Regeneration preparation method of ferrite anisotropic magnetic shoe grinding material

Through the regeneration and preparation method of ferrite heterogeneous magnetic tile grinding material, the magnetic properties of the grinding material are restored by using the ball milling and water reduction process, the problems of grinding material resources are solved and environmental pollution are achieved, and environmental protection and economic benefits are achieved. Improvement.

CN119092284APending Publication Date: 2024-12-06GUIZHOU FARADAY MAGNETOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311491636.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing permanent magnet ferrite material production process, the attenuation magnetic properties and environmental pollution of the grinding materials lead to waste of resources and increased environmental protection pressure.

Method used

Through a ferrite heterogeneous magnetic tile grinding material regeneration and preparation method, including grinding material impurity treatment, ball milling, ball grinding slurry water reduction, slurry filtration, drying and crushing sieving and bagging process, calcium carbonate is appropriately added , silicon oxide, alumina and other ingredients, ball milling time and flocculant are used to restore the magnetic properties of the grinding material.

Benefits of technology

It realizes the recovery of magnetic properties of attenuation in grinding materials, reduces production costs, meets environmental protection requirements, increases economic benefits and employment opportunities, and achieves clean production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092284A_ABST
    Figure CN119092284A_ABST
Patent Text Reader

Abstract

The invention relates to a ferrite anisotropic magnetic shoe grinding material regeneration preparation method, which comprises the following steps: grinding material impurity treatment, ball milling, ball milling slurry water reducing, slurry filter pressing, drying, crushing, screening and bagging, grinding material putting into a ball mill, and adding ingredients, calcium carbonate, silicon oxide, alumina, boric acid, ammonium bicarbonate and steel balls with the particle size of phi 0.8 cm; and then ball milling is started, the ball milling time is 6-8 hours, and the average particle size of the slurry obtained after ball milling is 0.8-1.0 micron. A ferrite anisotropic magnetic shoe grinding material is a byproduct generated in a product production process, is generally treated as a waste material, and affects the environment. Clean production is achieved, the environment-friendly requirement is met, employment is increased, and social benefits are good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sintered ferrite magnetic materials, in particular to a method for regenerating and preparing ferrite anisotropic magnetic tile grinding materials. Background Art

[0002] Permanent ferrite material is one of the important supporting materials that are indispensable for the development of high technology and national economy. It plays a huge role in promoting national defense construction and the development of the entire national economy. It is a national encouraged project and supports its priority development. With the continuous improvement of product miniaturization, lightness, thinness, environmental protection and energy saving requirements, higher requirements are put forward for the performance and environmental protection indicators of permanent ferrite products. Exploring and developing high-performance permanent ferrite materials and their preparation technologies, and developing new clean and environmentally friendly ferrite waste recycling processes have important innovative significance for improving the structural composition of current high-end products, and have always been one of the focuses in the field of magnetic material research.

[0003] Permanent ferrite anisotropic products are mostly made of ferric oxide Fe2O3 red magnetic powder or iron phosphorus magnetic powder as raw materials, with binders added, and are manufactured through processes such as powder making, pressing, sintering and grinding. Among them, grinding materials generated by grinding account for 12%-15%, which are usually treated as waste or industrial waste, causing waste and environmental pollution. Summary of the invention

[0004] Experiments under existing production process conditions show that the performance regeneration of ferrite grinding materials does not require the addition of barium carbonate and strontium carbonate, but the appropriate addition of calcium carbonate, silicon oxide, aluminum oxide and other formula materials can improve the performance of grinding material regeneration. At the same time, it is necessary to analyze the main factors affecting the activity of ferrite grinding materials: the surface morphology of the particles, i.e., the particles and their distribution, the shape of the particles, the structure of the raw materials, and the sintering temperature. The present invention provides a method for regenerating and preparing ferrite anisotropic magnetic tile grinding materials, which can restore the attenuated magnetic properties in the grinding materials and has low production costs.

[0005] The objective of the present invention is achieved through the following technical solutions: A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material comprises the following steps: step A of treating grinding material impurities, step B of ball milling, step C of reducing water in ball milled slurry, step D of slurry filter pressing, step E of drying, and step F of crushing, screening and bagging. In the step B of ball milling, the grinding material treated in step A is put into a ball mill, and ingredients are added in the following weight ratios: 0.8% to 1.0% calcium carbonate, 0.12% to 0.15% silicon oxide, 0.4% to 0.6% aluminum oxide, 0.012% to 0.015% boric acid, 0.012% to 0.015% ammonium bicarbonate, and 1.5% to 1.7% steel balls with a particle size of 0.8 cm; then ball milling is started, the ball milling time is 6 to 8 hours, and the average particle size of the slurry after ball milling is 0.8um to 1.0um.

[0006] In the step C of ball milling slurry water reduction process, the slurry treated in the step B is pumped into an aggregate tower, a flocculant is added, and the flocculant is polyacrylamide, and the added amount is 0.01% to 0.02% by weight; the agitator of the aggregate tower is turned on and operated for 10 to 15 minutes, and the sedimentation is performed for 2 to 3 hours, and then the clear water is discharged, and the water reduction rate reaches 55% to 62%.

[0007] In the slurry filtration process of step D, the discharge port of the aggregate tower is connected to the inlet of the automatic filter press, and a 2KW / 1.5-inch pipeline pump is connected in the middle; 150-200 mesh nylon mesh is used between the plates and frames of the automatic filter press; the hydraulic switch of the filter press is turned on, the valve of the aggregate tower is opened, and the pipeline pump is turned on to automatically feed the filter press, the feeding pressure is set to 10Mpa, the pressure holding time is 10 minutes, and then the pressure reducing valve of the filter press is opened to discharge the material, and the powder discharged from the filter press is block-shaped, and the moisture content of the block-shaped powder is less than 15%.

[0008] In the step E, the bulk powder treated in step D is changed into a 5-8 cm block and loaded into a bowl. 8 mm holes are drilled around the bowl and the bottom. The density of the holes is 4 / 10 cm. 2 ; Then put the bowl into the multi-layer drying rack and dry it in the drying room; the main engine of the drying room adopts an air energy frequency conversion system with a total power of 18kw and a temperature setting of 75℃. The moisture is discharged through the pipe and the hot air circulates in the drying room; the continuous drying time is 10 to 15 hours, and the moisture content of the powder is less than 0.55% when it leaves the drying room.

[0009] The beneficial effects of the present invention are as follows: ferrite anisotropic magnetic tile grinding material is a by-product produced in the production process, and is generally treated as waste material, which affects the environment. Through the ferrite anisotropic magnetic tile grinding material regeneration preparation method of the present invention, the attenuated magnetic properties in the grinding material can be restored, and the performance of the regenerated powder material reaches: Br3.54kGs, Hcb2.817kOe, Hcj3.816, BHm2.872MGOe. The present invention realizes clean production, meets environmental protection requirements, increases employment, and has good social benefits. Taking an enterprise with an annual output of 10,000 tons of ferrite anisotropic magnetic tiles as an example, 1,500 tons of grinding waste can be generated. By adopting the method for regenerating and preparing ferrite anisotropic magnetic tile grinding materials of the present invention, the total cost incurred in the whole process is calculated to be 950 yuan / ton, and the benefit of recycling is 5,000 yuan / ton. If the sales income of waste materials is 2,000 yuan / ton, the direct income is 2,050 yuan / ton. Based on an annual output of 1,500 tons, the economic benefit is more than 3 million yuan, which directly increases the product profit margin by 2.5%, and has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 : Demagnetization curve of the regenerated powder produced by the present invention. DETAILED DESCRIPTION Example

[0011] A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material comprises the following steps: Step A: The grinding material is passed through a multi-stage water fluid to remove the diamond sand and other impurities produced by the grinding wheel consumption during the production of the grinding bed, and the qualified grinding material is obtained as a recycled raw material.

[0012] Step B, the high performance of the recycled material is obtained by optimizing the formula and ball milling process. The weight ratio of the formula material is: 0.8% calcium carbonate, 0.12% silicon oxide, 0.4% aluminum oxide, 0.012% boric acid, 0.012% ammonium bicarbonate, 1.5% Ф0.8cm steel ball; the ball milling time is 6 hours; the average particle size of the recycled powder reaches 0.8um.

[0013] Step C, reducing the water of the ball-milled slurry, adding a flocculant, the flocculant is polyacrylamide, the addition amount is 0.01%; starting the aggregate tower agitator to run for 10 minutes, settling for 2 hours, and then releasing the clear water, the water reduction rate is 55%.

[0014] Step D, slurry filtration, select a plate and frame automatic filter press, hard connect the discharge port of the aggregate tower with the inlet of the automatic filter press, and connect a 2KW / 1.5-inch pipeline pump in the middle; 150-200 mesh nylon mesh is used to protect the plate and frame of the automatic filter press to prevent slurry leakage; then turn on the hydraulic switch of the filter press, open the aggregate tower valve, turn on the pipeline pump, and automatically feed the filter press. The automatic feeding pressure to the filter press is set to 10Mpa, and the pressure holding time is 10 minutes. Then, the filter press pressure reducing valve is opened to discharge the material. The powder discharged from the filter press is block-shaped, and the water content of the block powder is less than 15%.

[0015] Step E, drying in a bowl, wherein the block powder discharged from the filter press is changed into a block of 5-8 cm and placed in an iron box; the iron box is made of a steel plate with a thickness of 1.5 mm, a length of 40 cm, a width of 25 cm, and a height of 10 cm, with Ø8 mm holes drilled on the four sides and the bottom, and a density of 4 holes / 10 cm 2 , the weight of the bowls is 10~12kg / box; then the bowls are loaded into the multi-layer drying racks, and the drying is to push the drying racks with the bowls into the drying room for drying; the function of the drying room is: the main machine adopts an air energy frequency conversion system, the total power is 18kw, the temperature is set to 75℃, the moisture is discharged through the pipe, and the hot air circulates in the drying room; 2 racks / 2 tons are loaded in the drying room at a time, the continuous drying time is: 10-15 hours, and the moisture content of the powder is detected to be less than 0.6% out of the drying room.

[0016] The filling process is to change the block powder released by the filter press into 5~8cm blocks and put them into iron boxes, and then install multi-layer drying racks with a height of 20cm.

[0017] Step F, crushing, screening and bagging, the powder coming out of the drying room is crushed by a crusher, and impurities are removed by vibration screening to obtain qualified recycled powder, which is quantitatively bagged for secondary use.

[0018] Figure 1 The demagnetization curve of the recycled powder produced by this embodiment shows that its magnetic properties reach: Br3.54kGs, Hcb2.817kOe, Hcj3.816, BHm2.872MGOe. The four magnetic property indicators are high, and the moisture content and average particle size meet the national standards. Example

[0019] A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material comprises the following steps: Step B, the high performance of the recycled material is obtained by optimizing the formulation and ball milling process. The weight ratio of the formulated material is: calcium carbonate 0.9%, silicon oxide 0.13%, aluminum oxide 0.5%, boric acid 0.014%, ammonium bicarbonate 0.013%, Ф0.8 cm steel ball 1.6%; then ball milling is started, the ball milling time is 7 hours, and the average particle size of the powder is 0.9 um.

[0020] Step C, ball-milled slurry is water-reduced, and a flocculant is added, wherein the flocculant is polyacrylamide, and the addition amount is 0.02%; the aggregate tower agitator is turned on and operated for 12 minutes, and the sedimentation is performed for 2.5 hours, and then the clear water is discharged, and the water reduction rate reaches 58%.

[0021] The remaining steps are the same as implementation 1.

[0022] The performance of recycled powder reaches: Br3.55kGs, Hcb2.82kOe, Hcj3.852, BHm2.84MGOe. The four magnetic performance indicators are high, and the moisture content and average particle size meet the national standards. Example

[0023] A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material comprises the following steps: Step B, the high performance of the recycled material is obtained by optimizing the formulation and ball milling process. The weight ratio of the formulated material is: calcium carbonate 1.0%, silicon oxide 0.15%, aluminum oxide 0.6%, boric acid 0.015%, ammonium bicarbonate 0.015%, Ф0.8cm steel ball 1.7%; then ball milling is started, the ball milling time is 8 hours, and the average particle size of the powder is 1.0um.

[0024] Step C, ball-milled slurry is water-reduced, and a flocculant is added, wherein the flocculant is polyacrylamide, and the addition amount is 0.02%; the aggregate tower agitator is turned on and operated for 15 minutes, and the sedimentation is performed for 3 hours, and then the clear water is discharged, and the water reduction rate reaches 62%.

[0025] The remaining steps are the same as implementation 1.

[0026] The performance of recycled powder reaches: Br3.55kGs, Hcb2.814kOe, Hcj3.82, BHm2.856MGOe. The four magnetic performance indicators are high, and the moisture content and average particle size meet the national standards. Example

[0027] A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material comprises the following steps: Step A: The grinding material is passed through a multi-stage water fluid to remove the diamond sand and other impurities produced by the grinding wheel consumption during the production of the grinding bed, and the qualified grinding material is obtained as a recycled raw material.

[0028] Step B: ball milling process, the grinding material treated in step A is put into a ball mill, and ingredients are added in a weight ratio of: 1.2% calcium carbonate, 0.16% silicon oxide, 0.9% aluminum oxide, 0.018% boric acid, 0.018% ammonium bicarbonate, and 1.5% steel balls with a particle size of 0.8 cm; then ball milling is started, the ball milling time is 8 to 10 hours, and the average particle size of the slurry after ball milling is 0.7 um.

[0029] Step C is a ball mill slurry water reduction process, wherein the slurry treated in step B is pumped into an aggregate tower, and a flocculant is added, wherein the flocculant is polyacrylamide, and the amount added is 0.01% by weight; the agitator of the aggregate tower is turned on and operated for 10 to 15 minutes, and the mixture is allowed to settle for 2 to 3 hours, and then the clear water is discharged, and the water reduction rate reaches 45%.

[0030] Step D: Slurry filter pressing process, connecting the discharge port of the aggregate tower to the inlet of the automatic filter press, and connecting a 2KW / 1.5-inch pipeline pump in the middle; using 150-200 mesh nylon mesh between the plates and frames of the automatic filter press; turning on the hydraulic switch of the filter press, opening the aggregate tower valve, and turning on the pipeline pump to automatically feed the filter press, the feeding pressure is set to 10Mpa, the pressure holding time is 10 minutes, and then opening the filter press pressure reducing valve to discharge the material, the powder discharged from the filter press is block-shaped, and the moisture content of the block powder is less than 15%.

[0031] Step E: Bowling and drying process: the bulk powder treated in step D is changed into 5-8 cm blocks and put into bowls. 8 mm holes are drilled around and on the bottom of the bowl. The density of the holes is 4 / 10 cm. 2 ; Then put the bowl into the multi-layer drying rack and dry it in the drying room; the main engine of the drying room adopts an air energy frequency conversion system with a total power of 18kw and a temperature setting of 75℃. The moisture is discharged through the pipe and the hot air circulates in the drying room; the continuous drying time is 10 to 15 hours, and the moisture content of the powder is less than 0.55% when it leaves the drying room.

[0032] Step F is a crushing, screening and bagging process, in which the powder from the drying room is crushed by a crusher, and impurities are removed by vibration screening to obtain recycled powder.

[0033] In step G, the powder performance testing process is carried out by testing the performance of the recycled powder obtained in step F: Br3.44kGs, Hcb2.520kOe, Hcj3.425, BHm2.632MGOe; moisture content 0.55%; average particle size 0.7um.

[0034] Using the production process of Example 4, the magnetic properties of the recycled powder are low, the average particle size is fine, and the fluidity is poor, which affects the molding density. Example

[0035] A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material comprises the following steps: Step A: The grinding material is passed through a multi-stage water fluid to remove the diamond sand and other impurities produced by the grinding wheel consumption during the production of the grinding bed, and the qualified grinding material is obtained as a recycled raw material.

[0036] Step B: ball milling process, the grinding material treated in step A is put into a ball mill, and ingredients are added in a weight ratio of: 0.6% calcium carbonate, 0.10% silicon oxide, 0.3% aluminum oxide, 0.010% boric acid, 0.010% ammonium bicarbonate, and 1.7% steel balls with a particle size of 0.8 cm; then ball milling is started, the ball milling time is 5 to 6 hours, and the average particle size of the slurry after ball milling is 1.0 um.

[0037] Step C is a ball mill slurry water reduction process, wherein the slurry treated in step B is pumped into an aggregate tower, and a flocculant is added, wherein the flocculant is polyacrylamide, and the amount added is 0.02% by weight; the agitator of the aggregate tower is turned on and operated for 10 to 15 minutes, and the mixture is allowed to settle for 2 to 3 hours, and then the clear water is discharged, and the water reduction rate reaches 60%.

[0038] Step D: Slurry filter pressing process, connecting the discharge port of the aggregate tower to the inlet of the automatic filter press, and connecting a 2KW / 1.5-inch pipeline pump in the middle; using 150-200 mesh nylon mesh between the plates and frames of the automatic filter press; turning on the hydraulic switch of the filter press, opening the aggregate tower valve, and turning on the pipeline pump to automatically feed the filter press, the feeding pressure is set to 10Mpa, the pressure holding time is 10 minutes, and then opening the filter press pressure reducing valve to discharge the material, the powder discharged from the filter press is block-shaped, and the moisture content of the block powder is less than 15%.

[0039] Step E: Bowling and drying process: the bulk powder treated in step D is changed into 5-8 cm blocks and put into bowls. 8 mm holes are drilled around and on the bottom of the bowl. The density of the holes is 4 / 10 cm. 2 ; Then put the bowl into the multi-layer drying rack and dry it in the drying room; the main engine of the drying room adopts an air energy frequency conversion system with a total power of 18kw and a temperature setting of 75℃. The moisture is discharged through the pipe and the hot air circulates in the drying room; the continuous drying time is 10 to 15 hours, and the moisture content of the powder is less than 0.6% when it leaves the drying room.

[0040] Step F is a crushing, screening and bagging process, in which the powder from the drying room is crushed by a crusher, and impurities are removed by vibration screening to obtain recycled powder.

[0041] Step G is a powder performance testing process, in which the performance of the recycled powder obtained in step F is tested: Br3.26kGs, Hcb2.817kOe, Hcj3.48, BHm2.67MGOe; moisture content 0.55%; average particle size 0.9um~1.05um.

[0042] The four indicators of the remanence Br, intrinsic Hcb, intrinsic coercive force Hcj, and magnetic energy product BHm of the recycled powder obtained in Example 5 are relatively low.

Claims

1. A method for regenerating and preparing ferrite anisotropic magnetic tile grinding material, comprising the following steps: step A grinding material impurity treatment, step B ball milling process, step C ball milling slurry water reduction process, step D slurry filter press process, step E drying, step F crushing, screening and bagging process, characterized in that: In the ball milling process of step B, the grinding material treated in step A is put into a ball mill, and ingredients are added in a weight ratio of: 0.8% to 1.0% calcium carbonate, 0.12% to 0.15% silicon oxide, 0.4% to 0.6% aluminum oxide, 0.012% to 0.015% boric acid, 0.012% to 0.015% ammonium bicarbonate, and 1.5% to 1.7% steel balls with a particle size of 0.8 cm are added; then ball milling is started, the ball milling time is 6 to 8 hours, and the average particle size of the slurry after ball milling is 0.8um to 1.0um.

2. The method for regenerating and preparing ferrite anisotropic magnetic tile grinding material according to claim 1, characterized in that: In the step C of ball milling slurry water reduction process, the slurry treated in the step B is pumped into an aggregate tower, a flocculant is added, and the flocculant is polyacrylamide, and the added amount is 0.01% to 0.02% by weight; the agitator of the aggregate tower is turned on and operated for 10 to 15 minutes, and the sedimentation is performed for 2 to 3 hours, and then the clear water is discharged, and the water reduction rate reaches 55% to 62%.

3. The method for regenerating and preparing ferrite anisotropic magnetic tile grinding material according to claim 2, characterized in that: In the slurry filtration process of step D, the discharge port of the aggregate tower is connected to the inlet of the automatic filter press, and a 2KW / 1.5-inch pipeline pump is connected in the middle; 150-200 mesh nylon mesh is used between the plates and frames of the automatic filter press; the hydraulic switch of the filter press is turned on, the valve of the aggregate tower is opened, and the pipeline pump is turned on to automatically feed the filter press, the feeding pressure is set to 10Mpa, the pressure holding time is 10 minutes, and then the pressure reducing valve of the filter press is opened to discharge the material, and the powder discharged from the filter press is block-shaped, and the moisture content of the block-shaped powder is less than 15%.

4. The method for regenerating and preparing ferrite anisotropic magnetic tile grinding material according to claim 3, characterized in that: In the step E, the bulk powder treated in step D is changed into a 5-8 cm block and loaded into a bowl. 8 mm holes are drilled around the bowl and the bottom. The density of the holes is 4 / 10 cm. 2 ; Then put the bowl into the multi-layer drying rack and dry it in the drying room; the main engine of the drying room adopts an air energy frequency conversion system with a total power of 18kw and a temperature setting of 75℃. The moisture is discharged through the pipe and the hot air circulates in the drying room; the continuous drying time is 10 to 15 hours, and the moisture content of the powder is less than 0.55% when it leaves the drying room.