Sandwich-type polarization-maintaining gain fiber with composite structure and preparation method of sandwich-type polarization-maintaining gain fiber

By designing a sandwich-type bias-maintaining gain fiber with structural composite, using the combination of rare earth-doped glass materials and passive glass, the problem of complex processing of stress fibers and difficult to control geometric fiber parameters is solved, and efficient and stable fiber preparation is achieved and excellent birefringence properties.

CN119087574AInactive Publication Date: 2024-12-06SOUTH CHINA UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411572113.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing stress-type polarization-maintaining fibers have complex processing, low yield, and are susceptible to temperature disturbances; the structural parameters of geometric polarization-maintaining fibers are difficult to accurately control, and it is difficult to draw.

Method used

Design a composite structure sandwich-type bias-retaining gain fiber, adopting a sandwich-type core and cladding structure. The core includes rare earth-doped active and passive parts. The glass material is prepared by high-temperature melting method and on the drawing tower. Drawing optical fibers avoids the use of stress rods and plastic deformation.

Benefits of technology

The optical fiber preparation process with polarization-maintaining is simple, the yield is high, the birefringence coefficient is controllable, and the temperature stability is good, which avoids damage and fracture of the optical fiber cross-section and improves the birefringence performance and stability of the optical fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087574A_ABST
    Figure CN119087574A_ABST
Patent Text Reader

Abstract

The invention discloses a sandwich-type polarization-maintaining gain optical fiber with a composite structure and a preparation method of the sandwich-type polarization-maintaining gain optical fiber. The optical fiber comprises a sandwich type fiber core and a cladding. The sandwich-type fiber core comprises a first passive part and a second passive part which are located on the two sides of the sandwich-type fiber core, and a rare earth doped active part which is located in the middle of the sandwich-type fiber core and doped with rare earth luminous ions. By regulating and controlling waveguide structure parameters of the sandwich type optical fiber, the birefringence coefficient of the optical fiber is optimized, so that the optical fiber meets the comprehensive requirements for polarization maintaining and other transmission performance. The polarization-maintaining gain optical fiber provided by the invention belongs to a geometric polarization-maintaining optical fiber, and compared with a traditional elliptical core type polarization-maintaining optical fiber, the sandwich type optical fiber does not involve plastic deformation in the preparation process, the processing flow is simple, and the rate of finished products is high. The birefringence coefficient, the stability and the preparation yield of the rare earth doped special polarization maintaining optical fiber are effectively improved, and the application requirement of a novel optical fiber laser on the rare earth doped polarization maintaining optical fiber is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special laser optical fibers, and in particular relates to a sandwich-type polarization-maintaining gain optical fiber with a composite structure and a preparation method thereof. Background Art

[0002] Polarization Maintaining Optical Fiber (PMF) is widely used in fiber optic communications, fiber lasers, fiber gyroscopes, and interferometric sensing due to its ability to maintain linearly polarized light.

[0003] According to the principle of generating birefringence, polarization-maintaining optical fiber can be divided into stress-type polarization-maintaining optical fiber and geometric polarization-maintaining optical fiber. For conventional quartz glass optical fiber, stress-type polarization-maintaining optical fiber inserts stress rods into the optical fiber cladding to generate stress difference in the core in the vertical direction, and then generates mutually perpendicular refractive index difference in the core region through the elastic-optic effect, thereby generating stress birefringence of light. Common stress-type polarization-maintaining optical fibers include panda-type optical fiber and bowtie-type optical fiber (application number: CN202280010508.2). Stress-type polarization-maintaining optical fiber is limited by the requirements of expansion coefficient difference, and stress rods must be inserted or stress layers must be deposited during the preparation process of the preform rod; during the drilling process of the stress hole or the etching and melting process of the deposited layer, the complexity of the preform rod processing increases, and it is easy to damage the preform rod, resulting in a low yield of stress-type polarization-maintaining optical fiber. Finally, the finished stress-type polarization-maintaining optical fiber also faces problems such as susceptibility to temperature disturbance and easy cracking of the optical fiber end face; these characteristics limit the preparation and wide application of stress-type polarization-maintaining optical fiber.

[0004] Geometric polarization-maintaining optical fiber is designed by designing the waveguide structure of the optical fiber so that the core area has a non-circularly symmetrical structure, so that the propagation constants of the two mutually perpendicular linear polarization modes of the transmitted light are unequal, thereby producing geometric birefringence. Common geometric polarization-maintaining optical fibers are elliptical core optical fibers (application number: CN202110961721.9) and microstructure optical fibers with air hole structures (application number: CN202310816716.8). The plastic deformation involved in the preparation of elliptical core preforms makes it difficult to accurately control the ratio of the major and minor axes of the elliptical core, affecting the final parameters of the optical fiber; due to the presence of air holes, the preform construction process and the drawing process of microstructured polarization-maintaining optical fibers are relatively complicated, and there is a problem of difficulty in welding with ordinary step-index optical fibers.

[0005] In order to overcome the problems of complex processing, low yield and poor temperature stability of the current stress-type polarization-maintaining optical fiber preform, and the difficulty in accurately controlling the structural parameters of the current geometric polarization-maintaining optical fiber and the difficulty in drawing, it is necessary to design and prepare a special polarization-maintaining gain optical fiber that is not limited to the optical fiber matrix material, has a large birefringence coefficient, good temperature stability, a simple preparation process, and easy-to-control structural parameters. Summary of the invention

[0006] In order to solve the problems currently faced by special polarization-maintaining gain optical fibers, the present invention provides a sandwich-type polarization-maintaining gain optical fiber with a composite structure and a preparation method thereof.

[0007] The purpose of the present invention is achieved by at least one of the following technical solutions.

[0008] A structurally composite sandwich-type polarization-maintaining gain optical fiber, the optical fiber comprising a sandwich-type core and a cladding; The sandwich-type fiber core comprises a first passive part and a second passive part located at two sides of the sandwich, and a rare-earth doped active part doped with rare-earth luminescent ions located in the middle of the sandwich.

[0009] Furthermore, the diameter D1 of the sandwich core is 3-10 μm.

[0010] Furthermore, the diameter D2 of the cladding is 100-150 μm.

[0011] Furthermore, the thicknesses of the first passive part and the second passive part on both sides of the sandwich core are L2 and L3 respectively, and the structural parameters L2 / D1 and L3 / D1 of the sandwich core are both between 0.01 and 0.49.

[0012] Furthermore, the structure of the cladding layer includes a uniform step structure, a photonic crystal structure or a Bragg structure.

[0013] Furthermore, the rare earth luminescent ions doped in the rare earth doped active part of the sandwich core include Nd, Yb, Er, Tm, Ho or Pr.

[0014] Furthermore, the rare earth luminescent ion doping concentration in the rare earth doped active part of the sandwich core is greater than 1 mol%.

[0015] Furthermore, the material of the sandwich core includes phosphate glass, germanate glass, silicate glass or quartz glass.

[0016] Furthermore, in the sandwich core, the glass transition temperature difference between the rare earth doped active part, the first passive part and the second passive part is ≤50°C; The glass softening point temperature difference between the rare earth doped active part, the first passive part and the second passive part is ≤50°C; The thermal expansion coefficient of the glass between the rare earth doped active part, the first passive part and the second passive part is ≤10×10 -7 / ℃.

[0017] A method for preparing a structurally composite sandwich-type polarization-maintaining gain optical fiber comprises the following steps: S1. Preparation of glass materials: preparing bulk glass materials of the rare earth doped active part, the first passive part and the second passive part of the sandwich core, and cladding glass materials respectively by high temperature melting method; S2. Preparation of a sandwich-type fiber core rod: the three glass materials corresponding to the rare earth-doped active part, the first passive part and the second passive part of the sandwich-type fiber core prepared in step S1 are cut into required sizes according to a set ratio and polished to optical precision; then the three glass materials are stacked in sequence and tightly fitted, and placed in a high-temperature furnace for hot-melt bonding, and after bonding, the temperature is quickly lowered to the annealing temperature and precision annealed to obtain a sandwich-type large-block fiber core glass with a composite structure; the sandwich-type large-block fiber core glass is rounded and polished to a set diameter, and then placed in a drawing tower and drawn at a set temperature to obtain a composite fiber core rod with a sandwich structure; S3. Preparation of sandwich-type polarization-maintaining optical fiber: First, a large piece of cladding glass material is mechanically processed to obtain a cladding glass tube, and then the sandwich-type composite fiber core rod and the cladding glass tube are combined for drawing. The fiber diameter is controlled by controlling the drawing speed and the feeding speed, and finally a structurally composite sandwich-type polarization-maintaining optical fiber is obtained.

[0018] Preferably, in step S1, the high temperature melting method is to melt the raw materials in a high temperature furnace at 1300~1400°C (may fluctuate according to the quality of the raw materials) to obtain glass liquid, then cast the glass liquid into shape, quickly cool it down (cooling rate is greater than 10°C / min), and precisely anneal it (keep it at 600~670°C for 20 hours, and cool it to room temperature at a rate of 5°C / h) to obtain active and passive glass of suitable size.

[0019] Preferably, in step S2, the hot melt bonding is performed in a high temperature furnace at 720-800°C (which may fluctuate according to the size of the glass) for 5-10 minutes, rapid cooling (cooling rate is greater than 10°C / min) and precision annealing (keeping at 600-670°C for 20 hours and cooling to room temperature at a rate of 5°C / h) to obtain a sandwich-type bulk fiber core glass with a composite structure; the sandwich-type bulk fiber core glass is rounded and polished to a set diameter, and then placed in a drawing tower and drawn at 750-800°C to obtain a composite fiber core rod with a sandwich structure.

[0020] Preferably, in step S3, the fiber drawing is performed at 800-850° C., and the fiber diameter is controlled by controlling the fiber drawing speed and the feeding speed, so as to finally obtain a structurally complex sandwich-type polarization-maintaining optical fiber.

[0021] Compared with the prior art, the present invention has the following advantages: (1) Compared with stress-type polarization-maintaining optical fibers, the composite sandwich-type polarization-maintaining gain optical fiber provided by the present invention can achieve polarization maintenance of the mode without drilling holes and inserting stress rods, thereby avoiding damage and breakage of the optical fiber cross section caused by stress.

[0022] (2) Compared with elliptical core polarization-maintaining optical fibers, the sandwich-type polarization-maintaining gain optical fiber with a composite structure provided by the present invention reduces plastic deformation processing and effectively improves the yield rate of polarization-maintaining optical fiber preforms.

[0023] (3) Compared with commercial quartz active polarization-maintaining optical fibers, the composite sandwich-type polarization-maintaining optical fiber provided by the present invention has the characteristics of high rare earth ion doping concentration and large gain coefficient.

[0024] (4) The structure-composite sandwich-type polarization-maintaining gain optical fiber provided by the present invention has a sandwich-type composite fiber core ratio that can be precisely tuned, has good uniformity, and can obtain good birefringence. The birefringence coefficient of the present invention is ≥1×10 -4 . BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the waveguide structure of the sandwich-type polarization-maintaining gain optical fiber with a composite structure in the present invention; Figure 2 Provide x-polarization and y-polarization mode field distribution diagrams of the fundamental mode of the polarization-maintaining optical fiber for Example 1 of the present invention; Figure 3 4 is a relationship diagram between the birefringence coefficient and the core structure parameter L2 / D1 of the sandwich-type polarization-maintaining gain optical fiber of Examples 1 to 4 of the present invention. DETAILED DESCRIPTION

[0026] The present invention provides a sandwich-type polarization-maintaining gain optical fiber with a composite structure, which realizes an active polarization-maintaining optical fiber with high polarization-maintaining performance and high stability through the design of an optical fiber waveguide structure. In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the present invention is not limited to the embodiments.

[0027] Embodiment 1: A Tm / Ho co-doped composite sandwich polarization-maintaining optical fiber, such as Figure 1 As shown, the optical fiber includes a sandwich-type core 100 and a cladding 104; The sandwich-type fiber core 100 includes a first passive part 102 and a second passive part 103 located at two sides of the sandwich, and a rare-earth doped active part 101 doped with rare-earth luminescent ions located in the middle of the sandwich.

[0028] In this embodiment, the material of the sandwich core 100 and the cladding 104 is germanate glass.

[0029] In this embodiment, the glass composition of the first passive part 102, the second passive part 103 and the cladding 104 is (7-15)BaO-(7-15)Ga2O3-(65-85)GeO2-(1-5)La2O3.

[0030] In this embodiment, the rare earth doped active part 101 is Tm / Ho co-doped glass, and the composition is (7-15)BaO-(7-15)Ga2O3-(63-83)GeO2-(1-5)La2O3-1Tm2O3-1Ho2O3.

[0031] In this embodiment, by adjusting the composition ratio of the core and cladding glass, the refractive index of the rare earth doped active part 101 is 1.7376, and the refractive index of the first passive part 102, the second passive part 103 and the cladding 104 glass is 1.7165.

[0032] In this embodiment, the geometric parameters of the polarization-maintaining optical fiber are D1=8 μm, D2=125 μm, L1 / D1=0.24, L2 / D1=L3 / D1=0.38. At this time, the birefringence coefficient of the optical fiber is the largest at a wavelength of 2.0 μm, which is 1.28×10 -4 , the effective mode field area of ​​the optical fiber is 37.4 μm 2 . Figure 2 The x-polarization and y-polarization mode field distribution diagrams of the fundamental mode of the sandwich-type polarization-maintaining optical fiber are given.

[0033] In this embodiment, the Tm / Ho co-doped composite sandwich-type polarization-maintaining optical fiber is prepared by a rod-tube method, including the following steps: S1. Preparation of bulk glass materials: Tm / Ho co-doped active glass and passive glass are prepared by high-temperature melting method, and bulk glass materials of rare earth doped active part 101, first passive part 102 and second passive part 103 of sandwich core 100, as well as bulk cladding glass materials are prepared; the specific process is to weigh raw materials according to the formula and mix them thoroughly, then melt the raw materials in a high-temperature furnace at 1300~1400 ℃ (which may fluctuate according to the quality of the raw materials) to obtain glass liquid, then cast the glass liquid into shape, quickly cool down (cooling rate is greater than 10℃ / min), and precisely anneal (keep at 600~670℃ for 20 hours, and cool to room temperature at a rate of 5℃ / h), to obtain active and passive glass of suitable size; S2. Preparation of a sandwich-type fiber core rod: The three large glass materials of the rare earth-doped active part 101, the first passive part 102 and the second passive part 103 corresponding to the sandwich-type fiber core 100 prepared in step S1 are cut into required sizes according to a set ratio and polished to optical precision; then the three large glass materials are stacked in sequence and tightly fitted, hot-melted at 720-800 °C (which may fluctuate according to the size of the glass) for 5-10 minutes, rapidly cooled (cooling rate greater than 10 °C / min) and precisely annealed (600-670 °C for 20 hours, and cooled to room temperature at a rate of 5 °C / h) to obtain a sandwich-type large fiber core glass with a composite structure; the sandwich-type large fiber core glass is rounded and polished to a set diameter, then placed in a drawing tower, and drawn at 750-800 °C to obtain a composite fiber core rod with a sandwich structure; S3. Preparation of sandwich-type polarization-maintaining optical fiber: First, a large piece of cladding glass material is mechanically processed to obtain a cladding glass tube, and then the sandwich-type composite fiber core rod and the cladding glass tube are combined and drawn at 800~850℃ (depending on the size). The fiber diameter is controlled by controlling the drawing speed and feeding speed, and finally a structurally composite sandwich-type polarization-maintaining optical fiber is obtained.

[0034] The preparation process of the sandwich-type polarization-maintaining gain fiber mentioned above does not involve stress rods, the preparation process is simple, and the preparation process does not involve plastic deformation, and the fiber waveguide structure parameters can be accurately controlled; therefore, the polarization-maintaining fiber is not easily affected by temperature changes and the polarization-maintaining performance is affected, and the preparation process is simple. The theoretical birefringence coefficient of the fiber is 1.28×10 -4 , which can realize the direct output of polarization-maintaining laser in the 2 μm band, is expected to be applied to ultrafast or single-frequency fiber lasers in polarization-maintaining systems.

[0035] Embodiment 2: A Tm-doped composite sandwich-type polarization-maintaining optical fiber, wherein the sandwich-type composite fiber core 100 and the cladding 104 of the optical fiber are both made of germanate glass material.

[0036] In this embodiment, the glass composition of the first passive part 102, the second passive part 103 and the cladding 104 is (7-15)BaO-(7-15)Ga2O3-(65-85)GeO2-(1-5)La2O3.

[0037] In this embodiment, the rare earth doped active part 101 is Tm doped glass, and the composition is (7-15)BaO-(7-15)Ga2O3-(63-83)GeO2-(1-5)La2O3-2Tm2O3.

[0038] In this embodiment, the refractive index of the rare earth doped active part 101 is 1.7376, and the refractive index of the glass of the first passive part 102, the second passive part 103 and the cladding 104 is 1.7165.

[0039] In this embodiment, the geometric parameters of the polarization-maintaining optical fiber are D1=8 μm, D2=125 μm, L1 / D1= 0.18, L2 / D1=L3 / D1= 0.41. At this time, the birefringence coefficient of the optical fiber is the largest at a wavelength of 1.8 μm, which is 1.33×10 -4 , the effective mode field area of ​​the optical fiber is 35.9 μm 2 .

[0040] Furthermore, the preparation process of the polarization-maintaining optical fiber described in this embodiment is the same as that in Embodiment 1. The theoretical birefringence coefficient of the optical fiber is 1.33×10 -4 , which can realize the direct output of polarization-maintaining laser in the 1.8 μm band.

[0041] Embodiment 3: An Er-doped composite sandwich-type polarization-maintaining optical fiber, wherein the sandwich-type composite fiber core 100 and the cladding 104 of the optical fiber are both made of phosphate glass material.

[0042] In this embodiment, the glass composition of the first passive part 102, the second passive part 103 and the cladding 104 is (60-88)P2O5-(5-15)BaO-(5-15)Al2O3-(1-5)La2O3-(1-5)K2O.

[0043] In this embodiment, the rare earth doped active part 101 is Er doped glass, and the composition is (58-86)P2O5-(5-15)BaO-(5-15)Al2O3-(1-5)La2O3-(1-5)K2O3-2Er2O3.

[0044] The refractive index of the rare earth doped active part 101 is 1.5336, and the refractive index of the glass of the first passive part 102, the second passive part 103 and the cladding 104 is 1.5142.

[0045] Furthermore, the geometric parameters of the polarization-maintaining optical fiber in this embodiment are D1=8 μm, D2=125 μm, L1 / D1=0.18, L2 / D1= L3 / D1=0.41. At this time, the birefringence coefficient of the optical fiber is the largest at a wavelength of 1.55 μm, which is 1.32×10 -4 , the effective mode field area of ​​the optical fiber is 32.5 μm 2 .

[0046] Furthermore, the preparation process of the polarization-maintaining optical fiber described in this embodiment is the same as the method in Example 1, except that the temperature system is as follows: the melting temperature of the rare earth-doped active glass and the passive glass is 1000-1250°C (may fluctuate according to the quality of the raw materials), the hot melting temperature of the sandwich-type composite core glass is 550-620°C, the precision annealing is: keeping at 500-550°C for 30 hours and cooling to room temperature at a rate of 3°C / h, the drawing temperature of the sandwich-type composite core rod is 560-600°C, and the drawing temperature of the sandwich-type polarization-maintaining optical fiber is 580-650°C.

[0047] The theoretical birefringence coefficient of the sandwich-type polarization-maintaining gain optical fiber of the Er-doped structure composite described in this embodiment is 1.33×10 -4 , and has a high rare earth doping concentration, and is a 1.5 μm polarization-maintaining laser fiber material with high gain characteristics.

[0048] Example 4 A Nd-doped composite sandwich-type polarization-maintaining optical fiber, wherein the sandwich-type composite fiber core 100 and the cladding 104 of the optical fiber are both made of phosphate glass material.

[0049] The glass composition of the first passive part 102, the second passive part 103 and the cladding 104 is (60-88)P2O5-(5-15)BaO-(5-15)Al2O3-(1-5)La2O3-(1-5)K2O. The rare earth doped active part 101 is Nd doped glass with a composition of (58-86)P2O5-(5-15)BaO-(5-15)Al2O3-(1-5)La2O3-(1-5)K2O3-2Nd2O3.

[0050] Furthermore, in the optical fiber, the refractive index of the rare-earth doped active part 101 is 1.5331, and the refractive index of the glass of the first passive part 102, the second passive part 103 and the cladding 104 is 1.5142.

[0051] Furthermore, the geometric parameters of the polarization-maintaining optical fiber in this embodiment are D1=6 μm, D2=125 μm, L1 / D1=0.18, L2 / D1= L3 / D1=0.41. At this time, the birefringence coefficient of the optical fiber at a wavelength of 1.06 μm is the largest, which is 1.28×10 -4 , the effective mode field area of ​​the optical fiber is 15.5 μm 2 .

[0052] Furthermore, the preparation process of the polarization-maintaining optical fiber described in this embodiment is the same as that in Embodiment 3.

[0053] The theoretical birefringence coefficient of the Nd-doped polarization-maintaining gain fiber at a wavelength of 1.06 μm is 1.28×10-4 , has a high rare earth doping concentration, and is a high-gain polarization-maintaining optical fiber material in the 1 μm band; and the optical fiber properties are stable, and the birefringence coefficient is not easily affected by temperature changes.

[0054] Figure 3 A relationship diagram between the birefringence coefficient and the core structure parameter L2 / D1 of the composite polarization-maintaining optical fiber of the structure described in Examples 1 to 4 is given.

[0055] The above-described embodiments only express several implementation methods of the present invention, but should not be understood as limiting the scope of protection of the present invention. It should be pointed out that for those skilled in the art to which the present invention belongs, the supplement or optimization made to the present invention without departing from the concept of the present invention still falls within the scope of protection of the present invention.

Claims

1. A composite sandwich-type polarization-maintaining gain optical fiber, characterized in that: It comprises a sandwich-type fiber core (100) and a cladding (104); The sandwich-type fiber core (100) comprises a first passive part (102) and a second passive part (103) located on both sides of the sandwich, and a rare earth doped active part (101) doped with rare earth luminescent ions located in the middle of the sandwich.

2. The structure-complex sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The thicknesses of the first passive part (102) and the second passive part (103) on both sides of the sandwich-type fiber core (100) are L2 and L3 respectively, the diameter of the sandwich-type fiber core (100) is D1, and the structural parameters L2 / D1 and L3 / D1 of the sandwich-type fiber core (100) are both 0.01-0.

49.

3. The composite sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The diameter D1 of the sandwich-type fiber core (100) is 3-10 μm.

4. The composite sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The diameter D2 of the cladding (104) is 100-150 μm.

5. The composite sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The structure of the cladding (104) includes a uniform step structure, a photonic crystal structure or a Bragg structure.

6. The composite sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The rare earth luminescent ions doped in the rare earth doped active part (101) in the sandwich-type fiber core (100) include Nd, Yb, Er, Tm, Ho or Pr.

7. The composite sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The rare earth luminescent ion doping concentration in the rare earth doped active part (101) in the sandwich-type fiber core (100) is greater than 1 mol%.

8. The structure-complex sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: The material of the sandwich-type fiber core (100) includes phosphate glass, germanate glass, silicate glass or quartz glass.

9. The structure-complex sandwich-type polarization-maintaining gain optical fiber according to claim 1, characterized in that: In the sandwich-type fiber core (100), the glass transition temperature difference between the rare earth doped active part (101), the first passive part (102) and the second passive part (103) is ≤50°C; The glass softening point temperature difference between the rare earth doped active part (101), the first passive part (102) and the second passive part (103) is ≤50°C; The thermal expansion coefficient of the glass between the rare earth doped active part (101), the first passive part (102) and the second passive part (103) is ≤10×10 -7 / ℃.

10. A method for preparing a structurally composite sandwich-type polarization-maintaining gain optical fiber according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Preparation of glass materials: preparing the glass materials of the rare earth doped active part (101), the first passive part (102) and the second passive part (103) of the sandwich core (100) and the cladding glass material respectively by a high temperature melting method; S2, preparation of a sandwich-type fiber core rod: the three glass materials of the rare earth-doped active part (101), the first passive part (102) and the second passive part (103) corresponding to the sandwich-type fiber core (100) prepared in step S1 are cut into required sizes according to a set ratio and polished to optical precision; then the three large glass materials are stacked in sequence and tightly fitted, and placed in a high-temperature furnace for hot-melt bonding, and after bonding, the temperature is lowered to the annealing temperature and precision annealed to obtain a sandwich-type large fiber core glass with a composite structure; the sandwich-type large fiber core glass is rounded and polished to a set diameter, and then placed in a drawing tower and drawn at a set temperature to obtain a composite fiber core rod with a sandwich structure; S3. Preparation of sandwich-type polarization-maintaining optical fiber: First, the cladding glass material is mechanically processed to obtain a cladding glass tube, and then the sandwich-type composite fiber core rod and the cladding glass tube are combined for drawing. The optical fiber diameter is controlled by controlling the drawing speed and the feeding speed, and finally a structurally composite sandwich-type polarization-maintaining optical fiber is obtained.

Citation Information

Patent Citations

  • Single crystal fiber with Bragg structure cladding and manufacturing method thereof

    CN102253445A

  • Rare earth doped structure composite optical fiber with multiband gain effect and preparation method and application thereof

    CN118420214A

  • Optical fiber for optical amplification

    JP1998117034A

  • Optical fiber with multi section core

    US20100103958A1