Method for detecting sodium precipitation potential and sodium intercalation potential of sodium ion battery

Through the polarization and open circuit operation of sodium ion batteries, the voltage-time curve is detected, which solves the problem of difficult to judge the sodium analysis phenomenon in the existing technology, and realizes rapid and accurate detection of sodium ion batteries, improving the electrochemistry and Safety performance.

CN119087253APending Publication Date: 2024-12-06SHENZHEN BAK POWER BATTERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411194048.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing technology lacks efficient non-destructive testing methods to determine whether sodium ion batteries have sodium extraction, which has affected the battery circulation and safety performance, especially in large batteries.

Method used

By assembling the negative electrode sheet of the sodium ion battery with the sodium sheet, polarization and open circuit operation are performed, voltage-time relationship curves are obtained, and sodium embedding potential and sodium elimination potential are determined respectively. The polarization potential and polarization time are adjusted to achieve sodium Fast and accurate detection of ion batteries.

Benefits of technology

This method realizes rapid and accurate detection of sodium potential and sodium potential of sodium anode material without damaging the battery, helping the battery management system (BMS) to regulate the voltage range during the battery operation and improve electrochemical performance and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087253A_ABST
    Figure CN119087253A_ABST
Patent Text Reader

Abstract

The invention provides a sodium ion battery sodium precipitation potential and sodium intercalation potential detection method, and relates to the technical field of batteries. The detection method comprises the following steps: assembling a negative plate and a sodium plate to obtain a battery, and connecting the battery with a positive electrode and a negative electrode of an electrochemical workstation; polarization is carried out according to the set polarization potential and polarization time, then open circuit is carried out according to the set open circuit time, a relation curve of time and voltage is obtained, and a first equilibrium potential is obtained; when the first equilibrium potential is greater than 0, the first equilibrium potential is a sodium embedding potential; the polarization potential and the polarization time are adjusted, a second equilibrium potential is obtained, polarization and open circuit are repeatedly conducted till the second equilibrium potential is smaller than 0, and the second equilibrium potential is the sodium precipitation potential. According to the detection method, rapid and accurate detection of the sodium precipitation potential and the sodium intercalation potential of the sodium battery negative electrode material is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery. Background Art

[0002] Modern industry that uses carbon as an energy carrier has brought huge challenges to the sustainable development of human society. The development of low-carbon and efficient material preparation and resource utilization technologies is an inevitable choice to meet this challenge. Electrochemical energy storage represented by the excellent physical and chemical properties of lithium-ion batteries is highly favored because of its flexibility, convenience, easy maintenance, high energy storage and conversion efficiency. However, with the increase in demand for energy storage batteries, the uneven geographical distribution of lithium resources, the rising costs, and the price fluctuations of lithium carbonate, the use of low-cost sodium-ion batteries as an alternative is the best choice at present. Since sodium and lithium have similar electrochemical properties, sodium-ion batteries also have high energy density and extremely long cycle life.

[0003] However, due to the loss of active substances in the hard carbon negative electrode and fatigue damage to the crystal structure of the material during the cycle, polarization will become more and more significant. At this time, on the surface of the negative electrode, sodium ions are easily affected by the nucleation overpotential and the unfavorable kinetic environment to obtain electrons and thus deposit on the surface and pores of the hard carbon, which is the phenomenon of sodium precipitation. Sodium precipitation will not only lead to the loss of active sodium ions and cause capacity decay, but also promote the deterioration of gas production, heat release, and side reactions in severe cases. Then it will cause safety problems such as internal short circuit and thermal runaway. At present, the scientific community lacks theoretical research on the mechanism of sodium precipitation, and the industry is also deeply troubled by it, especially in large batteries.

[0004] The redox potential of sodium precipitation / sodium insertion reaction is particularly important for the selection of battery charge and discharge cut-off voltage and the management of BMS. If the negative electrode of the sodium ion battery does not touch the sodium precipitation potential by regulating the voltage, current, temperature and other parameters during the battery operation, it will have a positive guiding effect on the battery's cycle performance and safety performance. However, in battery testing, it is often difficult to judge whether sodium precipitation has occurred and the exact value of the sodium precipitation potential by the change of cycle data. Generally, it is necessary to disassemble the failed battery and observe it with the naked eye, or to perform physical and chemical characterization of the electrode to achieve it. In non-destructive analysis, conventional testing methods such as sodium insertion overcharge and discharge, three-electrode cyclic voltammetry, and differential capacitance require a lot of time and human resources. Electrochemical AC impedance can solve the above problems to a certain extent, but the reduction of the Nyquist semicircle corresponding to the charge transfer impedance may be caused by reasons other than sodium (lithium) precipitation (such as internal short circuit), which increases the uncertainty of the experiment.

[0005] Therefore, there is still a lack of efficient non-destructive testing technology for long-cycle sodium precipitation. Summary of the invention

[0006] The purpose of the present application is to provide a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery to solve the above problems.

[0007] To achieve the above objectives, the present application provides a method for detecting the sodium deposition potential and sodium insertion potential of a sodium ion battery, comprising:

[0008] Assembling the negative electrode sheet and the sodium sheet to obtain a battery, and connecting the battery to the positive and negative electrodes of an electrochemical workstation;

[0009] Polarize according to the set polarization potential and polarization time, then open the circuit according to the set open circuit time, obtain the relationship curve between time and voltage, and obtain the first equilibrium potential;

[0010] When the first equilibrium potential is greater than 0, the first equilibrium potential is a sodium insertion potential;

[0011] The polarization potential and the polarization time are adjusted to obtain a second equilibrium potential, and the polarization and the open circuit are repeated until the second equilibrium potential is less than 0, and the second equilibrium potential is a sodium precipitation potential.

[0012] Optionally, the polarization potential is -1V to -0.2V.

[0013] Optionally, the polarization potential set when obtaining the sodium insertion potential is greater than -0.5V and less than or equal to -0.2V.

[0014] Optionally, the polarization potential set when obtaining the sodium precipitation potential is greater than or equal to -0.5V and less than or equal to -1V.

[0015] Optionally, the polarization time is 10s-60s.

[0016] Optionally, the battery comprises a button cell.

[0017] Optionally, the open circuit time is greater than or equal to 120s.

[0018] Optionally, the method further includes: setting a plurality of groups of the polarization potentials and the polarization times to obtain a plurality of the relationship curves, and verifying whether the voltage platforms of the equilibrium potentials are consistent.

[0019] Optionally, when the voltage platforms of the multiple groups of equilibrium potentials are greater than 0 and consistent, the equilibrium potential is a sodium embedding potential;

[0020] When the voltage platforms of the plurality of groups of equilibrium potentials are less than 0 and are consistent, the equilibrium potential is the sodium precipitation potential.

[0021] Optionally, the negative electrode sheet comprises hard carbon.

[0022] Compared with the prior art, the beneficial effects of this application include:

[0023] The present application provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery. After a proper amount of sodium metal is deposited on the surface of the negative electrode by polarization, the circuit is disconnected. At this time, the sodium ions on the surface of the negative electrode diffuse into the interior of the negative electrode at a certain rate. The process is a two-phase equilibrium state. Then, open circuit potential-time data acquisition is performed, and the sodium insertion and precipitation potentials of the negative electrode are obtained through two different platforms that are normalized respectively. The detection method realizes rapid and accurate detection of the sodium precipitation potential and the sodium insertion potential of the sodium battery negative electrode material without causing damage to the battery. The data is beneficial for the BMS to regulate the voltage range (upper limit) during the operation of the battery, so that the battery has better electrochemical performance and safety performance during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0025] Figure 1 A flow chart of the steps of a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery provided in an embodiment;

[0026] Figure 2 This is the data curve test diagram of Example 1;

[0027] Figure 3 This is the data curve test diagram of comparative example 1;

[0028] Figure 4 This is the cyclic voltammetry test diagram of Control Example 1. DETAILED DESCRIPTION

[0029] As used herein:

[0030] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0031] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0032] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0033] In these examples, parts and percentages are by mass unless otherwise indicated.

[0034] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0035] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0036] The present application provides a method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery, comprising:

[0037] Assembling the negative electrode sheet and the sodium sheet to obtain a battery, and connecting the battery to the positive and negative electrodes of an electrochemical workstation;

[0038] Polarization is performed according to the set polarization potential and polarization time, and then static and open circuit potential are collected according to the set open circuit time to obtain a relationship curve between time and voltage, and obtain a first equilibrium potential;

[0039] It should be noted that when a certain amount of sodium metal is deposited on the surface of the negative electrode, if the circuit is disconnected at this time, the sodium ions will diffuse into the interior of the negative electrode during the open circuit and static process. This process presents an obvious platform on the voltage-current curve. The voltage value corresponding to the platform is the equilibrium potential value of sodium precipitation (less affected by the kinetic environment, the current is 0 in the open circuit state, and the reaction proceeds at a nearly reversible speed). Therefore, a certain polarization time (sodium ion deposition time) is necessary in order to deposit an appropriate amount of metallic sodium to highlight the voltage platform, that is, the corresponding equilibrium potential.

[0040] When the first equilibrium potential is less than 0, the first equilibrium potential is a sodium precipitation potential;

[0041] The polarization potential and the polarization time are adjusted to obtain a second equilibrium potential, and the polarization and the open circuit are repeated until the second equilibrium potential is greater than 0, and the second equilibrium potential is a sodium insertion potential.

[0042] It should be noted that, in theory, when sodium is precipitated at the negative electrode, the redox potential of Na / Na+ is 0V (vs.Na / Na+), but due to the actual kinetic environment such as the surface morphology (pores, particle size, etc.) of the hard carbon negative electrode and the applied current density, the reduction potential (sodium precipitation potential) should be less than 0V, that is, there is an overpotential, and the sodium insertion potential (oxidation potential) is greater than 0. Therefore, after repeated electrochemical experiments, the normalized sodium precipitation curve platform and the normalized sodium insertion curve should be clearly distinguished above and below 0V.

[0043] In some embodiments, the polarization potential is -1V to -0.5V.

[0044] Optionally, the polarization potential may be -1V, -0.9V, -0.8V, -0.7V, -0.6V, -0.5V, or any value between -1V and -0.5V.

[0045] It should be noted that when the polarization potential is -1V to -0.5V, a certain amount of metallic sodium can be deposited without damaging the electrode material (the potential is too negative). When the circuit is open, it takes a certain process for sodium ions to enter the hard carbon. During this period, there is a two-phase equilibrium on the negative electrode surface. The open circuit voltage curve can show an obvious platform area, which is convenient for judging the sodium precipitation potential.

[0046] In some embodiments, the polarization potential set when obtaining the sodium insertion potential is greater than -0.5V and less than or equal to -0.2V.

[0047] Optionally, the polarization potential set when obtaining the sodium insertion potential may be -0.4V, -0.3V, -0.2V, or any value between greater than -0.5V and less than or equal to -0.2V.

[0048] It should be noted that if the selected polarization potential is too low (negative), it may lead to excessive sodium precipitation, and the displayed voltage curve platform is the sodium precipitation platform. It takes a long time for the curve to enter the sodium embedding platform, and the polarization potential is too low, which may cause irreversible damage to the electrode material and affect subsequent tests; if the polarization potential is too high, the sodium ions may not enter the pores of the hard carbon by the pore-filling mechanism (adsorption / intercalation mechanism, voltage>0.1V), and the sodium ions are not the sodium ions deposited on the surface of the negative electrode, but come from the sodium ions in the counter electrode. Therefore, the polarization potential needs to be slightly lower, but not higher than -0.2V, and not lower than -0.5V to trigger the sodium precipitation platform, and only a very small amount of deposited sodium metal is used to diffuse into the pores of the hard carbon through it to determine the voltage value of the lowest sodium embedding platform.

[0049] In some embodiments, the polarization potential set when obtaining the sodium precipitation potential is greater than or equal to -0.5V and less than or equal to -1V.

[0050] Optionally, the polarization potential set when obtaining the sodium precipitation potential can be -0.5V, -0.6V, -0.7V, -0.8V, -0.9V, -1V, or any value between greater than or equal to -0.5V and less than or equal to -1V.

[0051] It should be noted that when the sodium precipitation potential is uncertain, appropriately increasing the polarization potential will help the deposition of sodium ions.

[0052] In some embodiments, the polarization time is 10s-60s.

[0053] Optionally, the polarization time can be 10s, 15s, 20s, 25s, 30s, 35s, 40s, 45s, 50s, 55s, 60s or any value between 10s and 60s.

[0054] It should be noted that this duration is used in conjunction with the polarization voltage to allow the battery to deposit an appropriate amount of metallic sodium before being left in an open circuit. The duration range is the optimal time obtained after experimental exploration (adapting to the polarization potential mentioned above). It can be appropriately increased or decreased within this range, but exceeding this range may have adverse effects, such as time cost (too long) or inability to effectively deposit an appropriate amount of metallic sodium (too short).

[0055] In some embodiments, the battery comprises a button cell.

[0056] It should be noted that the battery can be a button battery, or a cylindrical, square or polymer battery, and the type of battery is not limited.

[0057] In some embodiments, the open circuit time is greater than or equal to 120 seconds.

[0058] It should be noted that when the open circuit time is greater than or equal to 120s, a certain length of open circuit time and data collection is necessary. Considering the time cost, an open circuit time slightly greater than 120s is sufficient to stabilize the reaction and make the curve platform clear. A longer open circuit time can also be performed, depending on the specific situation.

[0059] In some embodiments, the method further includes: setting a plurality of groups of the polarization potentials and the polarization times to obtain a plurality of the relationship curves, and verifying whether the voltage platforms of the equilibrium potentials are consistent.

[0060] It should be noted that under different polarization times, the potential platform of sodium precipitation will not be affected, but only the time of the reaction will be affected. The more sodium deposited on the negative electrode surface, the closer the activity of sodium is to 1, and the more stable the platform is. Multiple experiments can eliminate the experimental errors caused by chance. At the same time, the normalized voltage curve platforms under similar kinetic environments can verify each other.

[0061] In some embodiments, when the voltage platforms of the plurality of sets of equilibrium potentials are greater than 0 and consistent, the equilibrium potential is a sodium embedding potential;

[0062] When the voltage platforms of the plurality of groups of equilibrium potentials are less than 0 and are consistent, the equilibrium potential is the sodium precipitation potential.

[0063] In some embodiments, the negative electrode sheet includes hard carbon.

[0064] It should be noted that hard carbon contains more micropores and mesopores for sodium ions to embed, but whether other types of negative electrodes can achieve the above effect remains to be studied.

[0065] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0066] Example 1

[0067] This embodiment provides a method for detecting sodium deposition potential and sodium insertion potential of a sodium ion battery, comprising:

[0068] S1: Take the rolled hard carbon negative electrode, active material mass: 7.5634 mg, nominal specific capacity: 350 g / mAh, surface density: 8.631 cm 2 , compacted density: 0.97g / cm 3 , after cutting, assembled with sodium sheet into LIR2430 button half-cell;

[0069] S2: On the CORRTEST electrochemical workstation, connect the positive and negative electrodes of the battery with a snap-on clamp;

[0070] S3: Set the script for customized testing: 1. Polarization potential is -1V, polarization time is 30s; 2. Open circuit potential, test time is 86400s;

[0071] S4: Start the program;

[0072] S5: 100s to terminate the program and obtain data curve 1;

[0073] S6: Two different polarization times of 20s and 40s were used respectively;

[0074] S7: Test again and output data curve 2-3;

[0075] S8: Use a polarization potential of -0.2 V and polarization times of 20 s, 30 s, and 40 s, and test again;

[0076] S9: Obtain the corresponding data curve 4-6.

[0077] The steps of the above-mentioned method for detecting the sodium precipitation potential and the sodium insertion potential of the sodium ion battery are as follows: Figure 1 shown.

[0078] The above obtained data curves are sorted as follows: Figure 2 shown.

[0079] The sodium embedding potential is generally above 0V, so it is preliminarily judged that the platform of curve 1 is the sodium precipitation platform. At this time, the test takes 2 minutes and 10 seconds. Curves 1-3 have the same sodium precipitation platform ①, which is an oxidation reaction: Na=Na + +e - The equilibrium potential, that is, the sodium precipitation potential is -0.018V; Curves 4-6 have the same platform ②, which is the sodium insertion platform, and the reaction is: nC+xNa + +xe - =Na x C n , the sodium embedding potential is 0.010V, there is a clear distinction between platform ② and platform ①, the test takes about 15 minutes, so far the sodium precipitation potential and sodium embedding potential have been confirmed, the result is stable and reproducible.

[0080] Example 2

[0081] This embodiment provides a method for detecting sodium deposition potential and sodium insertion potential of a sodium ion battery, comprising:

[0082] S1: Take the rolled hard carbon negative electrode, which is the same as the hard carbon negative electrode in Example 1, cut it and assemble it with the sodium sheet into a LIR2430 button half-cell;

[0083] S2: On the CORRTEST electrochemical workstation, connect the positive and negative electrodes of the battery with a snap-on clamp;

[0084] S3: Set the script for customized testing: 1. Polarization potential is -1V, polarization time is 40s; 2. Open circuit potential, test time is 86400s;

[0085] S4: Start the program;

[0086] S5: 100s to terminate the program and obtain data curve 1;

[0087] S6: Two different polarization times of 20s and 50s were used respectively;

[0088] S7: Test again and output data curve 2-3;

[0089] S8: Use a polarization potential of -0.2 V and polarization times of 20 s, 30 s, and 40 s, and test again;

[0090] S9: Obtain the corresponding data curve 4-6.

[0091] Curves 1-3 have the same sodium precipitation platform ①, and the sodium precipitation potential of the sodium precipitation platform ① is -0.02V; curves 4-6 have the same sodium insertion platform ②, and the sodium insertion potential of the sodium insertion platform ② is 0.012V. There is a clear distinction between platform ② and platform ①. The test takes about 17 minutes. At this point, the sodium precipitation potential and the sodium insertion potential have been confirmed. The result is stable and reproducible.

[0092] Example 3

[0093] This embodiment provides a method for detecting sodium deposition potential and sodium insertion potential of a sodium ion battery, comprising:

[0094] S1: Take the rolled hard carbon negative electrode, which is the same as the hard carbon negative electrode in Example 1, cut it and assemble it with the sodium sheet into a LIR2430 button half-cell;

[0095] S2: On the CORRTEST electrochemical workstation, connect the positive and negative electrodes of the battery with a snap-on clamp;

[0096] S3: Set the script for customized testing: 1. Polarization potential is -1V, polarization time is 20s; 2. Open circuit potential, test time is 86400s;

[0097] S4: Start the program;

[0098] S5: 100s to terminate the program and obtain data curve 1;

[0099] S6: Two different polarization times of 30s and 50s were used respectively;

[0100] S7: Test again and output data curve 2-3;

[0101] S8: Use a polarization potential of -0.2 V and polarization times of 20 s, 30 s, and 40 s, and test again;

[0102] S9: Obtain the corresponding data curve 4-6.

[0103] Curves 1-3 have the same sodium precipitation platform ①, and the sodium precipitation potential of the sodium precipitation platform ① is -0.017V; curves 4-6 have the same sodium insertion platform ②, and the sodium insertion potential of the sodium insertion platform ② is 0.011V. There is a clear distinction between platform ② and platform ①. The test takes about 17 minutes. At this point, the sodium precipitation potential and the sodium insertion potential have been confirmed. The result is stable and reproducible.

[0104] Example 4

[0105] This embodiment provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery, which is different from Embodiment 1 in that the polarization potential in S3 is -0.9V, and the polarization potential in S7 is -0.4V.

[0106] Example 5

[0107] This embodiment provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery, which is different from Embodiment 1 in that the polarization potential in S3 is -0.8V, and the polarization potential in S7 is -0.3V.

[0108] Example 6

[0109] This embodiment provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery, which is different from Embodiment 1 in that the polarization potential in S3 is -0.9V, and the polarization potential in S7 is -0.3V.

[0110] Example 7

[0111] This embodiment provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery, which is different from Embodiment 1 in that the polarization times corresponding to the two different polarization potentials are 40s, 50s, and 60s, respectively.

[0112] Example 8

[0113] This embodiment provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery, which is different from Embodiment 1 in that the polarization times corresponding to the two different polarization potentials are 20s, 40s, and 60s, respectively.

[0114] The sodium precipitation potential test results of Examples 4-8 are all -0.018V, the sodium insertion potential is all 0.01V, and the total test time is all between 18-20 minutes. The results are stable and reproducible.

[0115] Comparative Example 1

[0116] This comparative example provides a method for detecting the sodium precipitation potential and sodium insertion potential of a sodium ion battery, comprising:

[0117] S1: Take the rolled hard carbon negative electrode, which is the same as the hard carbon negative electrode in Example 1, cut it and assemble it with the sodium sheet into a LIR2430 button half-cell;

[0118] S2: On the CORRTEST electrochemical workstation, connect the positive and negative electrodes of the battery with a snap-on clamp;

[0119] S3: Set the script for customized testing: 1. Polarization potential is -0.1V, polarization time is 60s; 2. Open circuit potential, test time is 86400s;

[0120] S4: Start the program;

[0121] S5: 100s to terminate the program and obtain data curve 1;

[0122] S6: Change the polarization potential to -0.8 V and the polarization time to 5 s;

[0123] S7: Test again and output data curve 2;

[0124] S8: Change the polarization potential to -0.7 V, and the polarization time to 20 s and 40 s respectively;

[0125] S9: Test again and output data curve 3-4;

[0126] S10: change the polarization potential to -0.3 V, and the polarization time to 40 s, 50 s, and 60 s respectively;

[0127] S11: Test again and output data curves 5-7;

[0128] S12: Analyze the sodium evolution potential of the hard carbon negative electrode using cyclic voltammetry.

[0129] The data curves 1-7 obtained above are sorted as follows: Figure 3 shown.

[0130] The cyclic voltammetry test results are as follows Figure 4 shown.

[0131] Due to improper setting of polarization potential in S3, the activity of precipitated metallic sodium is insufficient to reach the detection limit of the method. At this time, the platform of data curve 1 is slightly greater than 0V, which is easily confused with the subsequent sodium embedding platform. Therefore, the polarization potential is adjusted to -0.8V in S6 to obtain the corresponding data curve 2. Although the polarization potential value is set within an appropriate range, the improper setting of polarization time causes the platform to tilt relatively seriously during the test. This phenomenon is caused by the fact that the potential is proportional to the sodium content in the pores of the material due to the small amount of sodium deposition, resulting in a mixture of sodium embedding and sodium precipitation. Therefore, the polarization time is adjusted to 30s on the basis of keeping the polarization potential unchanged.

[0132] In the cyclic voltammetry test (CV test) results, the sodium precipitation potential was -0.03V, which was basically consistent with the results of the open circuit chronopotentiometry (OCP). The potential was slightly negative than the latter because the existence of the polarization potential made the peak position more negative; the CV test took a total of 72.2 hours, which further verified the high timeliness and accuracy of the open circuit chronopotentiometry in confirming the sodium precipitation potential.

[0133] The results of the sodium precipitation equilibrium potential and sodium insertion equilibrium potential of the above-mentioned embodiments and comparative examples are shown in Table 1.

[0134] Table 1 Sodium precipitation equilibrium potential and sodium insertion equilibrium potential

[0135] sample Sodium equilibrium potential / V Sodium insertion equilibrium potential / V Example 1 -0.018 0.010 Example 2 -0.020 0.012 Example 3 -0.017 0.011 Example 4 -0.016 0.087 Example 5 -0.021 0.092 Example 6 -0.018 0.011 Example 7 -0.017 0.094 Example 8 -0.019 0.010 Comparative Example 1 -0.017 0.011

[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0137] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery, characterized in that: include: Assembling the negative electrode sheet and the sodium sheet to obtain a battery, and connecting the battery to the positive and negative electrodes of an electrochemical workstation; Polarize according to the set polarization potential and polarization time, then open the circuit according to the set open circuit time, obtain the relationship curve between time and voltage, and obtain the first equilibrium potential; When the first equilibrium potential is greater than 0, the first equilibrium potential is a sodium insertion potential; The polarization potential and the polarization time are adjusted to obtain a second equilibrium potential, and the polarization and the open circuit are repeated until the second equilibrium potential is less than 0, and the second equilibrium potential is a sodium precipitation potential.

2. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 1, characterized in that: The polarization potential is -1V to -0.2V.

3. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 2, characterized in that: The polarization potential set when obtaining the sodium insertion potential is greater than -0.5V and less than or equal to -0.2V.

4. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 2, characterized in that: The polarization potential set when obtaining the sodium precipitation potential is greater than or equal to -0.5V and less than or equal to -1V.

5. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 1, characterized in that: The polarization time is 10s-60s.

6. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 1, characterized in that: The battery comprises a button cell.

7. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 1, characterized in that: The open circuit time is greater than or equal to 120s.

8. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 1, characterized in that: Also includes: A plurality of groups of the polarization potentials and the polarization times are set to obtain a plurality of the relationship curves, and to verify whether the voltage platforms of the equilibrium potentials are consistent.

9. The method for detecting sodium precipitation potential and sodium insertion potential of a sodium ion battery according to claim 8, characterized in that: When the voltage platforms of the multiple groups of equilibrium potentials are greater than 0 and consistent, the equilibrium potential is a sodium embedding potential; When the voltage platforms of the plurality of groups of equilibrium potentials are less than 0 and are consistent, the equilibrium potential is the sodium precipitation potential.

10. The method for detecting sodium deposition potential and sodium insertion potential of a sodium ion battery according to any one of claims 1 to 9, characterized in that: The negative electrode sheet includes hard carbon.