Application of oxide additive in preparation of AgO polar plate by electrochemical method

By adding oxide additives such as cadmium oxide to the preparation of AgO plates in electrochemical method, the problem of low voltage and insufficient capacity of the zinc-silver oxide plates in the initial loading stage of zinc-silver battery electrochemical method is solved, and the battery performance and capacity are improved effect.

CN119092651APending Publication Date: 2024-12-06GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121807.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Electrochemical preparation of zinc-silver batteries The voltage is low, the activity is low, and the purity and capacity are insufficient, especially at low temperatures, which affect the performance of the battery.

Method used

Add oxide additives such as cadmium oxide, thallium oxide, indium oxide or tellurium oxide to the preparation of AgO plates by electrochemical method, and mixing them with silver powder and carbon materials at high temperature to form a high specific capacity silver oxide plate , improve the electrical performance of the plate.

Benefits of technology

It effectively improves the initial loading voltage and capacity of the silver oxide plate, forms a stable crystal structure with high specific capacity, enhances the electrode reactive active site, and improves battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092651A_ABST
    Figure CN119092651A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of positive electrode active materials of zinc-silver batteries, and particularly relates to application of an oxide additive in preparation of an AgO polar plate by an electrochemical method, the oxide additive is any one or a mixture of more of cadmium oxide, thallium oxide, indium oxide and tellurium oxide, the oxide is added in the preparation process of the silver oxide by the electrochemical method, so that the voltage and the capacity at the initial loading stage of the pole plate are effectively improved, and the prepared silver oxide pole plate has the characteristic of high specific volume.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of positive electrode active materials for zinc-silver batteries, and specifically relates to application of an oxide additive in preparing AgO pole plates by an electrochemical method. Background Art

[0002] The positive active material of the zinc-silver battery is AgO, and its preparation methods are mainly electrochemical methods and chemical oxidation methods. In order to increase the capacity of zinc-silver batteries, the main research focuses on the chemical oxidation method. AgO is prepared by using different types of oxidants, the preparation process is studied, the purity of AgO is improved, and AgO is improved by metal additives and surface treatment to improve the electrical properties of the AgO plate. However, the chemical oxidation method has high requirements on equipment and test conditions. It is more suitable for laboratory preparation methods and is not suitable for large-scale standardized production.

[0003] The electrochemical preparation method has a simple process, low equipment requirements, and is suitable for large-scale production. Patent publication number CN105734643A discloses an in-situ electrochemical preparation method for a nano silver oxide film, comprising the following steps: (1) washing a silver substrate with distilled water and anhydrous ethanol respectively, and blowing its surface dry with nitrogen; (2) adding sodium hydroxide reagent to distilled water, stirring to dissolve the solid, forming a sodium hydroxide solution, and making the molar concentration of the solution range between 0.1 mol / L and 2 mol / L; (3) connecting the three holes of the electrolytic cell to the silver substrate, the saturated calomel electrode reference electrode, and the platinum mesh counter electrode respectively, and the reference electrode is located between the silver substrate and the counter electrode, the silver substrate is the working electrode, and the three electrodes are connected to the three electrodes corresponding to the electrochemical workstation respectively; (4) setting the scanning speed, starting potential, intermediate potential, and end potential during the electrochemical polarization process, placing the solution prepared in step (2) into the electrolytic cell, and electrochemically polarizing the silver substrate to obtain a nano silver oxide film. After the electrochemical polarization process completes at least one cyclic voltammetric polarization, the forward scanning continues from the starting potential, and the polarization stops after reaching the intermediate potential. The nano silver oxide prepared directly on the silver substrate in this patent can be used for electronic components, button batteries, purifiers, and chemical catalyst devices, but the effect of this patent on improving the electrical properties of silver oxide is unknown.

[0004] At present, the electrochemical method for preparing silver oxide electrodes mostly uses carbon materials as additives to reduce the internal resistance of the AgO plate and improve its electrical performance. Graphite is cheap and is often added to silver powder as a conductive agent. Silver powder and carbon materials are mixed into mixed silver powder, and the mixed silver powder is pressed into a silver electrode by a molding method. The silver electrode is charged, rinsed and dried to obtain a silver oxide plate.

[0005] Zinc-silver batteries have high requirements for operating temperature. The silver oxide plates prepared by electrochemical methods have low activity and a voltage drop phenomenon at the initial stage of loading, which affects the performance of the battery, especially at low temperatures. Compared with chemical synthesis methods, the silver oxide plates prepared by electrochemical methods have lower purity and correspondingly lower capacity. The present invention aims to increase the initial voltage of loading and increase the capacity. Summary of the invention

[0006] In view of the deficiencies of the prior art, the present invention proposes an application of an oxide additive in preparing AgO pole plates by electrochemical method.

[0007] This is achieved specifically through the following technical solutions:

[0008] The invention discloses an application of an oxide additive in preparing an AgO plate by an electrochemical method. The oxide additive is a mixture of any one or more of cadmium oxide, thallium oxide, indium oxide and tellurium oxide.

[0009] The application comprises the following steps:

[0010] 1) Mixing powder: uniformly mixing silver powder, carbon material and oxide additive to obtain mixed silver powder;

[0011] 2) Pressing: Put a skeleton in a mold, and spread the mixed silver powder on the skeleton in batches, press and shape it, and then sinter it at high temperature to obtain a silver plate with a thickness of 0.3mm to 0.7mm;

[0012] 3) Formation: Under the conditions of formation temperature of 30-40°C and electrolyte concentration of 1.0g / ml~1.5g / ml, first charge at a constant current of 2A~12A for 10h~24h, then reduce the current to 1A~6A and charge for 10h~24h. After charging, put it into running deionized water for cleaning for 20h and dry it to obtain silver oxide plates.

[0013] The silver content in the silver powder is greater than 97.5%.

[0014] The mass ratio of the silver powder, the carbon material and the oxide additive is 98-99.9:1:0.05-1.

[0015] The pressing pressure is 2Mpa to 30Mpa.

[0016] The high temperature sintering temperature is 350° C. to 500° C., and the time is 10 min to 15 min.

[0017] Beneficial effects:

[0018] The invention adds oxides during the preparation process of silver oxide by the electrochemical method, effectively improving the voltage and capacity of the plate at the initial stage of loading, so that the prepared silver oxide plate has the characteristic of high specific capacity.

[0019] Cadmium oxide, thallium oxide, and indium oxide have similar metal ions to those of silver oxide and have strong binding ability with oxygen ions. Tellurium and oxygen in tellurium oxide belong to the same group of elements and can fill oxygen defects when silver oxide crystals are formed. The addition of a third element can increase the binding force between silver and oxygen and form a stable crystal structure.

[0020] The silver oxide plate with oxide added has a loose surface and a flaky multi-gap structure that is conducive to the wetting of the plate by the electrolyte and can provide more active sites for the electrode reaction. The silver oxide plate without oxide added has agglomeration on its surface and the crystals are stacked unevenly, which is not conducive to the wetting of the plate by the electrolyte. The SEM images of the silver oxide plate without oxide added and the silver oxide plate with oxide added are shown in Figure 1 and Figure 2, respectively. Figure 1 , Figure 2 shown.

[0021] Silver powder is the main active substance, and the amount of silver powder directly determines the performance of the plate. Carbon materials can reduce the internal resistance of the plate, but if the content is too high, the active substances will be reduced and the plate capacity will be reduced. If the oxide content is too high, the internal resistance of the plate will increase. The proportion of the quality of various powders should be strictly controlled when mixing powders. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM image of the silver oxide plate without adding oxide;

[0023] Figure 2 This is the SEM image of the silver oxide plate with added oxide;

[0024] Figure 3 This is a comparison chart of the initial loading voltage of the zinc-silver battery of the experimental group 1 and the control group 1;

[0025] Figure 4 This is a comparison chart of the discharge time of zinc-silver batteries in the experimental group 1 and the control group 1. DETAILED DESCRIPTION

[0026] The specific embodiments of the present invention are further described in detail below, but the present invention is not limited to these embodiments, and any improvement or substitution based on the basic spirit of the present embodiment still falls within the scope of protection required by the claims of the present invention.

[0027] Example 1

[0028] An application of an oxide additive in the electrochemical preparation of an AgO plate, the application steps comprising:

[0029] 1) Mixing powder: mixing silver powder, graphite powder and oxide additive in a mass ratio of 99.85:1:0.15 to obtain mixed silver powder; the oxide additive is TeO2;

[0030] 2) Pressing: Put a skeleton in the mold, and spread the mixed silver powder on the skeleton in batches, press it under a pressure of 15Mpa, and sinter it at a high temperature of 400℃ for 15min to obtain a silver plate with a thickness of 0.35mm;

[0031] 3) Formation: Under the conditions of formation temperature of 30°C and electrolyte concentration of 1.3g / ml, charge at a constant current of 10A for 5h, then reduce the current to 2.5A and charge for 15h. After charging, wash in running deionized water for 20h and dry to obtain silver oxide plates.

[0032] Example 2

[0033] An application of an oxide additive in the electrochemical preparation of an AgO plate, the application steps comprising:

[0034] 1) Mixing powder: silver powder, graphene and oxide additive are mixed evenly in a mass ratio of 98.5:1:0.5 to obtain mixed silver powder; the oxide additive is 0.25% of CdO and In2O3 respectively;

[0035] 2) Pressing: Put a skeleton in the mold, and spread the mixed silver powder on the skeleton in batches, press it into shape under a pressure of 15Mpa, and sinter it at a high temperature of 400℃ for 10min to obtain a silver plate with a thickness of 0.35mm;

[0036] 3) Formation: Under the conditions of formation temperature of 30°C and electrolyte concentration of 1.1g / ml, charge at a constant current of 10A for 18h, then reduce the current to 5A and charge for 12h. After charging, wash in running deionized water for 20h and dry to obtain silver oxide plates.

[0037] Example 3

[0038] An application of an oxide additive in the electrochemical preparation of an AgO plate, the application steps comprising:

[0039] 1) Mixing powder: mixing silver powder, graphite powder and oxide additive in a mass ratio of 99:1:1 to obtain mixed silver powder; the oxide additive is CdO and Tl2O3, each 0.5%;

[0040] 2) Pressing: Put a skeleton in the mold, and spread the mixed silver powder on the skeleton in batches. After pressing and molding under a pressure of 22Mpa, sinter at a high temperature of 450°C for 12 minutes to obtain a silver plate with a thickness of 0.45mm;

[0041] 3) Formation: Under the conditions of formation temperature of 35°C and electrolyte concentration of 1.3g / ml, charge at a constant current of 9A for 24h, then reduce the current to 5A and charge for 16h. After charging, wash in running deionized water for 20h and dry to obtain silver oxide plates.

[0042] Example 4

[0043] An application of an oxide additive in the electrochemical preparation of an AgO plate, the application steps comprising:

[0044] 1) Mixing powder: mixing silver powder, carbon material and oxide additive in a mass ratio of 99.5:1:0.5 to obtain mixed silver powder; the oxide additive is In2O3;

[0045] 2) Pressing: Put a skeleton in the mold, and spread the mixed silver powder on the skeleton in batches. After pressing and molding under a pressure of 10Mpa, sinter at 350℃ for 15min to obtain a silver plate with a thickness of 0.56mm.

[0046] 3) Formation: Under the conditions of formation temperature of 40°C and electrolyte concentration of 1.2g / ml, charge at a constant current of 16A for 18h, then reduce the current to 5A and charge for 10h. After charging, wash in running deionized water for 20h and dry to obtain silver oxide plates.

[0047] Example 5

[0048] An application of an oxide additive in the electrochemical preparation of an AgO plate, the application steps comprising:

[0049] 1) Mixing powder: mixing silver powder, carbon material and oxide additive in a mass ratio of 99.3:1:0.7 to obtain mixed silver powder; the oxide additive is CdO, In2O3 and TeO2, accounting for 0.2%, 0.25% and 0.25% respectively;

[0050] 2) Pressing: Put a skeleton in the mold, and spread the mixed silver powder on the skeleton in batches. After pressing and molding under a pressure of 6Mpa, sinter at a high temperature of 480°C for 10 minutes to obtain a silver plate with a thickness of 0.65mm;

[0051] 3) Formation: Under the conditions of formation temperature of 40°C and electrolyte concentration of 1.5g / ml, charge at a constant current of 12A for 10h, then reduce the current to 6A and charge for 18h. After charging, wash in running deionized water for 20h and dry to obtain silver oxide plates.

[0052] Comparative Example 1

[0053] Based on Example 1, the difference from Example 1 is that TeO2 is not added.

[0054] Test Example 1

[0055] The 7 silver oxide electrodes prepared in Example 1 and Comparative Example 1, 6 zinc plates, 22 mL potassium hydroxide electrolyte and a layer of triacetate cellulose membrane were assembled into a zinc-silver single battery. The single discharge test of the zinc-silver battery was counted as test group 1 and control group 1 respectively. The timing started when the electrolyte was added, and the load test was carried out after 60 seconds of no-load. The initial voltage of test group 1 was 1.475V, which was increased by about 10%. Figure 3 Adding oxide can effectively increase the capacity of the battery by 10%, see Figure 4 .

Claims

1. An application of an oxide additive in the electrochemical preparation of AgO plates, characterized in that: The oxide additive is a mixture of any one or more of cadmium oxide, thallium oxide, indium oxide and tellurium oxide.

2. The use according to claim 1, characterized in that: The steps of preparing the AgO plate by electrochemical method include: 1) Mixing powder: uniformly mixing silver powder, carbon material and oxide additive to obtain mixed silver powder; 2) Pressing: Put a skeleton in a mold, and spread the mixed silver powder on the skeleton in batches, press and shape it, and then sinter it at high temperature to obtain a silver plate with a thickness of 0.3mm to 0.7mm; 3) Formation: Under the conditions of formation temperature of 30-40°C and electrolyte concentration of 1.0g / ml~1.5g / ml, first charge at a constant current of 2A~12A for 10h~24h, then reduce the current to 1A~6A and charge for 10h~24h. After charging, put it into running deionized water for cleaning for 20h and dry it to obtain silver oxide plates.

3. The use according to claim 2, characterized in that: The silver content in the silver powder is greater than 97.5%.

4. The use according to claim 2, characterized in that: The mass ratio of the silver powder, the carbon material and the oxide additive is 98-99.9:1:0.05-1.

5. The use according to claim 2, characterized in that: The pressing pressure is 2Mpa to 30Mpa.