Microporous aluminum foil and preparation method thereof
By preparing 10-50nm microporous aluminum foil in lithium batteries, the dendrite problem caused by uneven coating during charging and discharging of lithium batteries is solved, the battery life is extended and the number of cycles is improved, and the uniformity and safety of electrode materials are achieved. sex.
Patent Information
- Application Number
- CN202411343067.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
AI Technical Summary
During the charging and discharging process of lithium batteries, due to uneven coating of slurry on the positive and negative electrode sheets, lithium ions deintercalation and dendrites are formed, which shortens the battery life and causes safety problems. There is a lack of effective microporous aluminum foil solutions in the prior art.
By preparing 10-50nm micropores on aluminum foil, using the tip discharge in the electrolyte to form micropores, control the pore size and apply it in the battery, ensuring that the electrolyte and ions can pass through, while preventing the penetration of the electrode slurry and avoiding dendrites. Formation.
It extends the service life of the battery, improves the number of cycle charge and discharge times of the battery, and ensures the uniformity and safety of the electrode material by controlling the aperture of the micropores.
Smart Images

Figure CN119092632A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium batteries, and in particular to a microporous aluminum foil and a preparation method thereof. Background Art
[0002] The negative electrode current collector of lithium-ion batteries is copper foil, and the positive electrode current collector is aluminum foil. The negative electrode material is coated on both sides of the copper foil, and the positive electrode material is coated on both sides of the aluminum foil. The positive and negative electrodes are separated by a diaphragm in the middle. In the actual production process, the slurry on the positive and negative electrode sheets is unevenly coated, resulting in uneven electrode slurries on the positive and negative electrode sheets, with more electrode slurry in the protruding parts and less electrode slurry in the concave parts. When the lithium battery is charged, the lithium ions in the electrode slurry are deintercalated from the positive electrode material and embedded into the negative electrode material through the diaphragm. The protruding part of the positive electrode sheet has more electrode slurry and provides more lithium ions. The corresponding negative electrode sheet cannot provide enough negative electrode material to absorb lithium ions at the protruding part of the positive electrode. These lithium ions that cannot be absorbed by the negative electrode material are deposited on the surface of the negative electrode to form dendrites, causing the battery life to decay rapidly. Dendrites piercing the diaphragm can also cause safety problems.
[0003] In order to solve a series of problems caused by uneven slurry coating, patent 201810703557.X discloses a method for preparing microporous copper foil for negative electrode of high-capacity lithium-ion battery, the preparation method includes an electrolytic cell provided on a raw foil machine frame, an anode plate in the electrolytic cell, the anode cell is connected to the positive electrode of the power supply through a copper bus, a cathode roller connected to the negative electrode of the power supply is provided above the anode cell, characterized in that the anode plate is densely covered with numerous needle points, and the resulting copper foil has a porosity of 20% and a pore diameter of 10um; in the actual production process, when the pore diameter of the copper foil micropores is ≥1um, when the electrode slurry is wet-coated, the solvent or glue in the slurry will flow through the micropores to the reverse side and stick to the coating roller, causing the coating machine to be unable to produce.
[0004] At present, there is no related existing technology of microporous aluminum foil, and there is no microporous aluminum foil product on the market. In order to solve the problems of uneven coating and lithium deposition during battery charging and discharging, microporous copper foil is relied on alone. The technical solution is single and the effect of solving the problem of lithium deposition is not ideal. Summary of the invention
[0005] The object of the present invention is to provide a microporous aluminum foil, which has micropores with a diameter of 10-50nm. When the aluminum foil is coated with a positive electrode material, the positive electrode slurry cannot penetrate from the micropores of this size. After the aluminum foil is assembled into a battery, the electrolyte has low viscosity and small surface tension, and can penetrate from the A side of the aluminum foil to the B side of the aluminum foil through the micropores; the ion diameter is less than 1nm, and the pore size of 10-50nm is sufficient for a large number of ions to pass through at the same time, which can avoid the generation of dendrites during charging and discharging due to uneven coating.
[0006] Another object of the present invention is to provide a method for preparing a microporous aluminum foil, which comprises preparing a raised and recessed microstructure on the aluminum foil, performing electrolytic corrosion in an electrolyte, discharging at the tip of the raised portion, preferentially losing aluminum ions, and then forming micropores at the raised portion, and the pore size of the micropores can be controlled to be 10-50nm.
[0007] The present invention solves the technical problem by adopting the following technical solutions.
[0008] On the one hand, an embodiment of the present invention provides a method for preparing a microporous aluminum foil, comprising the following steps:
[0009] S1, preparation of aluminum foil with microstructure;
[0010] S2, preparing an electrolyte, placing the aluminum foil in the electrolyte, and electrolyzing the aluminum foil so that the tip of the raised portion of the microstructure of the aluminum foil discharges, thereby forming micropores.
[0011] In some embodiments of the present invention, the micro-shaped structure comprises a plurality of protrusions and recesses, and the plurality of protrusions and the plurality of recesses are alternately and equidistantly distributed.
[0012] In some embodiments of the present invention, the microstructure on the aluminum foil is obtained by extrusion molding.
[0013] In some embodiments of the present invention, in step S2, the electrolyte includes, by mass percentage, 10.74% ethylene carbonate, 32.24% dimethyl carbonate, 10.75% ethyl methyl carbonate, and 46.27% aluminum hexafluorophosphate.
[0014] Metal aluminum is an amphoteric metal that can dissolve in both acid and alkali, so the electrolyte cannot be acidic or alkaline. The present invention uses an organic electrolyte to control the ambient temperature and humidity, so that aluminum metal will not dissolve in the electrolyte. However, by using aluminum foil as an anode and connecting it to the positive electrode of a power source, the aluminum atoms at the protruding tip of the aluminum foil can lose electrons and be converted into aluminum ions that enter the electrolyte, forming micropores at the protruding tip of the aluminum foil.
[0015] In some embodiments of the present invention, in step S2, the electrolysis comprises:
[0016] An anode roller, a cathode roller, a reel and a reel are arranged in the electrolytic cell. One end of the aluminum foil is connected to the reel, and the other end is connected to the reel by passing through the anode roller. -5 A-1.39*10 -4 A current, and the aluminum foil was wound up at a winding speed of 2 m / min.
[0017] On the other hand, an embodiment of the present invention provides a microporous aluminum foil, which is prepared by the microporous aluminum foil preparation method.
[0018] In some embodiments of the present invention, the pore size of the micropores is 10-50 nm.
[0019] Compared with the prior art, the embodiments of the present invention have at least the following advantages or beneficial effects:
[0020] The microporous aluminum foil provided by the present invention has micropores with a diameter of 10-50nm. When the aluminum foil with micropores of this size is coated with electrode slurry, the electrode slurry will not pass through the micropores. However, after the aluminum foil is assembled into a battery and injected with electrolyte, the electrolyte has low viscosity and small surface tension, and can penetrate from the A surface of the aluminum foil to the B surface of the aluminum foil through the micropores; and the ion diameter is less than 1nm, and the pore diameter of 10-50nm is sufficient for a large number of ions to pass through at the same time. When the aluminum foil is used in a battery, the generation of dendrites on the electrode can be avoided, thereby extending the service life of the battery and increasing the number of battery charge and discharge cycles.
[0021] The preparation method provided by the present invention can discharge the aluminum foil with microstructure at the tip under electrolysis, lose aluminum ions, and then form micropores at the protrusions of the aluminum foil, and the pore size of the micropores is controlled to be 10-50nm by controlling the current and electrolysis time. The preparation method is simple and fast, and can quickly obtain microporous aluminum foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 A microscopic image of an aluminum foil with a micro-shaped structure used in an embodiment of the present invention;
[0024] Figure 2 A schematic diagram of an electrolytic cell for preparing micropores in an embodiment of the present invention;
[0025] Figure 3 A schematic diagram of the structure of a microporous aluminum foil provided in an embodiment of the present invention installed in a battery;
[0026] Figure 4 A simplified schematic diagram of a microporous aluminum foil provided in an embodiment of the present invention;
[0027] Figure 5 for Figure 4 A magnified schematic diagram of part A;
[0028] Figure 6 This is a cross-sectional schematic diagram of a microporous aluminum foil coated with electrode slurry according to an embodiment of the present invention;
[0029] Icons: 201-negative electrode sheet A side, 202-copper foil, 203-negative electrode sheet B side, 204-diaphragm, 205-positive electrode sheet A side, 207-positive electrode sheet B side, 208-stacking, 209-micropores, 300-positive electrode slurry, 401-protrusions, 402-depressions, 501-anode roller, 502-cathode roller, 503-unwinding reel, 504-rewinding reel, 505-aluminum foil recovery reel, 506-microporous aluminum foil, 507-electrolyte, B-protrusion height, C-protrusion diameter, D-protrusion spacing, D1-slurry thickness on positive electrode sheet A side, D2-slurry thickness on positive electrode sheet B side, D3-slurry thickness at the bottom of the depression, D4-slurry thickness at the top of the protrusion. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0031] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other. The present invention will be described in detail below with reference to specific embodiments.
[0032] On the one hand, an embodiment of the present invention provides a method for preparing a microporous aluminum foil 506, comprising the following steps:
[0033] S1, preparation of aluminum foil with microstructure;
[0034] S2, preparing an electrolyte 507, placing the aluminum foil in the electrolyte 507, and electrolyzing it so that the tip of the protrusion 401 of the micro-structure of the aluminum foil discharges, thereby forming micropores 209.
[0035] In some embodiments of the present invention, the micro-shaped structure comprises a plurality of protrusions 401 and depressions 402, and the plurality of protrusions 401 and the plurality of depressions 402 are alternately and equidistantly distributed. Figure 1 , 4 As shown in Figure 6, the micro-structure on the aluminum foil has protrusions 401 and depressions 402 (seen from one side), and the protrusions 401 and depressions 402 are arranged alternately, one column of protrusions 401 and one column of depressions 402, and the columns of protrusions 401 and the columns of depressions 402 are arranged alternately. Specifically, in the embodiment provided by the present invention, the thickness of the aluminum foil is 8um, and the spacing between two columns of protrusions 401 or adjacent protrusions 401 is 140um.
[0036] It should be noted that the principle of preparing the micropores 209 by tip discharge in the present invention is as follows:
[0037] When the micro-shaped aluminum foil passes through the anode roller 501, due to the tip effect, the aluminum atoms at the top are electrolyzed first, and the aluminum atoms lose two electrons and are converted into aluminum ions that enter the electrolyte, thereby corroding micropores 209 at the tip.
[0038] In some embodiments of the present invention, the microstructure on the aluminum foil is obtained by extrusion molding. Specifically, a laser is first used to micro-shape the desired shape of the aluminum foil on a steel roller with a diameter of φ50mm-2000mm and a length of 100mm-2000mm. Two micro-shaped steel rollers are used. The steel rollers after micro-shaping are called forming devices. The forming devices are then installed on a rolling mill. The aluminum foil passes between the forming devices, the gap between the upper and lower forming devices is adjusted, and pressure is applied to the forming device to copy the surface shape of the forming device onto the aluminum foil. After extrusion molding, the micro-shaped aluminum foil of the present invention is obtained.
[0039] In some embodiments of the present invention, in step S2, the electrolyte 507 includes water, Cu S O4 and H2SO4, wherein the concentration of CuSO4 in the electrolyte 507 is 200g / L and the concentration of H2SO4 is 60g / L.
[0040] In some embodiments of the present invention, in step S2, the electrolysis comprises:
[0041] An anode roller 501, a cathode roller 502, a reel 503 and a reel 504 are arranged in the electrolytic cell. One end of the aluminum foil is connected to the reel 503, and the other end is connected to the reel 504 by passing through the anode roller 501. The anode roller 501 is connected to the positive electrode of the power supply, and the cathode roller 502 is connected to the negative electrode of the power supply. -5 A-1.39*10 -5 A current, and the aluminum foil was rolled up at a speed of 2 m / min. Figure 2 The micro-shaped aluminum foil is unwound from the unwinding reel 503, passes around the anode roller 501, and is rolled up on the reel 504 to obtain the microporous aluminum foil 506. The tip of the protrusion 401 of the micro-shaped aluminum foil will be electrolyzed to ionize aluminum ions; the aluminum foil with aluminum ions deposited on the cathode roller 502 is rolled up and recycled by the aluminum foil recycling reel 505.
[0042] The width of the micro-shaped aluminum foil is 300 mm, the thickness is 8 μm, the protrusion spacing D is 140 μm, and the protrusions 401 and the depressions 402 are alternately and equidistantly distributed. According to calculations, when a 10 nm aperture is required on the top of each protrusion 401, the amount of electricity released by 1 m2 of the micro-shaped aluminum foil is 2.78*10 -3 Coulomb, the area of foil flowing through the electrolytic cell in 1S is 0.01m 2 , the amount of electricity that can be released is 2.78*10-5 Coulomb, the electrolysis current is set to 2.78*10 -5 A;
[0043] The width of the micro-shaped aluminum foil is 300mm, the thickness is 8um, the protrusion spacing D is 140um, and the protrusions 401 and the depressions 402 are alternately and equidistantly distributed. After calculation: when it is necessary to shape a 50nm aperture on the top of each protrusion 401, 1m 2 The amount of electricity released by the micro-shaped aluminum foil is 1.39*10 -3 Coulomb, the area of foil flowing through the electrolytic cell in 1S is 0.01m 2 , the amount of electricity that can be released is 1.39*10 -5 Coulomb, the electrolysis current is set to 1.39*10 -5 A;
[0044] The diameter of the micropores 209 of the aluminum foil prepared by the above method is 10-50 nm.
[0045] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0046] Example 1
[0047] Select the micro-shaped aluminum foil substrate: width 300mm, convex height B12um, convex diameter C 48um, convex spacing D140um, electrolyze in the electrolytic cell, substrate winding speed 2m / min, electrolysis current 1.39*10 -4 A.
[0048] Example 2
[0049] Select micro-shaped aluminum foil substrate: width 300mm, convex height B12um, convex diameter C 36um, convex spacing D140um, electrolyze in the electrolytic cell, substrate winding speed 2m / min, electrolysis current 1.39*10 -4 A.
[0050] Example 3
[0051] Select micro-shaped aluminum foil substrate: width 300mm, convex height B12um, convex diameter C 24um, convex spacing D140um, electrolyze in the electrolytic cell, substrate winding speed 2m / min, electrolysis current 1.39*10 -4 A.
[0052] Embodiment 4:
[0053] Select the micro-shaped aluminum foil substrate: width 300mm, convex 401 height B12um, convex diameter C12um, convex spacing D140um, electrolysis in the electrolytic cell, substrate winding speed 2m / min, electrolysis current 1.39*10 -4 A.
[0054] Embodiment 5:
[0055] Select micro-shaped aluminum foil substrate: width 300mm, convex height B12um, convex diameter C 6um, convex spacing D140um, electrolyze in the electrolytic cell, substrate winding speed 2m / min, electrolysis current 1.39*10 -5 A.
[0056] Comparative Example 1:
[0057] Select the micro-shaped aluminum foil substrate: width 300mm, convex height B12um, convex diameter C120um, convex spacing D400um, electrolyze in the electrolytic cell, substrate winding speed 2m / min, electrolysis current 1.39*10 -4 A.
[0058] In summary, the parameters of the micro-shaped aluminum foils of Examples 1-5 and the comparative example are shown in Table 1 below.
[0059] Table 1 Micro-shaped aluminum foil parameters of Examples 1-5 and Comparative Examples
[0060] serial number Micro-shaped protrusion height / um Micro-shaped raised diameter / um Micro-shaped protrusion height-to-diameter ratio Example 1 12 48 1:4 Example 2 12 36 1:3 Example 3 12 24 1:2 Example 4 12 12 1:1 Example 5 12 6 2:1 Comparative Example 1 12 120 1:10
[0061] Experimental example
[0062] A. Lithium battery electrolyte permeability test
[0063] Use a pipette to suck up the electrolyte of the lithium battery and drop it on the upper surface of the microporous aluminum foil 506, stick a piece of pH test paper on the lower surface of the microporous aluminum foil 506, and observe the color change time of the pH test paper.
[0064] B. Slurry permeability test
[0065] Take 5.1g PVDF and dissolve it in 67.8g NMP, stir for 2h, add 81.6g CNT, stir for 2h, add 500.8g ternary material, add 24.7g NMP, stir for 3h, and prepare positive electrode slurry 300.
[0066] Use a small spoon to transfer 1 spoon of slurry onto the upper surface of the microporous aluminum foil 506, stick a piece of pH test paper on the lower surface of the microporous aluminum foil 506, and observe the color change time of the pH test paper.
[0067] C. Tensile strength test
[0068] Use a sampler to cut a microporous aluminum foil 506 with a length*width of 100*25mm, and conduct a room temperature tensile mechanical properties test. The gauge length is 50mm, the test rate is 5mm / min, and the tensile strength is recorded.
[0069] The results are shown in Table 2
[0070] Table 2 Performance of microporous aluminum foil of Examples 1-5 and Comparative Examples
[0071]
[0072] From the results of Example 1 to Example 5, as the ratio of the protrusion height to the diameter becomes larger, the time for the lithium battery electrolyte to penetrate the microporous aluminum foil 506 becomes shorter and shorter, indicating that the diameter of the micropores 209 becomes larger and larger; the slurry cannot penetrate the microporous aluminum foil; and the tensile strength does not change significantly;
[0073] In comparative example 1, the ratio of the protrusion height to the aperture is too small, the tip effect is not obvious, the micropores are too small, and the microporous aluminum foil does not have the characteristics;
[0074] As attached Figure 6 As shown, the top of the protrusion 401 of the microporous aluminum foil 506 is in a through-hole state, that is, the micropore 209. After the negative electrode material is coated on both sides of the microporous aluminum foil 506, the amount of negative electrode material at D1 and D2 is relatively balanced; the coating amount at D3 and D4 is unbalanced, and the amount of negative electrode material at D3 is more than that at D4. When the battery is charged and discharged, the corresponding negative electrode material at D4 cannot fully absorb the lithium ions migrated from the positive electrode sheet, but the excess lithium ions will pass through the through-hole and recombine with the negative electrode material at the corresponding position of D4; when the positive electrode sheet is unevenly coated, the excess lithium ions will also pass through the through-hole to prevent lithium precipitation.
[0075] When the electrode slurry is unevenly coated on the electrode surface, such as Figure 3 The positive electrode material is coated on both sides of the microporous aluminum foil 506, and the negative electrode material is coated on both sides of the copper foil 202. The positive and negative electrodes are separated by a separator in the middle. In the actual production process, there is an uneven coating phenomenon. Figure 3 It can be seen visually that there is a bulge in the coating on the positive electrode sheet A side 205, which is the pile 208 caused by uneven coating. During charging, when the negative electrode sheet B side 203 cannot provide enough negative electrode material to absorb the lithium ions deintercalated at the corresponding position 208 on the positive electrode sheet A side 205, the lithium ions will pass through the micropores 209 on the aluminum foil and recombine with the negative electrode material corresponding to the positive electrode sheet B side 207.
[0076] In summary, the microporous aluminum foil provided by the present invention has micropores with a diameter of 10-50nm. When the aluminum foil with micropores of this size is coated with electrode slurry, the electrode slurry will not pass through the micropores. However, after it is assembled into a battery and injected with electrolyte, the electrolyte has low viscosity and small surface tension, and can penetrate from the A side of the aluminum foil to the B side of the aluminum foil through the micropores; and the ion diameter is less than 1nm, and the pore size of 10-50nm is sufficient for a large number of ions to pass through at the same time. Applying it in a battery can avoid the formation of dendrites on the electrode, thereby extending the service life of the battery and increasing the number of battery charge and discharge cycles.
[0077] The preparation method provided by the present invention can discharge the aluminum foil with microstructure at the tip under electrolysis, lose aluminum ions, and then form micropores at the protrusions of the aluminum foil, and the pore size of the micropores is controlled to be 10-50nm by controlling the current and electrolysis time. The preparation method is simple and fast, and can quickly obtain microporous aluminum foil.
[0078] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a microporous aluminum foil, characterized in that: The following steps are involved: S1, preparation of aluminum foil with microstructure; S2, preparing an electrolyte, placing the aluminum foil in the electrolyte, and electrolyzing the aluminum foil so that the tip of the raised portion of the microstructure of the aluminum foil discharges, thereby forming micropores.
2. The method for preparing the microporous aluminum foil according to claim 1, characterized in that: The micro-modeling structure includes a plurality of protrusions and recesses, and the plurality of protrusions and the plurality of recesses are alternately and equidistantly distributed.
3. The method for preparing the microporous aluminum foil according to claim 1, characterized in that: The microstructure on the aluminum foil is obtained by extrusion molding.
4. The method for preparing the microporous aluminum foil according to claim 1, characterized in that: In step S2, the electrolyte includes, by mass percentage, 10.74% of ethylene carbonate, 32.24% of dimethyl carbonate, 10.75% of ethyl methyl carbonate, and 46.27% of aluminum hexafluorophosphate.
5. The method for preparing the microporous aluminum foil according to claim 1, characterized in that: In the step S2, the electrolysis comprises: An anode roller, a cathode roller, a reel and a reel are arranged in the electrolytic cell. One end of the aluminum foil is connected to the reel, and the other end is connected to the reel by passing through the anode roller. -5 A-1.39*10 -4 A current, and the aluminum foil was wound up at a winding speed of 2 m / min.
6. A microporous aluminum foil, characterized in that: The microporous aluminum foil is prepared by the method for preparing the microporous aluminum foil according to any one of claims 1 to 5.
7. The microporous aluminum foil according to claim 6, characterized in that: The pore size of the micropores is 10-50 nm.