Transparent photoresist composition and preparation method thereof, pixel device, semiconductor device and module device

By using N-heterocyclic enamine in transparent photoresist to copolymerize film-forming resins with side chains containing aromaticene chains, high thickness and low temperature curing are achieved, and the high temperature curing and heat resistance of existing photoresist are solved. The problem of insufficient improvements in the performance and stability of the dry film layer.

CN119087743APending Publication Date: 2024-12-06SHENZHEN BRTHRBORDER SEMICON MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410856346.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing transparent photoresist used for Micro LED requires high-temperature curing, and the cured dry film thickness is insufficient, so low-temperature curing cannot be achieved, affecting the heat resistance of quantum dot materials.

Method used

The film-forming resin is used to copolymerize N-heterocyclic enamine with side chains containing aromatic cyclic enamine chains. The double bonds of N-heterocyclic enamine participate in the stereo crosslinking reaction to increase the thickness of the transparent photoresist and realize the Low temperature curing.

Benefits of technology

The thickness and heat resistance of the dry film layer are improved, and can be cured under low temperature conditions, and remain stable under the erosion of acid and alkali, solvent, film stripping liquid, and copper etching liquid, with a surface resistivity of 5.0E×1016 ohms or above. Suitable for environments of 25-200℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087743A_ABST
    Figure CN119087743A_ABST
Patent Text Reader

Abstract

The invention discloses a transparent photoresist composition, a preparation method thereof, a semiconductor device structure, a pixel device structure and application of the transparent photoresist composition in automobiles and wearable equipment. Wherein the preparation materials of the transparent photoresist composition comprise acrylic resin, a photoinitiator, a photocuring monomer, an auxiliary agent, a solvent and film-forming resin, and the film-forming resin is prepared by copolymerizing an enamine group (i) with N-heterocyclic ring and an alkene chain (ii) with a side chain containing an aromatic ring. The transparent photoresist composition provided by the invention aims to improve the film thickness after construction such as coating, photoetching and the like, and can realize low-temperature curing at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photoresists, and in particular to a transparent photoresist composition and a preparation method thereof, a semiconductor device, a pixel device, and a module device. Background Art

[0002] The display principle of Micro LED (Micro Light Emitting Diode Display) is to thin-film, miniaturize and array the LED structure design of the three primary colors of red, green and blue, so that its size is only about 1-10 microns; then the micron-level LEDs are transferred to the circuit substrate in batches, and the circuits and transistors are installed under each micron LED to complete a simple Micro LED display. Each pixel of Micro LED contains three RGB LED sub-pixels that can be self-luminous and independently controlled. Since Micro LED uses a separate self-luminous micron-level LED, it is outstanding in color expression. The full width at half maximum (FWHM) of the main wavelength of the micron LED emission spectrum is only about 20nm, which can provide extremely high color saturation, usually greater than 120% NTSC, which is almost the same as the color gamut that can be provided by the current top OLED displays. At the same time, due to the stability of LED inorganic substances, the color can remain consistent and stable no matter how long it is used, which is unmatched by OLED.

[0003] Micro LED also has the advantages of power saving and ultra-high brightness. In traditional LCD TVs, the display efficiency is about 3%. The loss of TFT in LCD is very small because it is voltage-driven, but due to the energy loss in the color filter, polarizer and LC material, the efficiency of LCD is very low. Micro LED has a simple structure, low energy consumption, and higher photoelectric conversion efficiency. The power consumption can be as low as 10% of LCD and 50% of OLED. It greatly reduces the unit power consumption while allowing higher energy to be used for direct light emission.

[0004] The transparent photoresist currently used for Micro LED, even the high-temperature curing transparent photoresist that is maturely used on OGS, has a curing temperature of 230°C and a dry film thickness of 1.5-2.5μm. Although this photoresist can achieve a higher film thickness by adjusting the solid content and viscosity, it cannot achieve low-temperature curing.

[0005] In addition, in order to achieve precise control of the process, automation technology is used to achieve precise control of key processes such as photoresist coating, baking, exposure and development during the photolithography process. This includes strict control of parameters such as the speed of spin coating, baking temperature, exposure dose and time to ensure the uniformity and consistency of the photoresist layer. Real-time development detection is used to monitor the development process and control the development time to control the groove shape. Spectral detection and pattern matching methods are used to achieve non-destructive detection of the groove parameters of chrome grating grinding.

[0006] In order to facilitate real-time monitoring and feedback, integrated sensors and monitoring systems are used to monitor key parameters in the lithography process, such as the thickness and uniformity of the photoresist, in real time, and the process parameters are adjusted in real time based on the monitoring results to optimize the performance of the photoresist.

[0007] On this basis, the formula is optimized and feedback control rate technology is used to collect data feedback during the photolithography process to adjust the photoresist formula, thereby effectively screening out the photoresist formula with the best sensitivity, resolution and contrast.

[0008] The above contents are only used to assist in understanding the technical solution of the invention and do not constitute an admission that the above contents are prior art. Summary of the invention

[0009] The main purpose of the present invention is to provide a transparent photoresist composition and a preparation method thereof, a semiconductor device, a pixel device, and a module device, aiming to increase the film thickness and achieve low-temperature curing at the same time.

[0010] To achieve the above-mentioned purpose, the present invention provides a transparent photoresist composition, wherein the preparation materials of the transparent photoresist composition include acrylic resin, photoinitiator, auxiliary agent, solvent photocuring monomer and film-forming resin, and the film-forming resin includes an enamine (i) with an N-heterocyclic ring and an olefin chain (ii) with an aromatic ring in the side chain.

[0011] In one embodiment, the structure of the enamine with an N-heterocyclic ring is shown in formula (i):

[0012]

[0013] In formula (i), R1 and R2 are methyl groups or hydrogen atoms;

[0014] Z is one of a N-containing aromatic heterocycle and a N-containing aliphatic heterocycle.

[0015] In one embodiment, the structure of the olefin chain containing an aromatic ring in the side chain is shown in formula (ii):

[0016]

[0017] In formula (ii), R4 is a methyl group or a hydrogen atom;

[0018] R3 is H or a C2-C20 alkyl group;

[0019] Y is an unsaturated aromatic hydrocarbon group or a cyclic hydrocarbon structure.

[0020] In one embodiment, the structure of the film-forming resin is as shown in formula (1):

[0021]

[0022] In formula (1), n=60-180;

[0023] R1, R2 and R4 are methyl groups or hydrogen atoms;

[0024] R3 is H or a C2-C20 alkyl group;

[0025] Y is an unsaturated aromatic hydrocarbon group or a cyclic hydrocarbon structure;

[0026] Z is one of a N-containing aromatic heterocycle and a N-containing aliphatic heterocycle.

[0027] In one embodiment, the group of Z includes

[0028] One of them.

[0029] In one embodiment, the group of Y includes one of phenyl, methylphenyl, dimethylphenyl, trimethylphenyl, ethylphenyl, isopropylphenyl, butylphenyl, hydroxyphenyl, methoxyphenyl, acetoxyphenyl, butoxyphenyl, chlorophenyl, bromophenyl, dichlorophenyl, and chloromethylphenyl.

[0030] In one embodiment, the transparent photoresist composition is prepared from materials including, by weight:

[0031] Acrylic resin 5-40 parts;

[0032] Photoinitiator 0.5-10 parts;

[0033] 5-50 parts of photocurable monomer;

[0034] 5-50 parts of film-forming resin;

[0035] 0.2-5 parts of additives;

[0036] Solvent 10-200 parts.

[0037] In one embodiment, the acrylic resin includes one or more of a copolymer of methacrylic acid and methyl methacrylate, a copolymer of methacrylic acid and cyclohexyl methacrylate, a copolymer of methacrylic acid and glycidoxy methacrylate, a copolymer of methacrylic acid and 2-hydroxyethyl methacrylate, a copolymer of methacrylic acid and cyclohexyl methacrylate, and a copolymer of styrene and 2-hydroxyethyl methacrylate; and / or,

[0038] The photoinitiator includes an oxime ester initiator and an imidazole initiator; and / or,

[0039] The photocurable monomer includes an oligomer crosslinking agent containing olefinic double bonds; and / or,

[0040] The auxiliary agent includes one or more of a coupling agent, a leveling agent, a defoaming agent, a UV absorber, and a stabilizer; and / or,

[0041] The solvent includes one or more of N,N'-dimethylformamide, N-methylpyrrolidone (NMP), N-ethyl-2-pyrrolidone, N,N'-dimethylacetamide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazoline, N-cyclohexyl-2-pyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, γ-butyrolactone, propylene glycol monomethyl ether acetate, and diethylene glycol monomethyl ether.

[0042] In one embodiment, the average acid value of the acrylic resin is 75-140 mgKOH / g; and / or,

[0043] The usage ratio of the oxime ester initiator to the imidazole initiator is 1:1-1:3; and / or,

[0044] The ratio of the photoinitiator to the photocurable monomer is 1:6-1:100;

[0045] The photocurable monomer includes one or more of pentaerythritol triacrylate, pentaerythritol tetraacrylate, 3-hydroxymethyl pentaerythritol triacrylate, 3-hydroxyethyl pentaerythritol triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate.

[0046] The present invention also provides a method for preparing a transparent photoresist composition, which is used to prepare the transparent photoresist composition, comprising an N-heterocyclic intermediate, wherein the N-heterocyclic intermediate comprises

[0047] One of the methods, wherein an N-heterocyclic enamine is prepared by a Stork synthesis reaction; wherein the preparation materials of the transparent photoresist composition include an acrylic resin, a photoinitiator, an auxiliary agent, a solvent photocurable monomer and a film-forming resin, and the film-forming resin includes an enamine (i) with an N-heterocyclic ring and an olefin chain (ii) having an aromatic ring in the side chain.

[0048] In one embodiment, the film-forming resin is formed by copolymerizing a free radical solution of an enamine group (i) having an N-heterocyclic ring and a free radical solution of an olefin chain (ii) having an aromatic ring in the side chain.

[0049] The present invention also provides a pixel device, comprising a substrate and a dry film layer arranged on the substrate, wherein the dry film layer is formed by curing the above-mentioned transparent photoresist composition; wherein the substrate is a glass substrate, a Si substrate, a PET substrate, a CPI substrate, a COP substrate or a PEN substrate; the transparent photoresist composition is cured by spin coating, pre-baking, exposure, mid-baking, developing, post-UV and post-baking processes to form the dry film layer; the preparation materials of the transparent photoresist composition include acrylic resin, photoinitiator, auxiliary agent, solvent photocuring monomer and film-forming resin, and the film-forming resin includes an enamine (i) with an N-heterocyclic ring and an olefin chain (ii) with an aromatic ring in the side chain.

[0050] The present invention also proposes a semiconductor device, which includes a substrate pixel device of a micro-light-emitting diode (Micro-LED) display and / or a radio frequency chip, the substrate pixel device includes the above-mentioned pixel device, the pixel device includes a micro-light-emitting diode display having an upper layer, a lower layer, or an upper and lower two-layer structure containing the dry film layer, and the dry film layer is prepared using a black photoresist composition; wherein, a black photoresist composition, in parts by weight, includes: 2 to 20 parts of bisphenol fluorene acrylic resin, 1 to 10 parts of tertiary amine resin containing β to H atoms, 0.1 to 2 parts of perfluorinated substituted ethylene monomer auxiliary agent A, 0.2 to 5 parts of aromatic peroxide auxiliary agent B, 0.5 to 2 parts of photoinitiator, 5 to 10 parts of photocurable resin monomer, 10 to 50 parts of black colorant and 50 to 500 parts of polar organic solvent.

[0051] The present invention also proposes a module device, which includes a vehicle-mounted display screen, a wearable device display screen or a chip packaging device, and the vehicle-mounted display screen, the wearable device display screen or the chip packaging device includes the above-mentioned semiconductor device.

[0052] The film-forming resin of the technical solution of the present invention comprises an enamine with an N-heterocyclic ring and an olefin chain with an aromatic ring in the side chain, and the double bond of the enamine with the N-heterocyclic ring participates in a stereo cross-linking reaction, thereby increasing the thickness of the transparent photoresist composition, so that the dry film layer after curing does not collapse, thereby increasing the thickness of the dry film layer; at the same time, the transparent photoresist composition can be cured at low temperature, solving the problem of low heat resistance limit of quantum dot materials. The transparent photoresist composition of the present invention is resistant to acid, alkali, solvent, stripping liquid, copper etching liquid, and 25-200°C metal plating after film formation and curing into a dry film layer. Its surface resistivity is stable at 5.0E×10 16 Ohm or more. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0054] Figure 1 Schematic diagram of the molecular formula of the film-forming resin of the present invention;

[0055] Figure 2 A schematic diagram of the structure of a Micro-LED device in which the photoresist of the present invention is located;

[0056] Figure 3 This is a SEM morphology image of the pattern on the carrier board where the photoresist of the present invention is located;

[0057] Figure 4 This is a SEM development appearance image of the pattern on the carrier board where the photoresist of the present invention is located;

[0058] Figure 5 This is a picture taken under a microscope after the carrier board where the photoresist of the present invention is "dug" and developed;

[0059] Figure 6 This is a picture taken under a microscope after lines are made on the carrier board where the photoresist of the present invention is located. DETAILED DESCRIPTION

[0060] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] It should be noted that if the meaning of "and / or" appears in the full text is to include three parallel solutions, taking "A and / or B" as an example, it includes solution A, solution B, or a solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0062] "Include", "comprising", "containing", "containing", "having" or other variations herein are intended to cover non-closed inclusions, and no distinction is made between these terms. The term "comprising" means that other steps and ingredients that do not affect the final result may be added. The term "comprising" also includes the terms "mainly consisting of..." and "essentially consisting of..." The compositions and methods / processes of the present invention include, consist of, and are essentially composed of the necessary elements and restrictions described herein and any additional or optional ingredients, components, steps or restrictions described herein. All numerical values ​​or expressions used in the specification and claims involving component amounts, process conditions, etc. should be understood to be modified by "about" in all cases. All ranges involving the same component or property include endpoints, which can be independently combined. Since these ranges are continuous, they include every numerical value between the minimum and maximum values. It should also be understood that any numerical range cited in this application is intended to include all sub-ranges within the range. As used herein, "parts by weight", "parts by weight", "parts by mass" or "parts by mass" are used interchangeably, and the parts by weight may be any fixed weight expressed in milligrams, grams or kilograms (such as 1 mg, 1 g, 2 g, 5 g, or 1 kg, etc.). For example, a composition consisting of 1 part by weight of component a and 9 parts by weight of component b may be a composition consisting of 1 gram of component a + 9 grams of component b, or 10 grams of component a + 90 grams of component b, etc.

[0063] In the related technology, the transparent photoresist used for Micro LED requires high-temperature curing, and its curing temperature is generally above 200°C, and the thickness of the dry film after curing is only 1.5-2.5μm; and the heat resistance temperature limit of quantum dot materials is small.

[0064] To this end, the present invention provides a transparent photoresist composition.

[0065] In an embodiment of the present invention, the preparation materials of the transparent photoresist composition include acrylic resin, photoinitiator, photocurable monomer and film-forming resin, and the film-forming resin includes an enamine (i) with an N-heterocyclic ring and an olefin chain (ii) with an aromatic ring in the side chain.

[0066] The transparent photoresist composition is polymerized into a novel film-forming resin by an enamine with an N-heterocyclic ring and an olefin chain with an aromatic ring on the side chain. The transparent photoresist composition has a large dry film thickness after curing, and low-temperature curing can be achieved at the same time. The deformation of the dry film layer is small, and the low-temperature curing operation also reduces the influence of the quantum dot material.

[0067] The film-forming resin of the technical solution of the present invention comprises an enamine with an N-heterocyclic ring and an olefin chain with an aromatic ring in the side chain, and the double bond of the enamine with the N-heterocyclic ring participates in a stereo cross-linking reaction, thereby increasing the thickness of the transparent photoresist composition, so that the dry film layer after curing does not collapse, thereby increasing the thickness of the dry film layer; at the same time, the transparent photoresist composition can be cured at low temperature, solving the problem of low heat resistance limit of quantum dot materials. The transparent photoresist composition of the present invention is resistant to acid, alkali, solvent, stripping liquid, copper etching liquid, and 25-200°C metal plating after film formation and curing into a dry film layer. Its surface resistivity is stable at 5.0E×10 16 Ohm or more.

[0068] The structure of the enamine with an N-heterocyclic ring is various. In one embodiment, the structure of the enamine with an N-heterocyclic ring is shown in formula (i):

[0069]

[0070] In formula (i), R1 and R2 are methyl groups or hydrogen atoms; and Z is one of a N-containing aromatic heterocycle and a N-containing aliphatic heterocycle.

[0071] Similarly, there are various structures of the olefin chain containing an aromatic ring in the side chain. In one embodiment, the structure of the olefin chain containing an aromatic ring in the side chain is shown in formula (ii):

[0072]

[0073] In formula (ii), R4 is a methyl group or a hydrogen atom; R3 is H or a C2-C20 alkyl group; and Y is an unsaturated aromatic hydrocarbon group or a cyclic hydrocarbon structure.

[0074] There are various structures of film-forming resins copolymerized with enamines having N-heterocyclic rings and olefin chains having aromatic rings on the side chains. In one embodiment, the structure of the film-forming resin is as shown in formula (1):

[0075]

[0076] In formula (1), n=60-180; R1, R2 and R4 are methyl or hydrogen atoms; R3 is H or a C2-C20 alkyl group; Y is an unsaturated aromatic hydrocarbon group or a cyclic hydrocarbon structure; and Z is one of a N-containing aromatic heterocycle or a N-containing aliphatic heterocycle.

[0077] In one embodiment, the group of Z is selected from one of the following structures:

[0078]

[0079] In one embodiment, the group of Y includes one of phenyl, methylphenyl, dimethylphenyl, trimethylphenyl, ethylphenyl, isopropylphenyl, butylphenyl, hydroxyphenyl, methoxyphenyl, acetoxyphenyl, butoxyphenyl, chlorophenyl, bromophenyl, dichlorophenyl, and chloromethylphenyl.

[0080] In one embodiment, the preparation materials of the transparent photoresist composition include, by weight: 5-40 parts of acrylic resin; 0.5-10 parts of photoinitiator; 5-50 parts of photocurable monomer; 5-50 parts of film-forming resin; 0.2-5 parts of auxiliary agent; and 10-200 parts of solvent.

[0081] The transparent photoresist composition can be prepared by mixing acrylic resin, photoinitiator, photocurable monomer, film-forming resin, auxiliary agent and solvent in parts by weight, dispersing them uniformly, and filtering them to obtain a photosensitive solution of the transparent photoresist composition. In this operation, undissolved particles and impurities can be removed by filtering.

[0082] Further, in one embodiment, the acrylic resin includes one or more of a copolymer of methacrylic acid and methyl methacrylate, a copolymer of methacrylic acid and cyclohexyl methacrylate, a copolymer of methacrylic acid and glycidoxy methacrylate, a copolymer of methacrylic acid and 2-hydroxyethyl methacrylate, a copolymer of methacrylic acid and cyclohexyl methacrylate, and a copolymer of styrene and 2-hydroxyethyl methacrylate.

[0083] The average acid value of the acrylic resin cannot be too high or too low. If the average acid value is too high, it is easy to over-develop, resulting in poor patterning; if the average acid value is too low, it is difficult to achieve graphic accuracy during development, which also results in poor patterning. In one embodiment, the average acid value of the acrylic resin is 75-140 mgKOH / g.

[0084] In one embodiment, the photocurable monomer includes an oligomer crosslinker containing olefinic double bonds. Further, in one embodiment, the photocurable monomer includes one or more of pentaerythritol triacrylate, pentaerythritol tetraacrylate, 3-hydroxymethyl pentaerythritol triacrylate, 3-hydroxyethyl pentaerythritol triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate.

[0085] In one embodiment, the photoinitiator includes an oxime ester initiator and an imidazole initiator. Among them, the oxime ester initiator plays a photoinitiating role to achieve a photocuring effect; the imidazole initiator plays a photoinitiating and thermal initiating role in the pre-baking and post-baking stages. In one embodiment, the dosage ratio of the oxime ester initiator to the imidazole initiator is 1:1-1:3.

[0086] If the amount of the photoinitiator is too much, it will not only increase the cost, but also easily lead to photoinitiator residue, resulting in overexposure and affecting reliability; and if the amount of the photoinitiator is too little, it will lead to incomplete curing. Therefore, in one embodiment, the amount ratio of the photoinitiator to the photocurable monomer is 1:6-1:100. Further, in one embodiment, the amount ratio of the photoinitiator to the photocurable monomer is 1:15-1:100. Further, in one embodiment, the amount ratio of the photoinitiator to the photocurable monomer is 1:10-1:50. Further, in one embodiment, the amount ratio of the photoinitiator to the photocurable monomer is 1:6-1:20.

[0087] In one embodiment, the auxiliary agent includes one or more of a coupling agent, a leveling agent, a defoaming agent, an ultraviolet absorber, and a stabilizer. The auxiliary agent is used to increase low-temperature crosslinking and curing, thereby further improving the low-temperature curing effect of the transparent photoresist composition.

[0088] The solvent is used to dissolve and disperse the resin uniformly, and is also beneficial to photopolymerization and thermal polymerization. In one embodiment, the solvent includes one or more of N,N'-dimethylformamide, N-methylpyrrolidone (NMP), N-ethyl-2-pyrrolidone, N,N'-dimethylacetamide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazoline, N-cyclohexyl-2-pyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, γ-butyrolactone, propylene glycol monomethyl ether acetate, and diethylene glycol monomethyl ether.

[0089] The present invention also provides a method for preparing a transparent photoresist composition, which is used to prepare the transparent photoresist composition. The method for preparing the film-forming resin comprises the following steps:

[0090] S1, using the N-heterocyclic intermediate to obtain the enamine with N-heterocyclic ring;

[0091] S2, using the N-heterocyclic enamine monomer (i) and the Y group-containing monomer (ii) to perform free radical solution copolymerization under initiator conditions to synthesize the film-forming resin.

[0092] In step S1, a method for preparing an enamine is proposed, wherein the group of the following N-heterocyclic intermediate Z is selected from one of the following structures:

[0093]

[0094] The enamine with N-heterocyclic ring is synthesized via the Stork synthesis reaction route.

[0095] The reaction characteristics:

[0096] (1) Prepared from aldehydes, ketones and one equivalent of N-heterocyclic intermediates in the presence of a dehydrating agent;

[0097] (2) During the preparation reaction, acetal amines are usually produced, which can be converted into enamines by water distillation;

[0098] (3) Allyl-, benzyl-, propargyl-, or active alkyl halides such as active halogenated aromatic hydrocarbons;

[0099] (4) Large steric hindrance ketones or large steric hindrance amines form enamines, and the reaction rate is slow;

[0100] (5) This reaction regioselectively proceeds on the side of the ketone with fewer substituents.

[0101]

[0102] In one embodiment, the film-forming resin is prepared by free radical solution copolymerization of the above-mentioned enamine monomer (i) with an N-heterocyclic ring and the monomer (ii) containing a Y group under initiator conditions. The copolymer molecular equivalent is controlled between 20-200, preferably between 40-180, and more preferably between 80-150.

[0103] In one embodiment, the N-heterocyclic enamine monomer (i) includes, but is not limited to, the following compounds:

[0104]

[0105] In one embodiment, the substances with Y group monomer (ii) include but are not limited to the following compounds:

[0106]

[0107] The initiator includes but is not limited to the following compounds: one or a combination of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, and dodecanoyl peroxide.

[0108] The free radical reaction is generated in the same solvent as the photoresist composition, and the solvents are not listed one by one. The reaction starting temperature is 90°C, and the reaction is continued for 5 hours before the temperature is raised to 105°C for 3 hours. The degree of polymerization can be controlled by adjusting the amount and type of initiator.

[0109] The present invention further provides a pixel device, which includes a substrate and a dry film layer disposed on the substrate, wherein the dry film layer is formed by curing the transparent photoresist composition. The specific parameter performance of the pixel device refers to the above embodiment. Since the transparent photoresist composition adopts all the technical solutions of all the above embodiments, it at least has all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0110] In one embodiment, the substrate is a glass substrate, a Si substrate, a PET substrate, a CPI substrate, a COP substrate or a PEN substrate. The Slit process can be used to coat the transparent photoresist composition on the substrate, and after vacuum -1atm / 30s, it is baked at 120-140°C to form a dry film layer. It is understandable that the dry film layer can be an insulating protective layer. The transparent photoresist composition is cured by spin coating (Spin), pre-baking, exposure, mid-baking, developing, post-UV, and post-baking processes to form a dry film layer.

[0111] The present invention further provides a semiconductor device, which includes a substrate pixel device of a micro-light emitting diode (Micro-LED) display and / or a radio frequency chip, wherein the substrate pixel device includes the above-mentioned pixel device, and the pixel device includes a micro-light emitting diode display having an upper layer, a lower layer, or an upper and lower two-layer structure containing the dry film layer, wherein the dry film layer is prepared by a black photoresist composition;

[0112] Among them, a black photoresist composition comprises, by weight, 2 to 20 parts of bisphenol fluorene acrylic resin, 1 to 10 parts of tertiary amine resin containing β-H atoms, 0.1 to 2 parts of perfluorinated substituted ethylene monomer auxiliary A, 0.2 to 5 parts of aromatic peroxide auxiliary B, 0.5 to 2 parts of photoinitiator, 5 to 10 parts of photocurable resin monomer, 10 to 50 parts of black colorant and 50 to 500 parts of polar organic solvent.

[0113] In one embodiment, the method for preparing the black photoresist dry film layer comprises the following steps:

[0114] Coating: coating the transparent photoresist composition on the upper layer, the lower layer, or both layers of the transparent photoresist dry film layer;

[0115] Pre-baking: The coated substrate is baked at 85-120°C for 110-240s;

[0116] Exposure: Exposure energy 50-300mj / cm2;

[0117] Post-baking: 130-180℃, baking for 30-60min.

[0118] In the coating operation, Slit or Slit+Spin mode can be used, vacuum -1atm / 30s. The pre-baking operation removes the solvent in the photoresist, enhances adhesion, releases the stress in the photoresist film, and prevents the photoresist from contaminating the equipment. In the exposure operation, direct exposure can be used, parallel light can be used for exposure; visible light, ultraviolet light, electron beam and X-ray radiation energy can be used for exposure. The post-baking operation is used to cure the transparent photoresist composition into a dry film layer. The post-baking temperature is 130-180°C or below, thereby achieving low-temperature curing and avoiding high temperature from affecting the quantum dot material.

[0119] The dry film layer can be a thin layer: 0.5-2 μm; or a thick layer: 4-40 μm.

[0120] The dry film layer can be a thin layer or a thick layer. In one embodiment, the thickness of the dry film layer is 10-200 μm. Further, in one embodiment, the thickness of the dry film layer is 0.5-2.0 μm. Alternatively, in one embodiment, the thickness of the dry film layer is 4-40 μm. The thick dry film layer not only fills the gaps between the quantum dots, but is also greater than the height of the quantum dot pixel layer, thereby flattening and insulating the quantum dot pixel layer.

[0121] The present invention also proposes a module device, the module device includes a vehicle display screen, a wearable device display screen or a chip packaging device, and the vehicle display screen, the wearable device display screen or the chip packaging device includes the above-mentioned semiconductor device. Taking a wearable device as an example, the wearable device includes a main body and the above-mentioned pixel device, and the pixel device is installed on the main body to improve the display information such as images; in one embodiment, the wearable device includes VR, AR or MR.

[0122] The embodiments of the present invention will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0123] Example 1

[0124] A transparent photoresist composition comprises, by weight, 5 parts of acrylic resin, 1 part of photoinitiator, 8 parts of photocurable monomer, 8 parts of film-forming resin, 0.5 parts of auxiliary agent and 20 parts of solvent.

[0125] Dry film preparation method:

[0126] Coating: coating the transparent photoresist composition on the substrate to form a coating on the surface of the substrate;

[0127] Pre-baking: The coated substrate is baked at 90°C for 120 seconds;

[0128] Exposure: Exposure energy 100mj / cm2;

[0129] Post-baking: 90℃, bake for 30-60min, solidify into dry film layer.

[0130] Example 2

[0131] A transparent photoresist composition comprises, by weight, 5 parts of acrylic resin, 1.2 parts of photoinitiator, 8 parts of photocurable monomer, 10 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0132] The method for preparing the dry film layer is the same as that in Example 1.

[0133] Example 3

[0134] A transparent photoresist composition comprises, by weight, 8 parts of acrylic resin, 1.5 parts of photoinitiator, 8 parts of photocurable monomer, 6 parts of film-forming resin, 0.5 parts of auxiliary agent and 20 parts of solvent.

[0135] The method for preparing the dry film layer is the same as that in Example 1.

[0136] Example 4

[0137] A transparent photoresist composition comprises, by weight, 5 parts of acrylic resin, 1 part of photoinitiator, 10 parts of photocurable monomer, 15 parts of film-forming resin, 0.5 parts of auxiliary agent and 20 parts of solvent.

[0138] The method for preparing the dry film layer is the same as that in Example 1.

[0139] Example 5

[0140] A transparent photoresist composition comprises, by weight, 5 parts of acrylic resin, 1 part of photoinitiator, 6 parts of photocurable monomer, 8 parts of film-forming resin, 1 part of auxiliary agent and 20 parts of solvent.

[0141] The method for preparing the dry film layer is the same as that in Example 1.

[0142] Example 6

[0143] A transparent photoresist composition comprises, by weight, 6 parts of acrylic resin, 1 part of photoinitiator, 9 parts of photocurable monomer, 15 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0144] The method for preparing the dry film layer is the same as that in Example 1.

[0145] Example 7

[0146] A transparent photoresist composition comprises, by weight, 6 parts of acrylic resin, 1 part of photoinitiator, 9 parts of photocurable monomer, 13 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0147] The method for preparing the dry film layer is the same as that in Example 1.

[0148] Example 8

[0149] A transparent photoresist composition comprises, by weight, 6 parts of acrylic resin, 1.2 parts of photoinitiator, 10 parts of photocurable monomer, 14 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0150] The method for preparing the dry film layer is the same as that in Example 1.

[0151] Example 9

[0152] A transparent photoresist composition comprises, by weight, 6 parts of acrylic resin, 1.2 parts of photoinitiator, 9 parts of photocurable monomer, 15 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0153] The method for preparing the dry film layer is the same as that in Example 1.

[0154] Example 10

[0155] A transparent photoresist composition comprises, by weight, 5 parts of acrylic resin, 1.2 parts of photoinitiator, 10 parts of photocurable monomer, 14 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0156] The method for preparing the dry film layer is the same as that in Example 1.

[0157] Embodiment 11

[0158] A transparent photoresist composition comprises, by weight, 5 parts of acrylic resin, 1.2 parts of photoinitiator, 9 parts of photocurable monomer, 14 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0159] The method for preparing the dry film layer is the same as that in Example 1.

[0160] Example 12

[0161] A transparent photoresist composition comprises, by weight, 6 parts of acrylic resin, 1.2 parts of photoinitiator, 10 parts of photocurable monomer, 14 parts of film-forming resin, 0.8 parts of auxiliary agent and 25 parts of solvent.

[0162] The method for preparing the dry film layer is the same as that in Example 1.

[0163] Comparative Example 1

[0164] A transparent photoresist composition comprises, by weight, 3 parts of acrylic resin, 0.2 parts of photoinitiator, 2 parts of photocurable monomer, 1 part of film-forming resin, 0.1 parts of auxiliary agent and 200 parts of solvent.

[0165] The method for preparing the dry film layer is the same as that in Example 1.

[0166] Comparative Example 2

[0167] A transparent photoresist composition comprises, by weight, 30 parts of acrylic resin, 2 parts of photoinitiator, 20 parts of photocurable monomer, 10 parts of film-forming resin, 10 parts of auxiliary agent and 20 parts of solvent.

[0168] The method for preparing the dry film layer is the same as that in Example 1.

[0169] Comparative Example 3

[0170] A transparent photoresist composition comprises, by weight, 3 parts of acrylic resin, 1.2 parts of photoinitiator, 30 parts of photocurable monomer, 1 part of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0171] The method for preparing the dry film layer is the same as that in Example 1.

[0172] Comparative Example 4

[0173] A transparent photoresist composition comprises, by weight, 30 parts of acrylic resin, 1.2 parts of photoinitiator, 3 parts of photocurable monomer, 10 parts of film-forming resin, 0.5 parts of auxiliary agent and 25 parts of solvent.

[0174] The method for preparing the dry film layer is the same as that in Example 1.

[0175] The above Examples 1 to 12 and Comparative Examples 1 to 4 are mixed and filtered according to the component ratio to form a uniform transparent photoresist composition photosensitive liquid. And the dry film layer is formed according to the above dry film layer preparation method. The components and specific gravity are referred to the following Table 1:

[0176] Table 1 Distribution ratio of each group of samples

[0177]

[0178] In addition, two conventional transparent photoresists were purchased from the market as comparative examples 3 and 4. In order to verify the various properties of the transparent photoresist composition and the dry film layer of the present invention, the above five embodiments and four comparative examples were subjected to physical and chemical property tests and weather resistance tests.

[0179] 1. Physical and chemical properties test

[0180] (1) Viscosity: The above transparent photoresist is measured using a viscometer. 1 mL of transparent photoresist is placed in a rotary viscometer at a constant temperature of 25°C for measurement.

[0181] (2) Specific gravity: Pour more than 100 mL of transparent photoresist into a 100 mL specific gravity cup, weigh it according to the instructions, and calculate the specific gravity.

[0182] (3) Film uniformity: Take 1 ml of transparent photoresist and spin coat it. Then, use a step thickness meter (Japanese ET200A-3D step meter) or a probe film thickness meter to select 9 points, measure the film thickness, and calculate the film uniformity.

[0183] (4) Water absorption rate: Take about 1 gram of transparent photoresist and place it in aluminum foil, weigh it and record the actual weight. Use an oven to bake at 100°C for 2 hours, take it out and weigh it to record the water loss weight, and calculate the weight loss ratio.

[0184] (5) Surface resistivity: Use high resistance meter SM7120 to test according to national standard QJ 2220.2-1992 method.

[0185] (6) tg value: The transfer temperature of the sample was measured by using a DSC thermal analyzer with a temperature program of 100°C to 400°C (10°C / min).

[0186] (7) 100-grid test: Use a 100-grid knife to cut 10×10 (1 mm*1 mm) small grids on the surface, stick the test grid with 3M tape, and quickly tear off the tape at 90° vertically to see if it falls off.

[0187] (8) Film thickness: Take 1 ml of transparent photoresist and spin coat it. Then, measure its film thickness by yellow light process and using a step thickness meter (Japanese ET200A-3D step meter) or a probe film thickness meter. Use a probe film thickness meter to measure the thickness of the dry film layer.

[0188] The results are shown in Table 2.

[0189] Table 2 Physical and chemical properties test results

[0190]

[0191] According to Table 2, the viscosity of the photosensitive liquid of Examples 1 to 12 is about one hundred times that of Comparative Examples 1 and 3 to 4, and its viscosity is much higher than that of the comparative examples; and although the viscosity of Comparative Example 2 is not much different from that of the embodiments, its film formation uniformity and water absorption rate are high, the tg value is low, and the 100-grid test is 4B.

[0192] The surface resistivity of Examples 1 to 12 and Comparative Examples 1 to 4 all passed the test. Overall, the film uniformity, water absorption, tg value and hundred grid test of Examples 1 to 12 all passed the test and met the requirements, indicating that the transparent photoresist composition of the present application has good physical and chemical properties. In addition, the thickness of Examples 1 to 12 is at least 30 μm, while the thickness of Comparative Examples 1, 3 and 4 is only 1.45-1.50 μm, which is small and cannot form a relatively thick dry film layer. In other words, the transparent photoresist composition of the present application can achieve a thick film, and its physical and chemical properties meet the requirements.

[0193] 2. Weathering test

[0194] (1) Acid and alkali resistance: The photosensitive liquid coating was immersed in 2.38% TMAH, propylene glycol methyl ether acetate, and ethanol at room temperature 25°C for 10 minutes.

[0195] (2) High temperature and high humidity test ①: The photosensitive liquid coating was placed in a 65°C / 90% RH constant temperature and humidity test box for 240 hours, and then taken out and allowed to recover to room temperature for 2 hours.

[0196] (3) High temperature and high humidity test ②: The photosensitive liquid coating was placed in a constant temperature and humidity test chamber at 85°C / 85%RH for 240 hours, and then taken out and allowed to recover at room temperature for 2 hours.

[0197] (4) Boiling test: The photosensitive liquid coating is tested in a water bath, placed in a 90°C constant temperature water bath and boiled for 1 hour.

[0198] After the above operations (1) to (4) were completed, a hundred-grid test was performed to observe the shedding. The results are shown in Table 3.

[0199] Table 3 Weathering test results

[0200]

[0201] Remark:

[0202] 5B represents the highest level of adhesion, indicating that the cut edge is completely smooth and there is no peeling at the edge of the grid;

[0203] 4B indicates a high level of adhesion, which means that there is a small flake peeling at the intersection of the cuts, and the total peeling area is less than 5%;

[0204] 3B means that there are small pieces of peeling at the edges and intersections of the cut, and the total peeling area is between 5% and 15%;

[0205] 2B means that there is flaking at the edges and intersections of the cut, and the total flaking area is between 15% and 35%;

[0206] 1B means that there is flaking at the edges and intersections of the cut, and the total flaking area is between 35% and 65%;

[0207] 0B means that there is flaking at the edge and intersection of the cut, and the total flaking area is greater than 65%.

[0208] As can be seen from Table 3, the acid and alkali resistance, high temperature and high humidity test and boiling water test results of Examples 1 to 12 are all 5B, the adhesion level of the dry film layer is high, the cut edge is completely smooth, and there is no peeling at the grid edge, indicating that the embodiments of the present application have passed the weather resistance test. In the weather resistance test, the hundred-grid test results of Comparative Examples 1 to 2 are 0B, which did not pass the weather resistance test; the hundred-grid test results of Comparative Examples 3 to 4 are also 1-4B, and some are even 0B, but their dry film layers are relatively thin, while the dry film layer thickness of the embodiments of the present application is large, and the weather resistance performance effect of a thinner dry film layer is achieved.

[0209] Therefore, the transparent photoresist composition of the present application can withstand the corrosion of 2.38% TMAH, propylene glycol methyl ether acetate, and ethanol when it is formed into a dry film layer, and can withstand the corrosion of 25-200°C metal plating. In an environment of 85°C / 85% high humidity, its surface resistivity is stable at 5.0E×10 16 The film-forming resin of the present application participates in a stereo cross-linking reaction through the double bond of the N-heterocyclic enamine, thereby increasing the thickness of the transparent photoresist composition, so that the dry film layer does not collapse after curing, thereby increasing the thickness of the dry film layer; and the photosensitive liquid is cured at low temperature, solving the problem of low heat resistance temperature limit of quantum dot materials.

[0210] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art, but in case of conflict, the definitions in this specification shall prevail.

[0211] The foregoing examples are merely illustrative and are used to explain some features of the method of the present invention. The appended claims are intended to claim the widest possible range that can be conceived, and the embodiments presented herein are only illustrations of selected implementations according to the combination of all possible embodiments. Therefore, it is the applicant's intention that the appended claims are not limited by the selection of examples that illustrate the features of the present invention. Some numerical ranges used in the claims also include sub-ranges within them, and changes in these ranges should also be interpreted as being covered by the appended claims where possible.

Claims

1. A transparent photoresist composition, characterized in that: The preparation materials of the transparent photoresist composition include acrylic resin, photoinitiator, photocurable monomer, auxiliary agent, solvent and film-forming resin, and the film-forming resin includes enamine (i) with N-heterocyclic ring and olefin chain (ii) with aromatic ring in the side chain.

2. The transparent photoresist composition according to claim 1, characterized in that The structure of the enamine with N-heterocyclic ring is shown in formula (i): In formula (i), R1 and R2 are methyl groups or hydrogen atoms; Z is one of a N-containing aromatic heterocycle or a N-containing aliphatic heterocycle; And / or, the structure of the film-forming resin is as shown in formula (1): In formula (1), n=60-180; R1, R2 and R4 are methyl groups or hydrogen atoms; R3 is H or a C2-C20 alkyl group; Y is an unsaturated aromatic hydrocarbon group or a cyclic hydrocarbon structure; Z is one of a N-containing aromatic heterocycle or a N-containing aliphatic heterocycle; And / or, the structure of the olefin chain containing an aromatic ring in the side chain is as shown in formula (ii): In formula (ii), R4 is a methyl group or a hydrogen atom; R3 is H or a C2-C20 alkyl group; Y is an unsaturated aromatic hydrocarbon group or a cyclic hydrocarbon structure.

3. The transparent photoresist composition according to claim 2, characterized in that The group of Z includes One of; And / or, the group of Y includes one of phenyl, methylphenyl, dimethylphenyl, trimethylphenyl, ethylphenyl, isopropylphenyl, butylphenyl, hydroxyphenyl, methoxyphenyl, acetoxyphenyl, butoxyphenyl, chlorophenyl, bromophenyl, dichlorophenyl, and chloromethylphenyl.

4. The transparent photoresist composition according to any one of claims 1 to 3, characterized in that: The transparent photoresist composition is prepared from the following materials in parts by weight: Acrylic resin 5-40 parts; Photoinitiator 0.5-10 parts; 5-50 parts of photocurable monomer; 5-50 parts of film-forming resin; 0.2-5 parts of additives; Solvent 10-200 parts.

5. The transparent photoresist composition according to claim 4, characterized in that The acrylic resin includes one or more of a copolymer of methacrylic acid and methyl methacrylate, a copolymer of methacrylic acid and cyclohexyl methacrylate, a copolymer of methacrylic acid and glycidoxy methacrylate, a copolymer of methacrylic acid and 2-hydroxyethyl methacrylate, a copolymer of methacrylic acid and cyclohexyl methacrylate, and a copolymer of styrene and 2-hydroxyethyl methacrylate; and / or, the photoinitiator comprises an oxime ester initiator and an imidazole initiator; and / or, the photocurable monomer comprises an oligomer crosslinking agent containing olefinic double bonds; And / or, the auxiliary agent includes one or more of a coupling agent, a leveling agent, a defoaming agent, a UV absorber, and a stabilizer; And / or, the solvent includes one or more of N,N'-dimethylformamide, N-methylpyrrolidone, N-ethyl-2-pyrrolidone, N,N'-dimethylacetamide, diethylene glycol dimethyl ether, cyclopentanone, γ-butyrolactone, α-acetyl-γ-butyrolactone, tetramethyl urea, 1,3-dimethyl-2-imidazoline, N-cyclohexyl-2-pyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, pyridine, γ-butyrolactone, propylene glycol monomethyl ether acetate, and diethylene glycol monomethyl ether.

6. The transparent photoresist composition according to claim 5, characterized in that The average acid value of the acrylic resin is 75-140 mgKOH / g; and / or, The usage ratio of the oxime ester initiator to the imidazole initiator is 1:1-1:3; and / or, The ratio of the photoinitiator to the photocurable monomer is 1:6-1:100; The photocurable monomer includes one or more of pentaerythritol triacrylate, pentaerythritol tetraacrylate, 3-hydroxymethyl pentaerythritol triacrylate, 3-hydroxyethyl pentaerythritol triacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate.

7. A method for preparing a transparent photoresist composition, for preparing the transparent photoresist composition according to any one of claims 1 to 6, characterized in that: The N-heterocyclic intermediate as claimed in claim 3 is used to prepare the N-heterocyclic enamine through the Stork synthesis reaction.

8. The method for preparing the transparent photoresist composition according to claim 7, characterized in that: The film-forming resin is prepared by copolymerizing a free radical solution of an enamine group (i) with an N-heterocyclic ring and a free radical solution of an olefin chain (ii) with an aromatic ring in the side chain.

9. A pixel device, characterized in that: It comprises a substrate and a dry film layer disposed on the substrate, wherein the dry film layer is formed by curing the transparent photoresist composition according to any one of claims 1 to 6; Wherein, the substrate is a glass substrate, a Si substrate, a PET substrate, a CPI substrate, a COP substrate or a PEN substrate; the transparent photoresist composition is cured by spin coating, pre-baking, exposure, mid-baking, development, post-UV and post-baking processes to form the dry film layer.

10. A semiconductor device, characterized in that: A substrate pixel device comprising a micro-light emitting diode (Micro-LED) display and / or a radio frequency chip, wherein the substrate pixel device comprises the pixel device as claimed in claim 9, wherein the pixel device comprises a micro-light emitting diode display having an upper layer, a lower layer, or an upper and lower layer structure containing the dry film layer, wherein the dry film layer is prepared using a black photoresist composition; Among them, a black photoresist composition comprises, by weight, 2 to 20 parts of bisphenol fluorene acrylic resin, 1 to 10 parts of tertiary amine resin containing β-H atoms, 0.1 to 2 parts of perfluorinated substituted ethylene monomer auxiliary A, 0.2 to 5 parts of aromatic peroxide auxiliary B, 0.5 to 2 parts of photoinitiator, 5 to 10 parts of photocurable resin monomer, 10 to 50 parts of black colorant and 50 to 500 parts of polar organic solvent.

11. A module device, characterized in that: The module device includes a vehicle-mounted display screen, a wearable device display screen or a chip packaging device, and the vehicle-mounted display screen, the wearable device display screen or the chip packaging device includes the semiconductor device as described in claim 10.

Citation Information

Cited By

  • Transparent photoresist composition and preparation method therefor, pixel device, semiconductor device, and module device

    WO2026001655A1