Method for forming groove and semiconductor process equipment
By modifying the initial groove into a vertical sidewall and arc-shaped middle groove at the bottom in a self-aligned double-patterning process, and combining the cyclic etching step, the depth load effect problem caused by the parity effect in the mask layer is solved. A more uniform etching effect and smaller etching depth differences are achieved.
Patent Information
- Application Number
- CN202411239446.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
In the self-aligning dual-pattern process, the parity effect within the mask layer results in a depth loading effect of the film layer to be etched, increasing the etch depth difference between the target trenches.
By forming initial trenches in the film layer to be etched and modifying them into intermediate trenches with vertical sidewalls and arcuate bottoms, etching, deposition and scavenging substeps performed by cyclically performing etching, deposition and scavenging, combining chemical and physical etching by forming initial trenches in the film layer to be etched and modifying them into intermediate trenches with vertical sidewalls and arcuate bottoms, the etching, deposition and scavenging substeps performed by cyclically combined with chemical and physical etching The gas gradually forms the target trench to reduce the difference in etching depth.
It effectively weakens the load effect in the film layer to be etched, improves the uniformity of etching, reduces the difference in etching depth between target trenches, and improves the stability of the process and product quality.
Smart Images

Figure CN119092402A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a groove and a semiconductor process equipment. Background Art
[0002] As the size of semiconductor processes continues to shrink, the self-aligned double patterning process (SADP) is gradually used to form a mask layer to reduce the opening size of the mask layer, thereby reducing the critical size, for example, reducing the critical size from more than 50nm to less than 30nm. However, in the process of etching the mask layer to form an opening using the self-aligned double patterning process, an odd-even effect will be generated in the mask layer. After this odd-even effect is transmitted to the film layer to be etched below the mask layer, a depth loading effect (Loading Effect) will be generated in the film layer to be etched. Summary of the invention
[0003] The present application provides a method for forming a trench and a semiconductor process equipment to solve the technical problems existing in the related art.
[0004] The first aspect of the present application provides a method for forming grooves, which is applied to a film layer to be etched, comprising: a first etching step, forming a plurality of initial grooves in the film layer to be etched, wherein the cross-section of the initial grooves is an inverted trapezoid; a first modification step, modifying each initial groove into an intermediate groove, wherein the intermediate groove is a groove structure with vertical side walls and an arc-shaped bottom; and a second etching step, etching each intermediate groove to form a target groove.
[0005] In one embodiment, the difference ratio between the bottom opening widths of the intermediate grooves is smaller than the difference ratio between the bottom opening widths of the initial grooves.
[0006] In one embodiment, the first modification step is isotropic etching; and / or the process gas used in the first modification step includes a fluorine-containing gas, and the flow rate range of the fluorine-containing gas is 200sccm to 250sccm; and / or the upper electrode power used in the first modification step is in the range of 800W to 1000W, and the process time is in the range of 5s to 10s.
[0007] In one embodiment, after the second etching step, the method further includes: a second modification step of modifying the bottom of each target trench to reduce the difference in etching depth of each target trench.
[0008] In one embodiment, the process conditions of the second modification step include:
[0009] The process gas includes chemical etching gas and physical bombardment gas, and the flow ratio between the physical etching gas and the chemical etching gas ranges from 1.8 to 2.2;
[0010] And / or, the process gas includes a sidewall protection gas, and the flow rate of the sidewall protection gas is 3% to 5% of the total flow rate of the process gas.
[0011] In one embodiment, the second etching step includes a sub-cycle of cyclically executing an etching sub-step, a deposition sub-step, and a cleaning sub-step, wherein the etching sub-step, the deposition sub-step, and the cleaning sub-step are executed sequentially in each sub-cycle; the etching sub-step is used to etch the bottom of the middle groove; the deposition sub-step is used to deposit a passivation layer on the side wall of the middle groove; and the cleaning sub-step is used to remove the deposition by-products at the bottom of the middle groove.
[0012] In one embodiment, the process conditions of the clearing sub-step include: the power of the lower electrode is in the range of 50W to 80W.
[0013] In one embodiment, the method further includes: a second modification step, after the second etching step, for modifying the bottom of the target trench, and the process gas type of the second modification step is the same as the process gas type of the etching sub-step.
[0014] In one embodiment, the content of the chemical etching gas in the second modification step is less than that in the etching sub-step, and the content of the sidewall protection gas in the second modification step is greater than that in the etching sub-step.
[0015] A second aspect of the present application provides a semiconductor process equipment, characterized in that it includes a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, the controller includes at least one processor and at least one memory, the memory stores a computer program, and when the computer program is executed by the processor, it implements the method of forming a groove in any of the above-mentioned embodiments.
[0016] The advantages or beneficial effects of the above technical scheme include at least: when a plurality of initial grooves with an inverted trapezoidal cross-section are formed in the film layer to be etched, each initial groove is modified into an intermediate groove with vertical side walls and an arc-shaped bottom by using the first modification step, so that the opening width of each intermediate groove has a tendency to decrease along the thickness direction of the film layer to be etched, which is weaker than the tendency of the opening width of each initial groove to decrease along the thickness direction of the film layer to be etched. In the second etching step, it is convenient for the process gas to smoothly enter each intermediate groove and for the etching by-products to be smoothly discharged from each intermediate groove, which is beneficial to improving the uniformity of etching and reducing the load effect in the film layer to be etched, thereby reducing the difference in etching depth between each target groove. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings herein are incorporated into and constitute a part of the specification, illustrate embodiments consistent with the present application, and together with the specification are used to explain the principles of the present application. In addition, these drawings and text descriptions are not intended to limit the scope of the concept of the present application in any way, but to illustrate the concept of the present application for those skilled in the art by referring to specific embodiments.
[0018] Figures 1A to 1D It is a schematic cross-sectional structure diagram of each step of forming an opening in a mask layer using a self-aligned double patterning process in the related art.
[0019] Figure 2 Shown is a schematic diagram of an electron microscope for forming a target groove in the related art.
[0020] Figure 3 FIG. 1 is a schematic flow chart of a method for forming a trench according to an embodiment of the present application.
[0021] FIG. 4A to FIG. 4D Shown are schematic cross-sectional views of various steps in the method for forming a groove.
[0022] Figure 5A Shown Figure 4A Schematic diagram of an electron microscope.
[0023] Figure 5B Shown Figure 4B Schematic diagram of an electron microscope.
[0024] Figure 5C Shown Figure 4D Schematic diagram of the electron microscope of the first target groove and the second target groove.
[0025] Fig. 6A Shown is a schematic diagram of the cross-sectional structure of modifying each initial groove.
[0026] Figure 6B for Fig. 6A A partial schematic diagram of .
[0027] Figure 7 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application. DETAILED DESCRIPTION
[0028] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0029] Figures 1A to 1D It is a schematic cross-sectional structure diagram of each step of forming a mask opening in a mask layer using a self-aligned double patterning process in the related art.
[0030] In the related art, a method for forming a mask opening in a mask layer includes the following steps S110 to S140 .
[0031] Step S110: Figure 1A As shown, a mask layer 12, a mandrel layer 13 and a sidewall layer 14 are sequentially formed on the film layer 11 to be etched; wherein the mandrel layer 13 has a plurality of spaced mandrels 131, and the sidewall layer 14 covers the top surface of the mandrel 131, the sidewall surface of the mandrel 131 and the exposed upper surface of the mask layer 12.
[0032] Step S120: Figure 1A to Figure 1B As shown, the sidewall layer 14 located on the top of the mandrel 131 and a portion of the upper surface of the mask layer 12 is removed by etching until a portion of the upper surface of the mask layer 12 is exposed, thereby forming a sidewall 141 covering the sidewall surface of the mandrel 131 .
[0033] Step S130: Figure 1B to Figure 1C As shown, the mandrel 131 is removed by etching, and the sidewall 141 remains.
[0034] Step S140: Figure 1C to Figure 1D As shown, the mask layer 12 is etched using the sidewall 141 as a mask to form a mask opening 121 in the mask layer 12 .
[0035] like Figure 1C As shown in FIG. 1 , during the process of etching away the mandrel 131 , a small amount of loss will occur on the side of the sidewall 141 away from the mandrel 131 , so that the widths of the openings on both sides of the same sidewall 141 will be slightly different, showing a periodic phenomenon of one large and one small. For example, the width of the odd-numbered opening 141A is greater than the width of the even-numbered opening 141B. This phenomenon is called the odd-even effect. Figure 1D As shown, when the mask layer 12 is etched using the spacer 141 as a mask, the odd-even effect is transferred to the mask layer 12, so that the widths of the odd-numbered mask openings 121A of the mask layer 12 are slightly larger than the widths of the even-numbered mask openings 121B.
[0036] The inventors discovered during the implementation of the present application that in the related art, the use of a self-aligned double patterning process to form a mask opening 121 in the mask layer 12 will produce an odd-even effect, so that the opening widths of two adjacent mask openings 121 are different, and due to the limitations of the etching process, the actual morphology of the opening defined by the sidewall 141 will not be completely transmitted vertically downward, but the opening width of the mask opening 121 will gradually decrease along the thickness direction of the mask layer 12, forming a morphology with an inverted trapezoidal cross section. The downward transmission of this cross-sectional morphology of the mask opening 121 will aggravate the load effect of the film layer 11 to be etched, thereby increasing the etching depth difference between each target groove 111 in the film layer 11 to be etched. For example, Figure 2 As shown, this increases the difference between the etching depth h1 of the first target trench 111A and the etching depth h2 of the second target trench 111B in the film layer 11 to be etched.
[0037] Based on this, an embodiment of the present application provides a method for forming a trench and a semiconductor process equipment to at least solve the above-mentioned technical problems.
[0038] Figure 3 FIG. 1 is a schematic flow chart of a method for forming a trench according to an embodiment of the present application. FIG. 4A to FIG. 4D Shown are schematic cross-sectional views of various steps in the method for forming a groove.
[0039] Please also read Figure 3 , FIG. 4A to FIG. 4C The method for forming a groove is applied to the film layer 11 to be etched. The method for forming a groove includes the following steps S110 to S130.
[0040] Step S110: Figure 4A and Figure 5A In the first etching step, a plurality of initial grooves 112 are formed in the film layer 11 to be etched, and the cross section of the initial grooves 112 is an inverted trapezoid.
[0041] Step S120: FIG. 4A to FIG. 4B , Figure 5B As shown, in the first modification step, each initial groove 112 is modified into an intermediate groove 113, and the intermediate groove 113 is a groove structure with vertical side walls and an arc-shaped bottom.
[0042] Step S130: FIG. 4B to FIG. 4C As shown, in the second etching step, each intermediate trench 113 is etched to form a target trench 111 .
[0043] In the above scheme, when a plurality of initial grooves 112 having an inverted trapezoidal cross-section are formed in the film layer 11 to be etched, each initial groove 112 is modified into an intermediate groove 113 having a vertical side wall and an arc-shaped bottom by using a first modification step, so that the opening width of each intermediate groove 113 has a tendency to decrease along the thickness direction D1 of the film layer 11 to be etched, which is weaker than the tendency of the opening width of each initial groove 112 to decrease along the thickness direction D1 of the film layer 11 to be etched. In the second etching step, it is convenient for the process gas to smoothly enter each intermediate groove 113 and for the etching by-products to be smoothly discharged from each intermediate groove 113, which is beneficial to improving the uniformity of etching and reducing the load effect in the film layer 11 to be etched, thereby reducing the difference in etching depth between each target groove 111.
[0044] In one embodiment, please refer to Fig. 6A and Figure 6B, the difference ratio between the bottom opening widths of each intermediate groove 113 is smaller than the difference ratio between the bottom opening widths of each initial groove 112 .
[0045] For example, Fig. 6A As shown, the initial trench 112 includes a first initial trench 112A and a second initial trench 112B adjacent to each other, and the bottom opening width of the first initial trench 112A is greater than the bottom opening width of the second initial trench 112B. For example, the bottom opening width of the first initial trench 112A is 3.5 nm, and the bottom opening width of the second initial trench 112B is 3 nm. After the first initial trench 112A is modified into the first intermediate trench 113A and the second initial trench 112B is modified into the second intermediate trench 113B by the first modification step, the bottom opening width of the first intermediate trench 113A is 6.5 nm, and the bottom opening width of the second intermediate trench 113B is 6 nm.
[0046] The difference ratio P1 between the bottom opening widths of the initial trenches 112 may be the difference ratio between the bottom opening width w1 of the first initial trench 112A and the bottom opening width w2 of the second initial trench 112B, and the difference ratio P1 may be calculated by the following formula (1):
[0047]
[0048] The above formula (1) can be used to calculate that the difference ratio P1 between the bottom opening widths of the initial grooves 112 is about 16.7%. Similarly, referring to the above formula (1), the difference ratio P2 between the bottom opening widths of the intermediate grooves 113 can be calculated to be about 8.3%. It can be seen that the difference ratio P2 between the bottom opening widths of the intermediate grooves 113 is reduced by 8.4% compared with the difference ratio P1 between the bottom opening widths of the initial grooves 112.
[0049] In addition, the reduction amount E of the influence degree of the difference between the bottom opening widths of each intermediate trench 113 on the difference between the etching depths of each target trench 111 compared with the influence degree of the difference between the bottom opening widths of each initial trench 112 on the difference between the etching depths of each target trench 111 can be calculated by the following formula (2):
[0050]
[0051] In practical applications, there is a difference ratio between the bottom opening widths of each initial groove 112. This opening difference will affect the difference in etching depth between each target groove 111. Specifically, the greater the difference ratio, the greater the impact on the etching depth difference. For example, the related technology directly etches each initial groove 112 into a corresponding target groove 111, which will cause the opening difference between each initial groove 112 to have a greater impact on the etching depth difference between each target groove 111, and it is easy to produce a more serious depth loading effect between each target groove 111.
[0052] Compared with the related art, the above scheme can reduce the influence of the opening difference on the etching depth difference between each target groove 111 by first modifying each initial groove 112 into an intermediate groove 113 and making the difference ratio P2 between the bottom opening widths of each intermediate groove 113 smaller than the difference ratio P1 between the bottom opening widths of each initial groove 112. For example, using the above formula (2), it can be calculated that the influence on the etching depth difference between each target groove 111 is reduced by 50.3%, which helps to reduce the depth load effect, thereby reducing the etching depth difference between each target groove 111.
[0053] In one embodiment, please refer to Fig. 6A and Figure 6B , the first modification step is isotropic etching.
[0054] Exemplarily, the first modification step is used to isotropically etch the groove walls of the first initial groove 112A and the second initial groove 112B, so that the side walls of the first initial groove 112A and the second initial groove 112B are expanded outward, and the expansion dimension w increases along the thickness direction D1 of the film layer 11 to be etched. For example, the expansion dimension w of a side wall of each initial groove 112 can be increased from 0.5nm to 1nm along the thickness direction D1 of the film layer 11 to be etched, thereby expanding the opening width of the first initial groove 112A and the second initial groove 112B; and expanding the bottom walls of the first initial groove 112A and the second initial groove 112B outward and downward, wherein the downward expansion dimension h of each initial groove 112 decreases gradually from the middle to the two sides of each initial groove 112, for example, starting from 0.5nm. In this way, the first initial trench 112A and the second initial trench 112B can be modified into a trench structure with vertical sidewalls and an arc-shaped bottom. The trench wall of each initial trench 112 is surrounded by two sidewalls and a bottom wall.
[0055] It should be noted that although the driving force for fluorine ions to etch the groove walls of the first initial groove 112A and the second initial groove 112B in all directions is basically equal, since the cross-sectional shape of the plasma source composed of fluorine plasma is elliptical, the distances of the groove walls of the first initial groove 112A and the second initial groove 112B from the plasma source in all directions are different, so that the bottom of the first initial groove 112A and the second initial groove 112B will eventually be modified into an arc shape that matches the cross-sectional shape of the plasma source.
[0056] In one embodiment, the process gas used in the first modification step includes a fluorine-containing gas, and the flow rate of the fluorine-containing gas is in the range of 200 sccm to 250 sccm (including the end points).
[0057] For example, see FIG. 4A to FIG. 4B The material of the film layer 11 to be etched is a silicon (Si)-containing material, and the chlorine-containing gas can be carbon tetrafluoride (CF4), trifluoromethane (CHF3), difluoromethane (CH2F2), etc. There is a positive proportional relationship between the ratio of fluorine atoms to carbon atoms in the fluorine-containing gas and the etching rate of the fluorine-containing gas on the silicon-containing material, that is, the higher the fluorine-carbon ratio of the fluorine-containing gas, the faster the etching rate of the fluorine-containing gas on the silicon-containing material. Therefore, carbon tetrafluoride can be preferably used as the etching gas for the first modification step.
[0058] In one embodiment, the upper electrode power used in the first modification step ranges from 800 W to 1000 W (including the endpoint values), and the process time ranges from 5 s to 10 s (including the endpoint values).
[0059] The upper electrode power is used to control the density of fluorine ions generated by the electrolysis of fluorine-containing gases. By configuring the upper electrode power to be between 800W and 1000W, the density of fluorine ions generated by the electrolysis of fluorine-containing gases can be controlled within a suitable range. Please refer to Fig. 6A and Figure 6B By configuring the lower electrode power to be 0 W, that is, not loading bias power, the fluorine ions can isotropically etch the groove wall of the initial groove 112 .
[0060] The process time is used to control the degree of modification of the initial trench 112. Fig. 6A When the process time is less than 5s, the modification degree of the initial groove 112 is low, the opening width of the initial groove 112 is small, the etching rate of the groove wall of the initial groove 112 by the fluorine ions is low, and the production capacity is low; when the process time is greater than 10s, the fluorine ions will consume a large amount of the mask layer 12 on the film layer 11 to be etched. By selecting the process time of the first modification step to be between 5s and 10s, it can be ensured that the initial groove 112 is modified into the intermediate groove 113 at a suitable etching rate, and it can be ensured that the fluorine ions will not consume a large amount of the mask layer 12.
[0061] In one embodiment, please refer to FIG. 4C to FIG. 4D , Figure 5C After the second etching step, the method further includes a second modification step, which is used to modify the bottom of each target trench 111 to reduce the difference in etching depth of each target trench 111 .
[0062] For example, Figure 4C As shown, the target trench 111 includes a first target trench 111A and a second target trench 111B adjacent to each other; after the second etching step, the etching depth h1 of the first target trench 111A is greater than the etching depth h2 of the second target trench 111B. Figure 4D and Figure 5C As shown, in the second modification step, the bottom of each target groove 111 is modified to reduce the difference in etching depth of each target groove 111. The bottom of the first target groove 111A and the second target groove 111B are modified so that the etching depth h1 of the first target groove 111A is close to the etching depth h2 of the second target groove 111B.
[0063] For further information, please continue to refer to FIG. 4C to FIG. 4D In the second modification step, the modification of the bottom of each target groove 111 is mainly physical etching. In the second modification step, since the bombardment force of physical etching decreases along the thickness direction D1 of the film layer 11 to be etched, the etching depth h1 of the first target groove 111A is greater than the etching depth h2 of the second target groove 111B. When etching starts, the bombardment force on the first target groove 111A is less than the bombardment force on the second target groove 111B, so that the etching rate of the bottom of the first target groove 111A is less than the etching rate of the bottom of the second target groove 111B; as the process As time goes by, the bombardment force on the first target groove 111A gradually approaches the bombardment force on the second target groove 111B, so that the etching rate on the bottom of the first target groove 111A gradually approaches the etching rate on the bottom of the second target groove 111B, and the difference in etching depth between the first target groove 111A and the second target groove 111B gradually decreases until the etching depth h1 of the first target groove 111A approaches the etching depth h2 of the second target groove 111B.
[0064] For example, after the second etching step, the etching depth h1 of the first target trench 111A and the etching depth h2 of the second target trench 111B may both be between to and the etching depth h1 of the first target groove 111A is greater than the etching depth h2 of the second target groove 111B; after the second modification step, the etching depth h1 of the first target groove 111A and the etching depth h2 of the second target groove 111B are both
[0065] In the above scheme, after the second etching step, the bottom of each target groove 111 is modified by the second modification step to reduce the etching depth difference of each target groove 111, which is conducive to uniform bottom morphology of each target groove 111, thereby improving etching uniformity and improving product yield. In addition, after the second etching step is used in combination with the first modification step, it is conducive to completely eliminating the etching depth difference between each target groove 111, achieving the purpose of completely solving the depth load.
[0066] In one embodiment, the process conditions of the second modification step include at least one of the following:
[0067] The process gas includes a chemical etching gas and a physical bombardment gas, and the flow ratio between the physical etching gas and the chemical etching gas is in the range of 1.8 to 2.2 (including the end value);
[0068] The process gas includes a side wall protection gas, and the flow rate of the side wall protection gas is 3% to 5% (including the end point value) of the total flow rate of the process gas.
[0069] For example, please refer to FIG. 4C to FIG. 4D , the material of the film layer 11 to be etched is silicon. After the first target groove 111A and the second target groove 111B are formed, silicon oxides, such as silicon dioxide (SiO2), exist at the bottom of the first target groove 111A and the second target groove 111B. The chemical etching gas has a strong ability to etch silicon, but a weak ability to etch silicon oxides. When the ratio of the flow rate of the physical etching gas to the flow rate of the chemical etching gas is less than 1.8, the content of the chemical etching gas in the process gas is relatively high, and it is easy to cause a local load effect at the bottom of the target groove 111 due to the selective etching of the chemical etching gas. When the ratio of the flow rate of the physical etching gas to the flow rate of the chemical etching gas is greater than 2.2, the content of the physical etching gas in the process gas is relatively high, and the content of the chemical etching gas is relatively low, which will reduce the etching efficiency. By selecting the ratio of the flow rate of the physical etching gas to the flow rate of the chemical etching gas to be between 1.8 and 2.2, the local load effect at the bottom of each target groove 111 can be effectively controlled and optimized, and a high etching efficiency can be ensured.
[0070] For example, please refer to FIG. 4C to FIG. 4DIn the second modification step, the sidewall protection gas is used to form a dense and continuous sidewall protection layer (not shown in the drawings) on the bottom sidewall of each target groove 111, and the sidewall of the bottom sidewall of each target groove 111 is protected to prevent the process gas from selectively etching the bottom of each target groove 111. Among them, when the flow rate of the sidewall protection gas accounts for less than 3% of the total flow rate of the process gas, the thickness of the sidewall protection layer formed by the sidewall protection gas on the bottom sidewall of each target groove 111 is thin, and the sidewall protection layer is easily destroyed under the action of physical bombardment, and the etching rate of the target groove 111 with the destroyed sidewall protection layer is faster than that of the target groove 111 without being destroyed, causing local load deterioration. When the flow rate of the sidewall protection gas accounts for more than 5% of the total flow rate of the process gas, the thickness of the sidewall protection layer formed by the sidewall protection gas on the bottom sidewall of each target groove 111 is thick, which is easy to cause etching to stop. In the second modification step, by selecting the flow rate of the sidewall protection gas to be between 3% and 5% of the total flow rate of the process gas, it is beneficial to ensure that the etching depth of each target groove 111 is uniform, there is no load effect, and etching stops are not caused.
[0071] In one embodiment, the second etching step includes a sub-cycle of cyclically executing an etching sub-step, a passivation sub-step, and a cleaning sub-step, wherein the etching sub-step, the passivation sub-step, and the cleaning sub-step are executed sequentially in each sub-cycle, wherein the number of sub-cycles may be greater than or equal to 2, preferably 3.
[0072] Please refer to FIG. 4B to FIG. 4C The etching sub-step is used to etch the bottom of the middle trench 113, the passivation sub-step is used to form a passivation layer on the sidewall of the middle trench 113 (not shown in the drawings), and the cleaning sub-step is used to remove the deposition by-products located at the bottom of the middle trench 113, wherein the deposition by-products at the bottom of the middle trench 113 may include the passivation layer located at the bottom of the middle trench 113.
[0073] In the above scheme, in each sub-cycle, the bottom of the middle groove 113 is first etched by the etching sub-step, and then the passivation sub-step is used to form a passivation layer on the side wall of the middle groove 113, which can protect the side wall of the middle groove 113 from serious lateral etching, so that the side wall morphology of the middle groove 113 is continuous and vertical, and then the deposition byproducts located at the bottom of the middle groove 113 are removed by the cleaning sub-step, which can improve the etching efficiency of the next sub-cycle and prevent the difference in etching depth between each middle groove 113 from being amplified, which is conducive to ensuring the uniform etching depth of each middle groove 113. Such a cyclic execution of the etching sub-step, the passivation sub-step and the cleaning sub-step can ensure that the target groove 111 with a continuous and vertical side wall morphology is obtained under the premise of high-efficiency etching, and is conducive to the uniform etching depth between each target groove 111.
[0074] In one embodiment, the process conditions of the clearing sub-step include: the lower electrode power is 50W to 80W (including end points).
[0075] In the cleaning sub-step, the lower electrode power is used to allow the plasma to obtain vertically downward bombardment energy. The greater the lower electrode power, the greater the bombardment energy obtained by the plasma, and the greater the bombardment force on the deposition byproducts at the bottom of the middle groove 113. Since the thickness of the deposition byproducts at the bottom of the middle groove 113 is usually less than If the power of the lower electrode is too large, the bombardment energy of the plasma will be too large. The plasma will not only remove the deposition by-products, but most of the plasma will continue to reflect toward the side walls of the middle groove 113 when it reaches the bottom of the middle groove 113, causing damage to the side walls of the middle groove 113 and morphological displacement. Therefore, by controlling the power of the lower electrode to be between 50W and 80W, the plasma can obtain a suitable bombardment energy to ensure that the deposition by-products at the bottom of the middle groove 113 are removed by the bombardment of the plasma, and that only a small part of the plasma is reflected onto the side walls of the middle groove 113 after reaching the bottom of the middle groove 113. In this way, the passivation layer formed in the passivation sub-step can continue to protect the side walls of the middle groove 113 from being vertical without morphological displacement.
[0076] Furthermore, the process conditions of the cleaning sub-step include: the process gas includes fluorine-containing carbon-containing gas, the carbon-containing fluorine-containing gas includes carbon tetrafluoride and trifluoromethane, the flow rate range of carbon tetrafluoride and trifluoromethane can both be 50sccm~100sccm (including endpoint values), and the flow rate ratio of carbon tetrafluoride to trifluoromethane is in the range of 1~1.2 (including endpoint values).
[0077] In one embodiment, the type of process gas in the second modification step is the same as the type of process gas in the etching sub-step.
[0078] Exemplarily, the process gases of the second modification step and the etching sub-step include chemical etching gas, physical etching gas and sidewall protection gas. Specifically, the chemical etching gas can be chlorine, the physical etching gas can be argon, and the sidewall protection gas can be oxygen. In the second modification step, the flow rate range of chlorine is 100sccm to 200sccm, the flow rate range of argon is 200sccm to 400sccm, and the flow rate range of oxygen is 10sccm to 20sccm; in the etching sub-step, the flow rate range of chlorine and argon is 200sccm to 300sccm, and the flow rate range of oxygen is 10sccm to 15sccm.
[0079] See also FIG. 4C to FIG. 4DIn the second modification step, the physical etching gas is mainly used to physically bombard the bottom of the target trench 111 to promote depth transfer, the chemical etching gas plays an auxiliary etching role, and the sidewall protection gas is used to form a continuous and dense sidewall protection layer on the bottom sidewall of the target trench 111. FIG. 4B to FIG. 4C In the etching sub-step, the chemical etching gas is mainly used to chemically react with the bottom of the middle trench 113 to promote the transfer of etching depth, the physical etching gas is used to improve the uniformity of etching, and the sidewall protection layer is used to protect the sidewall of the middle trench 113. Therefore, although the process gas type of the second modification step and the etching sub-step is the same, the etching properties of the two are different.
[0080] In the above scheme, by setting the process gas type of the second modification step to be the same as the process gas type of the etching sub-step, the consistency of the process gas type can be maintained and resources can be saved.
[0081] In one embodiment, the content of the chemical etching gas in the second modification step is less than that in the etching sub-step, and the content of the sidewall protection gas in the second modification step is greater than that in the etching sub-step.
[0082] For example, see FIG. 4C to FIG. 4D , continue to take the example that the material of the film layer 11 to be etched is silicon, the chemical etching gas is chlorine, and the sidewall protection gas is oxygen. In the second modification step and the etching sub-step, the chlorine reacts with silicon to generate loose etching byproducts such as SiCl or SiCl2, and the sidewall protection gas reacts with silicon to generate silicon oxide (SiO2).
[0083] If the process parameters in the etching sub-step are extended to the second modification step, the content of the chemical etching gas is high and the content of the sidewall protection gas is low. As the aspect ratio of the target groove 111 gradually increases, for example, when the etching depth is close to 10, the etching byproducts (such as SiCl or SiCl2) deposited at the bottom of the target groove 111 will be difficult to discharge; and because the etching byproducts are loose and not dense, they are easily randomly distributed at the bottom of each target groove 111 under the action of physical bombardment, resulting in a slow etching rate in the area where the etching byproducts are thickly distributed, and a fast etching rate in the area where the etching byproducts are thinly distributed. This random distribution difference will increase the unevenness of the etching depth between each target groove 111. In addition, because the content of the sidewall protection gas is low, it will also lead to the inability to form a uniform and dense sidewall protection layer on the bottom sidewall of the target groove 111, which is not conducive to effective protection of the bottom sidewall of each target groove 111.
[0084] Based on this, in the second modification step, by setting the content of the chemical etching gas to be smaller than the content of the chemical etching gas in the etching sub-step, the content of the sidewall protection gas in the second modification step is greater than the content of the sidewall protection gas in the etching sub-step, the generation of etching by-products can be reduced, thereby reducing the random distribution differences of the etching by-products under the action of physical bombardment, which is beneficial to improving the uniformity of the etching depth between each target groove 111, and improving the uniformity and density of the sidewall protection layer.
[0085] It should be noted that the content of chemical etching gas and the content of sidewall protection gas in the second modification step are designed according to the specific process requirements of the bottom of the target trench with an aspect ratio close to 10 and a dynamic balance between physical bombardment and chemical passivation, and therefore cannot be used in the etching sub-step. If the process parameters in the second modification step are used in the etching sub-step, the content of chemical etching gas is low and the content of sidewall protection gas is high. Since silicon oxide is more stable than SiCl and SiCl2, it is difficult for chlorine to react with silicon oxide, which will cause etching to stop.
[0086] Figure 7 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application.
[0087] like Figure 7 As shown, the semiconductor process equipment 200 may include a process chamber 20, an inlet assembly 20A, an upper electrode assembly 20B and a lower electrode assembly 20C, a gas extraction assembly 20D and a controller ( Figure 7 The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for forming a groove in any one of the above embodiments is implemented.
[0088] Exemplarily, the controller can be a host computer or a slave computer. The controller can control the valve opening of the air inlet component 20A to introduce the corresponding process gas into the process chamber 20; the controller can also control the opening and closing degree of the valve of the air inlet component 20A to control the flow rate of the process gas. The controller can also control the exhaust component 20D to exhaust the interior of the process chamber 20, such as controlling the valve opening degree or the exhaust pump speed of the exhaust component 20D, to control the pressure inside the process chamber 20, discharge reaction byproducts, etc.
[0089] The upper electrode assembly 20B may include an RF coil 21, an upper RF power source 23 and an upper matcher 25. The controller is also used to control the upper RF power source 23 to provide RF power to the RF coil 21 through the upper matcher 25, so that the RF coil 21 excites the process gas inside the process chamber 20 to generate plasma 100.
[0090] The lower electrode assembly 20C may include a wafer carrier 22, a lower RF power supply 24, and a lower matcher 26. The controller is also used to control the lower RF power supply 24 to provide RF power to the wafer carrier 22 through the lower matcher 26 to provide RF bias. The wafer carrier 22 may be, for example, an electrostatic chuck, a mechanical chuck, or a vacuum adsorption chuck.
[0091] The semiconductor process equipment 200 of the embodiment of the present application may be an inductively coupled plasma (ICP) device or a capacitively coupled plasma (CCP) device. The embodiment of the present application does not limit the type of the semiconductor process equipment 200.
[0092] It should be noted that, since the semiconductor process equipment adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0093] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they contradict each other.
[0094] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0095] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for forming a groove, characterized in that: Applied to the film layer to be etched, including: In a first etching step, a plurality of initial grooves are formed in the film layer to be etched, wherein the cross section of the initial grooves is an inverted trapezoid; In a first modification step, each of the initial grooves is modified into an intermediate groove, wherein the intermediate groove is a groove structure with vertical sidewalls and an arc-shaped bottom; In the second etching step, each of the intermediate grooves is etched to form a target groove.
2. The method according to claim 1, characterized in that The difference ratio between the bottom opening widths of the intermediate grooves is smaller than the difference ratio between the bottom openings of the initial grooves.
3. The method according to claim 1, characterized in that The first modification step is isotropic etching; And / or, the process gas used in the first modification step includes a fluorine-containing gas, and the flow rate of the fluorine-containing gas is in the range of 200 sccm to 250 sccm; And / or, the upper electrode power used in the first modification step is in the range of 800W to 1000W, and the process time is in the range of 5s to 10s.
4. The method according to claim 1, characterized in that: After the second etching step, the method further comprises: In the second modification step, the bottom of each of the target grooves is modified to reduce the difference in etching depth of each of the target grooves.
5. The method according to claim 4, characterized in that The process conditions of the second modification step include: The process gas includes a chemical etching gas and a physical bombardment gas, and the flow ratio between the physical etching gas and the chemical etching gas is in the range of 1.8 to 2.2; And / or, the process gas includes a sidewall protection gas, and the flow rate of the sidewall protection gas is 3% to 5% of the total flow rate of the process gas.
6. The method according to claim 1, characterized in that The second etching step includes a sub-cycle of cyclically executing an etching sub-step, a deposition sub-step and a cleaning sub-step, wherein in each sub-cycle, the etching sub-step, the deposition sub-step and the cleaning sub-step are executed sequentially; The etching sub-step is used to etch the bottom of the middle trench; The deposition sub-step is used to deposit a passivation layer on the sidewall of the middle trench; The cleaning sub-step is used to remove the deposition byproducts located at the bottom of the middle trench.
7. The method according to claim 6, characterized in that The process conditions of the cleaning sub-step include: the power range of the lower electrode is 50W to 80W.
8. The method according to claim 6, characterized in that The method further comprises: The second modification step, after the second etching step, is used to modify the bottom of the target trench, and the process gas type of the second modification step is the same as the process gas type of the etching sub-step.
9. The method according to claim 8, characterized in that The content of the chemical etching gas in the second modification step is less than that in the etching sub-step, and the content of the sidewall protection gas in the second modification step is greater than that in the etching sub-step.
10. A semiconductor process equipment, characterized in that: The method comprises a process chamber, an air inlet assembly, an upper electrode assembly, a lower electrode assembly and a controller, wherein the controller comprises at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for forming a groove as described in any one of claims 1 to 9 is implemented.