodine salt, ethylene glycol, polyvinyl pyrrolidone and carbon nitride are mixed and subjected to hydrothermal reaction to obtain the bismuth oxyiodide / carbon nitride composite material.

[0039] In the present invention, the bismuth salt preferably comprises bismuth nitrate; the bismuth nitrate is preferably Bi(NO 3 ) 3 ·5H 2O; the iodine salt preferably includes potassium iodide; the molar ratio of the bismuth salt to the iodine salt is preferably 1.0-1.1:1; the dosage ratio of the bismuth salt to ethylene glycol is preferably 1.0-1.1 mol:70-90 mL, and more preferably 1 mol:80 mL; the dosage ratio of the polyvinyl pyrrolidone to ethylene glycol is preferably 0.15-0.25 g:70-90 mL, and more preferably 0.2 g:80 mL.

[0040] In the present invention, the carbon nitride (gC 3 N 4 ) preferably comprises the following steps:

[0041] The urea is heated from room temperature to a first temperature at a first heating rate, and is heated from the first temperature to a second temperature at a second heating rate, and is kept warm, and is naturally cooled to room temperature to obtain the carbon nitride.

[0042] In the present invention, the first heating rate is preferably 5°C / min, the first temperature is preferably 250°C; the second heating rate is preferably 10°C / min, the second temperature is preferably 550°C, and the insulation time is preferably 2h. In the present invention, the carbon nitride is preferably a yellow porous material.

[0043] In the present invention, the mixing includes: dispersing bismuth salt and iodine salt in ethylene glycol, then adding polyvinyl pyrrolidone for stirring and dissolving to obtain a mixed solution; adding carbon nitride to the mixed solution for ultrasonic dispersion. In the present invention, the dispersion is preferably carried out under stirring, and the stirring time is preferably 10 minutes; the stirring and dissolving time is preferably 20 minutes; and the ultrasonic dispersion time is preferably 30 minutes.

[0044] In the present invention, the temperature of the hydrothermal reaction is preferably 140 to 180°C, more preferably 160°C; the time is preferably 12 to 16 hours. After the hydrothermal reaction, the present invention also preferably includes cooling the obtained system to room temperature, washing the obtained sample with anhydrous ethanol and distilled water after separation; and drying the washed sample in an oven at 60°C overnight.

[0045] The present invention also provides the use of the bismuth oxyiodide / carbon nitride composite material described in the above technical solution or the bismuth oxyiodide / carbon nitride composite material prepared by the preparation method described in the above technical solution as an electrode material in a self-powered electrochemical sensor.

[0046] The present invention also provides a self-powered electrochemical sensor, comprising a photoanode, a cathode and an electrolyte, wherein the electrode material on the photoanode is the bismuth oxyiodide / carbon nitride composite material described in the above technical scheme or the bismuth oxyiodide / carbon nitride composite material prepared by the preparation method described in the above technical scheme.

[0047] In the present invention, the photoanode preferably includes a substrate and an electrode material located on the surface of the substrate; the substrate is preferably ITO conductive glass; the electrode material is the bismuth iodide / carbon nitride composite material described in the above technical solution or the bismuth iodide / carbon nitride composite material prepared by the preparation method described in the above technical solution; the content of the electrode material on the photoanode is preferably 0.01 g / cm 2 ; The size of the photoanode is preferably 1*1.2cm.

[0048] In the present invention, the method for preparing the photoanode preferably comprises:

[0049] The electrode material, anhydrous ethanol and Nafion D520 solution are ultrasonically mixed to obtain a slurry;

[0050] The slurry is drop-coated on preheated ITO conductive glass and dried to obtain the photoanode.

[0051] In the present invention, the mass concentration of the Nafion D520 solution is preferably 4-6%, and more preferably 5%. In the present invention, the amount ratio of the electrode material, anhydrous ethanol and Nafion D520 solution is preferably 0.01g:260μL:40μL. In the present invention, the time of ultrasonic mixing is preferably 30min. In the present invention, the preheating temperature is preferably 70°C. The present invention has no special limitation on the process of drip coating, and it can be adopted by those skilled in the art. In the present invention, the drying time is preferably more than 10h.

[0052] In the present invention, the cathode preferably comprises carbon paper and a cathode material supported on the carbon paper, and the cathode material preferably comprises iron phthalocyanine. In the present invention, the content of the cathode material on the cathode is preferably 0.001 g / cm 2 In the present invention, the size of the cathode is preferably 1*1 cm.

[0053] In the present invention, the method for preparing the cathode preferably comprises:

[0054] The cathode material, anhydrous ethanol and Nafion D520 solution are ultrasonically mixed to obtain a slurry;

[0055] The slurry is coated on carbon paper and dried to obtain the cathode.

[0056] In the present invention, the mass concentration of the Nafion D520 solution is preferably 4-6%, and more preferably 5%. In the present invention, the amount ratio of the cathode material, anhydrous ethanol and Nafion D520 solution is preferably 0.001g:260μL:40μL. In the present invention, the time of the ultrasonic mixing is preferably 30min. The present invention has no special limitation on the coating process, and the process well known to those skilled in the art can be adopted. In the present invention, the drying time is preferably more than 10h.

[0057] In the present invention, the electrolyte is preferably a nitric acid solution. In the present invention, the concentration of the electrolyte is preferably 0.05 to 0.2 mol / L, and more preferably 0.1 mol / L.

[0058] The present invention has no special limitation on the construction method of the self-powered electrochemical sensor, and any method known to those skilled in the art may be adopted.

[0059] The present invention also provides the self-powered electrochemical sensor described in the above technical solution for detecting Cd 2+ Application in.

[0060] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0061] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0062] Example 1

[0063] Step 1: Carbon nitride CN was synthesized by a programmed temperature control method. Urea was heated from room temperature to 250°C at a heating rate of 5°C / min, and then further heated to 550°C at a rate of 10°C / min. Finally, it was kept at 550°C for 2 hours. After natural cooling, yellow porous CN was obtained.

[0064] Step 2: Prepare bismuth iodide / carbon nitride composite material by one-step hydrothermal method: 0.4851 g bismuth nitrate pentahydrate (Bi(NO 3 ) 3 ·5H 2O) and 0.166g potassium iodide (KI) were added to 80mL ethylene glycol and stirred continuously for 10min. 0.2g PVP was added to the solution and stirred rapidly for 20min until dissolved. Subsequently, 0.12g of the CN obtained above was dispersed in the above mixed solution and ultrasonicated for 30min. The obtained mixed system was transferred to a 100mL polytetrafluoroethylene container and hydrothermally reacted at 160°C for 12h. After cooling to room temperature, the samples were collected and washed several times with anhydrous ethanol and distilled water. Finally, the washed samples were placed in an oven at 60°C and dried overnight to obtain a composite material, recorded as BiOI / CN-34% (34% is the mass ratio of CN to BiOI). The process flow diagram is shown in the figure. Fig.10 shown.

[0065] Step 3: Prepare the photoanode: Cut the ITO electrode glass into a size of 1×1.2cm, weigh 0.01g of the above-obtained composite material and put it into a vial, add 260μL of anhydrous ethanol and 40μL of a 5% mass concentration of Nafion D520 solution, ultrasonicate for 30min, and wait for it to be completely dispersed to obtain a slurry. After heating the heating table to 70°C, place a clean ITO electrode glass on it, place the ITO electrode glass conductive surface upward, drop the slurry on the ITO electrode glass, and place it in a vacuum drying oven to dry for more than 10 hours to obtain a photoanode, in which the content of the electrode material on the anode is 0.01g / cm 2 .

[0066] Step 3: Prepare the cathode: Cut the carbon paper into 1×1 cm size, weigh 0.001 g of iron phthalocyanine (Fe II Pc) was placed in a vial, 260 μL of anhydrous ethanol and 40 μL of a 5% Nafion D520 solution were added, and ultrasonic treatment was performed for 30 min. After the dispersion was complete, the mixture was evenly coated on carbon paper, and then placed in a vacuum drying oven for more than 10 h to obtain a cathode, wherein the content of the electrode material on the cathode was 0.001 g / cm 2 .

[0067] Step 4: HNO 3 (0.1 M) was used as the electrolyte, and the photoanode and cathode obtained above were constructed into a self-powered electrochemical sensor.

[0068] Example 2

[0069] Bismuth oxyiodide / carbon nitride composite materials were prepared and self-powered electrochemical sensors were constructed in the manner of Example 1, except that the amount of CN added during the preparation of the bismuth oxyiodide / carbon nitride composite material was 0.04 g, and the obtained bismuth oxyiodide / carbon nitride composite material was recorded as BiOI / CN-11%.

[0070] Example 3

[0071] Bismuth oxyiodide / carbon nitride composite materials were prepared and self-powered electrochemical sensors were constructed in the manner of Example 1, except that the amount of CN added during the preparation of the bismuth oxyiodide / carbon nitride composite material was 0.2 g, and the obtained bismuth oxyiodide / carbon nitride composite material was recorded as BiOI / CN-56%.

[0072] Comparative Example 1

[0073] A self-powered electrochemical sensor was constructed in the manner of Example 1, except that the electrode material of the anode was CN.

[0074] Comparative Example 2

[0075] Bismuth iodide / carbon nitride composite materials were prepared and self-powered electrochemical sensors were constructed in the manner of Example 1, except that the electrolyte was a sulfuric acid solution with a concentration of 0.1 mol / L.

[0076] Performance Testing

[0077] Test Example 1

[0078] Figure 1 This is the SEM image of the bismuth iodide / carbon nitride composite material obtained in Example 1. Figure 1 It can be seen that BiOI appears as loose and regular nanospheres, and flocculent CN is dispersed on the surface and around the BiOI nanospheres. In addition, the EDS elemental analysis diagram clearly shows that Bi, O, I, C and N elements are evenly distributed on the BiOI / CN-34% heterojunction.

[0079] Test Example 2

[0080] Figure 2 The XRD patterns of the bismuth oxyiodide / carbon nitride composite material and bismuth oxyiodide and carbon nitride obtained in Example 1 are as follows; Figure 2 It can be seen that the XRD spectrum of CN shows two diffraction peaks at 12.9° and 27.2°, which are respectively attributed to the in-plane stacking of 3-s triazine rings of the (100) crystal plane of graphite carbon CN and the interlayer stacking of conjugated aromatic groups of the (002) crystal plane. The diffraction peaks at 29.2°, 31.8°, 45.7° and 54.5° correspond to the (102), (110), (200), and (212) crystal planes of tetragonal BiOI (JCPDS No.10-0445), respectively. The diffraction peaks of BiOI can also be observed in BiOI / CN-34%. The results show that the synthesis of CN and BiOI monomers is successful.

[0081] Test Example 3

[0082] Figure 3The BET diagram of the bismuth oxyiodide / carbon nitride composite material and bismuth oxyiodide and carbon nitride obtained in Example 1, wherein Figure 3 (a) is the adsorption isotherm, Figure 3 (b) is a pore size distribution diagram; the specific test results are shown in Table 1;

[0083] Table 1 Specific surface area and pore size of the bismuth iodide / carbon nitride composite material obtained in Example

[0084] <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Total pore volume (cm 3 / g)]]> Average pore size (nm) BiI 15.66 0.05 13.5 CN 57.66 0.22 15.6 BiOI / CN - 34% 68.62 0.14 8.2

[0085] like Figure 3 As shown in (a), the adsorption isotherm of pure BiOI is 4 The hysteresis loop of type IV curve indicates that its mesoporous structure may be mainly caused by narrow cracks. This is consistent with the results observed in the SEM image. The isotherm adsorption line of CN is 3 The isothermal adsorption line of BiOI / CN-34% is a type IV curve. It is worth noting that at a relative pressure of 0.4 to 0.8 (P / P 0 ) has H 4 The characteristics of the hysteresis loop have H in the relative pressure range of 0.8 to 1.0. 3 The characteristics of the hysteresis loop indicate that its mesoporous structure is caused by the stacking of BiOI nanosheets and CN particles, which is consistent with the results observed in the SEM image. The average pore size of BiOI is concentrated around 7-10nm, and the average pore size of CN is mainly distributed between 20 and 200nm, indicating that the loose flocculent structure of CN forms mesopores and macropores of different sizes. The average pore size of BiOI / CN-34% is mainly distributed between 3-4nm and 20-200nm. It has both the mesoporous structure of BiOI and the macroporous structure of CN. The combination of the two may be the reason why it has a large specific surface area (68.62m 2 / g) is one of the reasons.

[0086] Test Example 4

[0087] The self-powered electrochemical sensors obtained in Example 1 and Comparative Example 2 were irradiated with a xenon lamp light source (Zhongjiao Jinyuan CLE-S500) at room temperature, and different concentrations of Cd 2+ Study on the self-powered electrochemical sensor for Cd 2+ detection performance.

[0088] Figure 4 The self-powered electrochemical sensor of Example 1 is 2+ The test results of the detection performance of Figure 4 (a) shows the OCPT change of the self-powered electrochemical sensor and Cd 2+ The concentration relationship diagram, Figure 4 (b) is OCPT and Cd 2+ Linear relationship graph between logarithms of concentrations;

[0089] Figure 4 (a) shows that the OCPT of the sensor increases with the Cd 2+ The concentration of Cd increases, and OCPT increases with lg c (c is Cd 2+ The concentrations showed a linear relationship (Figure b). The linear equation was OCPT = 0.02317lg c + 0.07 (R 2 =0.9881, c is Cd 2+ The detection limit was calculated to be 0.033 μM by the signal-to-noise ratio method (S / N=3).

[0090] Fig. 9 The OCPT change of the self-powered electrochemical sensor obtained in Comparative Example 2 and the Cd 2+ The concentration relationship diagram shows that when using H 2 SO 4 When used as an electrolyte, there is no linear relationship between OCPT and concentration. Therefore, H 2 SO 4 Make electrolyte.

[0091] Test Example 5

[0092] Figure 5 The self-powered electrochemical sensor obtained in Example 1 is 2+ The selective test results, the test conditions refer to Test Example 4;

[0093] In order to verify the self-powered electrochemical sensor for Cd 2+ The selectivity of the self-powered electrochemical sensor obtained in Example 1 was tested for 0.05 μM Cd 2+ With 0.3 μM other heavy metal ions (including Fe 2+ , Fe 3+ , Cu 2+ 、Zn 2+ , Pb 2+ 、Ni 2+ )'s OCPT. Figure 5 The results showed that the self-powered electrochemical sensor could detect Cd 2+ The OCPT response of the self-powered electrochemical sensor is still the most obvious. 2+ Good selectivity.

[0094] Test Example 6

[0095] Figure 6The self-powered electrochemical sensor obtained in Example 1 is 2+ The test results of the stability of the OCPT response, the test conditions refer to Test Example 4;

[0096] In order to evaluate the stability of the self-powered electrochemical sensor under long-term light irradiation, 0.05 μM Cd 2+ The OCPT was tested. Figure 6 The results showed that the OCPT response remained basically unchanged, indicating that the self-powered electrochemical sensor was sensitive to Cd 2+ The detection has excellent stability.

[0097] Test Example 7

[0098] Figure 7 Self-powered electrochemical sensor for Cd 2+ Repeatability test results of the test. For test conditions, see Test Example 4.

[0099] In order to evaluate the self-powered electrochemical sensor for Cd 2+ To improve the reproducibility of the detection, different batches of BiOI / CN-34% modified electrodes were tested. Figure 7 As shown in the figure, the relative standard deviation of the results of 5 repeated experiments was 0.458%, indicating that the self-powered electrochemical sensor constructed by different batches of BiOI / CN-34% modified electrodes was effective for Cd 2+ The detection has good repeatability.

[0100] Test Case 8

[0101] Figure 8 The test result of hydrogen peroxide production of BiOI / CN-34% obtained in Example 1;

[0102] The test method is as follows: weigh 0.01g BiOI / CN-34%, add 50mL distilled water, and then place it in an ultrasonic device for 30 minutes. After it is completely dispersed, it is irradiated. After irradiation for 30, 60, and 90 minutes, take 4mL of the suspension and centrifuge it for 10 minutes. After the centrifugation, take 2mL of the supernatant and mix it with 1mL H 2 O 2 The indicator was mixed and placed in a UV-visible spectrophotometer. The measurement was performed every 10 minutes, and each group was measured three times in total. The value at a wavelength of 437 nm was read, and H 2 O 2 concentration.

[0103] from Figure 8 It can be seen that BiOI / CN-34% can produce H 2 O 2 , and the output H 2O 2 The concentration of Cd increases with time, proving that the sensor has the ability to self-power and can meet the requirements of detecting Cd 2+ needs.

[0104] Test Example 9

[0105] Fig.11 These are the transient photocurrent test results of five electrode materials: BiOI, CN, BiOI / CN-11%, BiOI / CN-34%, and BiOI / CN-56%.

[0106] The transient photocurrent test uses a three-electrode system, where a saturated calomel electrode (SCE) is the reference electrode and a platinum sheet is the counter electrode. After testing, the OCPT of all samples is around +0.3V vs. SCE, so the photocurrent test is carried out under +0.3V vs. SCE conditions. Fig.11 It can be seen that the order of photocurrent intensity from high to low is BiOI / CN-34%>BiOI / CN-56%>BiOI / CN-11%>BiOI>CN. The specific test results are shown in Table 2.

[0107] Table 2 Transient photocurrent test results

[0108]

[0109] The higher the photocurrent intensity, the higher the - and h + This result shows that the construction of BiOI / CN-Xp-n ​​heterojunction improves the separation efficiency of photogenerated - and h + The separation efficiency can be improved, thereby enhancing the photocatalytic activity.

[0110] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A bismuth oxyiodide / carbon nitride composite material, characterized in that: It comprises a bismuth iodide oxide substrate and carbon nitride supported on the surface of the bismuth iodide oxide substrate; A pn heterojunction structure is formed between the bismuth oxyiodide matrix and the carbon nitride.

2. The bismuth oxyiodide / carbon nitride composite material according to claim 1, characterized in that: The mass of the carbon nitride is 10-60% of the mass of the bismuth oxyiodide matrix.

3. The method for preparing the bismuth oxyiodide / carbon nitride composite material according to claim 1 or 2, characterized in that: The following steps are involved: Bismuth salt, iodine salt, ethylene glycol, polyvinyl pyrrolidone and carbon nitride are mixed and subjected to hydrothermal reaction to obtain the bismuth oxyiodide / carbon nitride composite material.

4. The preparation method according to claim 3, characterized in that: The bismuth salt includes bismuth nitrate; the iodine salt includes potassium iodide; the molar ratio of the bismuth salt to the iodine salt is 1.0-1.1:1; The dosage ratio of the bismuth salt to ethylene glycol is 1.0-1.1 mol: 70-90 mL; The usage ratio of polyvinyl pyrrolidone to ethylene glycol is 0.15-0.25 g:70-90 mL.

5. The preparation method according to claim 3, characterized in that: The mixing includes: The bismuth salt and the iodine salt are dispersed in ethylene glycol, and then polyvinyl pyrrolidone is added to stir and dissolve to obtain a mixed solution; the carbon nitride is added to the mixed solution to perform ultrasonic dispersion.

6. The preparation method according to claim 3, characterized in that: The temperature of the hydrothermal reaction is 140-180° C. and the time is 12-16 hours.

7. Use of the bismuth oxyiodide / carbon nitride composite material according to claim 1 or 2 or the bismuth oxyiodide / carbon nitride composite material prepared by the preparation method according to any one of claims 3 to 6 as an electrode material in a self-powered electrochemical sensor.

8. A self-powered electrochemical sensor comprising a photoanode, a cathode and an electrolyte, characterized in that: The electrode material on the photoanode is the bismuth oxyiodide / carbon nitride composite material according to claim 1 or 2 or the bismuth oxyiodide / carbon nitride composite material prepared by the preparation method according to any one of claims 3 to 6.

9. The self-powered electrochemical sensor according to claim 8, characterized in that: The cathode comprises carbon paper and a cathode material loaded on the carbon paper; the cathode material comprises iron phthalocyanine; and the electrolyte is a nitric acid solution.

10. The self-powered electrochemical sensor according to claim 8 or 9 is used to detect Cd 2+ Application in.

Citation Information

Cited By

  • Broadband spectral response type BiVO4-based photocatalytic electrode as well as preparation method and application thereof

    CN119715714A

  • A broad-spectrum response type BiVO4-based photocatalytic electrode and a preparation method and application thereof

    CN119715714B