XBC battery slurry based on Cu alloy and preparation method thereof

By using a combined slurry of Cu alloy and Ag powder in the xBC battery, the contact resistance and body resistance of the electrode are solved, the manufacturing cost is reduced and the conductivity of the electrode is improved, and the efficient power generation efficiency of the xBC battery is achieved.

CN119092178AInactive Publication Date: 2024-12-06JIANGSU RIYU PHOTOVOLTAIC NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411237996.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The ohmic contact effect of the electrode in the P region of the xBC battery is poor, the contact resistance and body resistance are large, and the manufacturing cost and electrode performance are difficult to take into account, especially due to the difficulty in corrosion of the Al2O3+SiNx passivation film and the influence of Al's conductivity, the electrodes are caused by the influence of the corrosion of the Al2O3+SiNx passivation film, which leads to the influence of the electrodes. The application effect in xBC batteries is not ideal.

Method used

Using the xBC cell slurry based on Cu alloy, the conductive phase and carrier are formed through the combination of Cu alloy powder, Ag powder, glass phase and auxiliary materials. The multi-morphology of Cu alloy powder and the different particle size distribution of Ag powder are used to reduce the slurry. The melting point of the material is avoided and the formation of metal oxide film is improved, thereby improving the conductivity.

Benefits of technology

The amount of Ag is significantly reduced, the manufacturing cost of electrode slurry is controlled, the conductivity of the electrode is improved, the formation of oxide films of Cu and Al is avoided, and the sintering effect and electrical performance of the electrode are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005028308910000061
    Figure BDA0005028308910000061
Patent Text Reader

Abstract

The invention relates to xBC battery slurry based on a Cu alloy. The xBC battery slurry comprises 85-90 wt% of a conductive phase; based on the total mass of the conductive phase, the conductive phase comprises 5-45wt% of Cu alloy powder and 55-95wt% of Ag powder; 3 to 6 wt% of a glass phase; 0.5 to 3 wt% of an auxiliary material; and the balance is a carrier. The invention also relates to a preparation method of the slurry, which comprises the following steps: S1, putting the solvent into a heating container, keeping the temperature at 50 DEG C, slowly adding the resin and stirring to form the organic carrier; s2, adding an auxiliary agent into the organic carrier, keeping the temperature at 50 DEG C, continuously stirring so that the auxiliary agent and the organic solvent are fully and uniformly mixed to form an auxiliary material, and then standing at room temperature for more than 12 hours for later use; s3, adding a glass phase and Ag powder into the auxiliary material, and stirring and dispersing; s4, Cu alloy powder is added into the auxiliary materials, stirring and dispersing are continued, and paste is obtained; and S5, uniformly dispersing the paste obtained in the step S4 to obtain the slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic cells and conductive pastes, and in particular to a Cu alloy-based xBC cell paste and a preparation method thereof. Background Art

[0002] BC is the abbreviation of Back Contact, which means back-contact photovoltaic cells; there are many types of BC cells, such as PBC, IBC, HBC, etc., collectively referred to as xBC cells. Compared with existing TOPCon cells, HJT cells, etc., the biggest feature of xBC is that there is no grid line on the front, and the back is no longer a simple N area or P area, but usually a staggered P and N areas are prepared on the back of the battery, so that the positive and negative electrodes are integrated on the back of the battery. Thanks to this structure, there will be no electrode grid lines blocking the front of the xBC battery, which not only improves the power generation efficiency but also improves the aesthetics of the front. Because BC cells adopt a design without metal grid lines on the front, the power generation per watt is usually about 2% to 3% higher than that of TOPCon cells.

[0003] At present, the problem faced by the P-region electrode of xBC battery is that the ohmic contact effect is not good, the contact resistance and body resistance are both large, and it is difficult to balance the manufacturing cost and electrode performance; in addition, since N-type silicon wafers have a higher body life, they can ensure that the non-equilibrium carriers can smoothly reach the back pn junction area before recombination. Therefore, most BC batteries currently use N-type silicon wafers as substrates, and the Al2O3+SiN x The passivation film is difficult to corrode and the "window opening" effect is poor. In addition, in order to control the cost of slurry preparation, more Al and Ag are often co-doped. Although Al has good conductivity, the Al in the electrode is prone to produce Al2O3 oxide film and the finer Al powder is easy to agglomerate and difficult to disperse in the slurry system, which further affects the effect of ohmic contact. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a Cu alloy-based xBC battery slurry and a preparation method thereof, which better balances the manufacturing cost and comprehensive performance of the xBC battery. The technical solution of the present invention is as follows:

[0005] In a first aspect, the present invention provides a Cu alloy-based xBC battery slurry comprising:

[0006] 85-90wt% of a conductive phase; based on the total mass of the conductive phase, it includes 5-45wt% of Cu alloy powder and 55-95wt% of Ag powder;

[0007] 3-6 wt% glass phase;

[0008] 0.5-3wt% auxiliary materials;

[0009] The remainder is carrier.

[0010] In one possible implementation,

[0011] The Cu alloy powder is at least one of Cu-Ti, Cu-Ag and Cu-Al powder.

[0012] In the above possible implementation, further,

[0013] The Cu alloy powder is a mixture of micron-sized spherical Cu alloy powder, micron-sized flaky Cu alloy powder and nano-sized spherical Cu alloy powder;

[0014] The D50 particle size of the micron-sized spherical Cu alloy powder and the micron-sized flaky Cu alloy powder is 1.0 to 2.5 μm, and the D50 particle size of the nano-sized spherical Cu alloy powder is 500 to 800 nm.

[0015] Based on the total mass of the Cu alloy powder, the mass proportion of the nano-scale spherical Cu alloy powder does not exceed 5-10wt%.

[0016] Further,

[0017] Based on the total mass of the Cu alloy powder, the mass of the micron-sized flaky Cu alloy powder does not exceed 20-30wt%.

[0018] Further,

[0019] The Ag powder comprises 65-70 wt% of micron-grade spherical Ag powder, 25-30 wt% of micron-grade flake Ag powder and 2-5% of nanometer-grade spherical Ag powder.

[0020] In a possible implementation, the glass phase includes a first glass powder and a second glass powder, and based on the total mass of the glass phase:

[0021] The first glass powder comprises 35-60 wt % of Bi2O3, 25-40 wt % of B2O3, and 5-20 wt % of SiO2;

[0022] The mass percentage of the second glass powder is 8-12wt%; the second glass powder is a mixture of at least two of BaO, ZnO, GaO, K2O, and Na2O.

[0023] In a possible implementation, the auxiliary material is a mixture of WO3, metal fluoride and boron powder; based on the total mass of the auxiliary material:

[0024] The content of WO3 is 30-50wt%;

[0025] The metal fluoride content is 10-15wt%;

[0026] The content of the boron powder is 30-45wt%; the D50 particle size of the boron powder is 1-2.5 μm.

[0027] In one possible implementation,

[0028] The carrier includes a mixed solvent and a resin;

[0029] The mixed solvent is a mixture of terpineol and butyl carbitol and / or citric acid, and the mass proportion of the terpineol is ≥60%;

[0030] Based on the total weight of the carrier, the resin comprises 5-8wt% of ethyl cellulose, 0-5wt% of Span series and / or Tween series, 1.5-2.5wt% of sodium dodecylbenzene sulfonate, and 0.2-0.8wt% of polyamide.

[0031] In a second aspect, the present invention provides a method for preparing the above slurry, comprising the following steps:

[0032] S1. Place terpineol in a heating container, maintain the temperature at 45° C., slowly add butyl carbitol and / or citric acid and keep stirring, stir at a stirring speed of 15 rpm for 3 to 5 minutes, so that butyl carbitol and / or citric acid are fully mixed in terpineol to obtain a mixed solvent;

[0033] S2, mixing the various components of the resin evenly, keeping the mixed solvent at 45°C, adding the mixed resin to the mixed solvent, keeping the temperature at 50°C after the resin is completely added, and stirring continuously for 2.5 to 3 hours to make the resin and the mixed solvent fully mixed to form a liquid carrier with a uniform and stable texture, and cooling to room temperature for standby use;

[0034] S3, adding the glass phase and Ag powder into the carrier, stirring and dispersing at a speed of 20 to 30 rpm;

[0035] S4, stirring at a speed of 20 to 30 rpm, mixing the auxiliary materials and the Cu alloy powder evenly, and then adding them to the carrier, stirring continuously for 8 to 12 hours to obtain a paste;

[0036] S5. Disperse the paste obtained in S4 7 to 8 times, each time for 10 to 20 minutes, to obtain the slurry.

[0037] The above technical solution provided by this application has at least the following technical effects or advantages:

[0038] The xBC battery P-zone slurry disclosed in the present invention uses Cu alloy powder and Ag powder as the main body of the conductive phase. First, the amount of Ag used is reduced, thereby significantly controlling the manufacturing cost of the electrode slurry; second, Cu and other conductive base metals are distributed in the slurry system in the form of alloys, which, on the one hand, significantly reduces the melting point of the slurry and makes it easier to carry out the metallization process, and on the other hand, it is well avoided that metals such as Cu and Al produce oxide films during sintering and use, thereby affecting the conductive performance. DETAILED DESCRIPTION

[0039] The specific implementation modes of the present invention are described below by way of examples.

[0040] Example 1

[0041] This embodiment provides an xBC battery slurry, including:

[0042] 85wt% of a conductive phase; based on the total mass of the conductive phase, it includes 5wt% of Cu alloy powder and 95wt% of Ag powder;

[0043] 3wt% glass phase;

[0044] 1wt% of auxiliary materials;

[0045] The remainder is carrier.

[0046] Based on the total mass of the Cu alloy powder, it comprises:

[0047] 80wt% Cu-Al, 15wt% Cu-Ti, 5wt% Cu-Ag;

[0048] Cu alloy powder is composed of alloy powders of different morphologies, including:

[0049] 70wt% of micron-sized spherical Cu alloy powder, 20wt% of micron-sized flaky Cu alloy powder and 10wt% of nano-sized spherical Cu alloy powder.

[0050] Based on the total mass of the Ag powder, the Ag powder includes 65wt% of micron-sized spherical Ag powder, 30wt% of micron-sized flaky Ag powder and 5% of nanometer-sized spherical Ag powder.

[0051] The glass phase includes a first glass powder and a second glass powder, and according to the total mass of the glass phase:

[0052] The first glass powder comprises 35wt% Bi2O3, 35wt% B2O3, and 20wt% SiO2;

[0053] The mass percentage of the second glass powder is 10wt%; the second glass powder is a mixture of BaO, ZnO, GaO, K2O, and Na2O.

[0054] The auxiliary materials include: 40wt% WO 3, 15wt% of metal fluoride and 45wt% of boron powder; the metal fluoride may be CaF2, AlF3, NaF, etc., and the D50 particle size of the boron powder is 1-2.5μm.

[0055] The carrier includes a mixed solvent and a resin;

[0056] The mixed solvent is a mixture of terpineol, butyl carbitol and citric acid, and the mass proportion of terpineol is 70wt% based on the total mass of the mixed solvent;

[0057] Based on the total mass of the carrier, the resin includes 5wt% of ethyl cellulose, 5wt% of Span series and / or Tween series, 1.5wt% of sodium dodecylbenzene sulfonate, and 0.5wt% of polyamide.

[0058] Example 2

[0059] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of Embodiment 1, except that:

[0060] The conductive phase includes 45 wt % of Cu alloy powder and 55 wt % of Ag powder.

[0061] Example 3

[0062] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of Embodiment 1, except that:

[0063] The conductive phase includes 25 wt % of Cu alloy powder and 75 wt % of Ag powder.

[0064] Example 4

[0065] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of embodiment 3, except that:

[0066] Based on the total mass of the Cu alloy powder, it comprises:

[0067] 50wt% Cu-Al, 40wt% Cu-Ti, 10wt% Cu-Ag.

[0068] Example 5

[0069] This embodiment provides an xBC battery slurry, the components of which are substantially the same as those of embodiment 3, except that:

[0070] Based on the total mass of the Cu alloy powder, it comprises:

[0071] 50wt% Cu-Al, 10wt% Cu-Ti, 40wt% Cu-Ag.

[0072] The preparation methods of the slurries of Examples 1 to 5 are basically the same, and all include the following steps:

[0073] S1. Place terpineol in a heating container, maintain the temperature at 45°C, slowly add butyl carbitol and citric acid and keep stirring, stir at a stirring speed of 15 rpm for 5 minutes to fully mix butyl carbitol and citric acid in terpineol to obtain a mixed solvent;

[0074] S2, mixing the various components of the resin evenly, keeping the mixed solvent at 45°C, adding the mixed resin to the mixed solvent, keeping the temperature at 50°C after the resin is completely added, and stirring for 3 hours to make the resin and the mixed solvent fully mixed to form a liquid carrier with a uniform and stable texture, and cooling to room temperature for standby use;

[0075] S3, adding the glass phase and Ag powder into the carrier, stirring and dispersing at a speed of 20 to 30 rpm;

[0076] S4, stirring at a speed of 20 to 30 rpm, mixing the auxiliary materials and the Cu alloy powder evenly, and then adding them to the carrier, stirring continuously for 10 hours to obtain a paste;

[0077] S5. Disperse the paste obtained in S4 8 times, each time for 10 to 20 minutes, to obtain the slurry.

[0078] Next, the slurries provided in Examples 1 to 5 are tested to illustrate the beneficial effects of the embodiments of the present application.

[0079] This experiment provides control groups 1 to 5. The slurry components and preparation methods of control groups 1 to 5 are basically the same as those of Example 1, except that:

[0080] Control group 1, whose conductive phase composition is 95wt% Ag powder and 5wt% Cu powder;

[0081] Control group 2, whose conductive phase composition is 75wt% Ag powder and 25wt% Cu powder;

[0082] Control group 3, whose conductive phase composition is 55wt% Al powder and 45wt% Cu powder;

[0083] Control group 4, whose conductive phase composition is 75wt% Ag powder and 25wt% Ti powder;

[0084] Control group 5, the conductive phase composition is 75wt% Ag powder and 25wt% Al powder.

[0085] Using screen printing technology, the slurries of Examples 1 to 5 and the slurries of Control Groups 1 to 5 were printed on silicon wafer substrates to form cells, which were dried in an infrared drying furnace, and then sintered at 740 to 800°C in a belt sintering furnace, and cooled after sintering to form silicon crystalline solar cells. After screen printing and sintering, the cross-sections of the metal grid lines of Examples 1 to 5 were close to Gaussian distribution. The line width was controlled at about 25 μm and the line height was about 5 μm.

[0086] For the prepared batteries, Examples 1 to 5 are designated as S1 to 5, and Control Groups 1 to 5 are designated as D1 to 5, and the contact resistance and line resistance are tested using a TLM contact resistance meter. The test results are shown in Table 1 below:

[0087] Table 1 - Electrical performance test of Examples 1 to 4 and Control Groups 1 to 6

[0088]

[0089]

[0090] From Table 1 we can see that:

[0091] After sintering into electrodes, the slurries provided by S1~S5 basically have relatively ideal line resistance and contact resistance performance. Among them, the electrical performance of S2~S5 is slightly weaker than that of S1. It has been verified that this is because S1 has the highest Ag content, so its conductive performance is the best;

[0092] By observing the appearance and cross-sectional micromorphology of the finished electrodes of S1 to S5, it is found that S1 to S5 all have relatively ideal microstructures after sintering. This is because the base metals such as Al, Cu, and Ti are introduced in the form of alloys rather than in the form of single metals, which greatly reduces the melting point of the system and avoids the situation where high-melting-point metals such as Cu and Ti directly enter the system and cannot be fully melted and sintered.

[0093] The comprehensive performance of S2 is poorer than that of other embodiments. This is because the Ag content in the system is too low and the Cu alloy content is too high. The alloy will cause metal lattice distortion during the formation process, which will have a certain impact on the movement of electrons, and ultimately affect the electrical performance. However, since the alloy elements used in S2 are all metals with strong conductivity, the impact of lattice distortion is still within the controllable range.

[0094] In S3 to S5, as the content of Cu-Al and Cu-Ag changes, the electrical properties also change synchronously. Overall, it can be seen that when the Cu-Ag content increases, the conductive properties of the slurry will be optimized to a certain extent.

[0095] Among D1 to D5, the overall electrical performance of D1 is relatively excellent. This is because Ag accounts for the vast majority of the slurry mass ratio. However, too high an Ag content will greatly increase the electrode cost, which is not conducive to cost reduction and efficiency improvement.

[0096] The electrical performance of D2~4 is much worse than that of S1~S5, and even compared with D1. It has been verified that the problem is that the Cu or Ti content in D2~4 is too high. The melting point of Cu is 1084.6℃, and the melting point of Ti is 1668℃. It is difficult to fully sinter at a sintering temperature of 740~800℃. Observation of the microscopic morphology shows that a large part of the Cu powder or Ti powder in the electrode is basically not tightly connected with other components, which leads to abnormally high line resistance and contact resistance, which cannot meet the normal use requirements of xBC electrodes.

[0097] The electrical performance of D5 is better than that of D2~4, but the contact resistance is higher. It has been verified that this is because the Al content in the slurry system is too high, which leads to the appearance of an oxide film on the surface of the grid motor after sintering, seriously affecting the contact resistance performance.

[0098] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0099] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A Cu alloy-based xBC battery slurry, characterized in that: include: 85-90 wt% conductive phase; Based on the total mass of the conductive phase, it includes 5-45wt% Cu alloy powder and 55-95wt% Ag powder; 3-6 wt% glass phase; 0.5-3wt% auxiliary materials; The remainder is carrier.

2. The Cu alloy-based xBC battery slurry according to claim 1, characterized in that: The Cu alloy powder is at least one of Cu-Ti, Cu-Ag and Cu-Al powder.

3. The Cu alloy-based xBC battery slurry according to claim 2, characterized in that: The Cu alloy powder is a mixture of micron-sized spherical Cu alloy powder, micron-sized flaky Cu alloy powder and nano-sized spherical Cu alloy powder; The D50 particle size of the micron-sized spherical Cu alloy powder and the micron-sized flaky Cu alloy powder is 1.0 to 2.5 μm, and the D50 particle size of the nano-sized spherical Cu alloy powder is 500 to 800 nm. Based on the total mass of the Cu alloy powder, the mass proportion of the nano-scale spherical Cu alloy powder does not exceed 5-10wt%.

4. The Cu alloy-based xBC battery slurry according to claim 3, characterized in that: Based on the total mass of the Cu alloy powder, the mass of the micron-sized flaky Cu alloy powder does not exceed 20-30wt%.

5. The Cu alloy-based xBC battery slurry according to claim 1, characterized in that: The Ag powder comprises 65-70 wt% of micron-grade spherical Ag powder, 25-30 wt% of micron-grade flake Ag powder and 2-5% of nanometer-grade spherical Ag powder.

6. The Cu alloy-based xBC battery slurry according to claim 1, characterized in that: The glass phase includes a first glass powder and a second glass powder, and according to the total mass of the glass phase: The first glass powder comprises 35-60 wt % of Bi2O3, 25-40 wt % of B2O3, and 5-20 wt % of SiO2; The mass percentage of the second glass powder is 8-12wt%; the second glass powder is a mixture of at least two of BaO, ZnO, GaO, K2O, and Na2O.

7. The Cu alloy-based xBC battery slurry according to claim 1, characterized in that: The auxiliary material is a mixture of WO3, metal fluoride and boron powder; based on the total mass of the auxiliary material: The content of WO3 is 30-50wt%; The metal fluoride content is 10-15wt%; The content of the boron powder is 30-45wt%; the D50 particle size of the boron powder is 1-2.5 μm.

8. The Cu alloy-based xBC battery slurry according to claim 1, characterized in that: The carrier includes a mixed solvent and a resin; The mixed solvent is a mixture of terpineol and butyl carbitol and / or citric acid, and the mass proportion of the terpineol is ≥60%; Based on the total weight of the carrier, the resin comprises 5-8wt% of ethyl cellulose, 0-5wt% of Span series and / or Tween series, 1.5-2.5wt% of sodium dodecylbenzene sulfonate, and 0.2-0.8wt% of polyamide.

9. The method for preparing the slurry according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Place terpineol in a heating container, maintain the temperature at 45° C., slowly add butyl carbitol and / or citric acid and keep stirring, stir at a stirring speed of 15 rpm for 3 to 5 minutes, so that butyl carbitol and / or citric acid are fully mixed in terpineol to obtain a mixed solvent; S2, mixing the various components of the resin evenly, keeping the mixed solvent at 45°C, adding the mixed resin to the mixed solvent, keeping the temperature at 50°C after the resin is completely added, and stirring continuously for 2.5 to 3 hours to make the resin and the mixed solvent fully mixed to form a liquid carrier with a uniform and stable texture, and cooling to room temperature for standby use; S3, adding the glass phase and Ag powder into the carrier, stirring and dispersing at a speed of 20 to 30 rpm; S4, stirring at a speed of 20 to 30 rpm, mixing the auxiliary materials and the Cu alloy powder evenly, and then adding them to the carrier, stirring continuously for 8 to 12 hours to obtain a paste; S5. Disperse the paste obtained in S4 7 to 8 times, each time for 10 to 20 minutes, to obtain the slurry.

Citation Information

Patent Citations

  • Main grid slurry containing silver-copper alloy powder and preparation method thereof

    CN114709003A

  • Low-temperature slurry for heterojunction photovoltaic cell and preparation method of low-temperature slurry

    CN115762850A

  • Method for metalizing TOPCon solar cell by using silver-coated copper paste and solar cell

    CN117650184A

  • P-region conductive paste for xBC battery, preparation method, electrode and battery

    CN118197676A

  • Copper alloy powder for conductive paste

    JP2001131655A