Low-nickel high-capacity sodium ion battery positive electrode material, preparation method and sodium ion battery
By preparing the positive electrode material of low nickel and high capacity of sodium ion batteries, the cost and performance problems caused by the high nickel content in sodium ion batteries are solved, and higher gram capacity and cycling performance are achieved, which promotes the market application of sodium ion batteries.
Patent Information
- Application Number
- CN202410965802.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-12-06
AI Technical Summary
The high nickel content in the positive electrode materials of existing sodium ion batteries leads to high costs, limited capacity and poor circulation performance, which cannot promote the large-scale market application of sodium ion batteries.
The chemical formula of the cathode material of low nickel and high capacity sodium ion battery is Nax (NiaFebMncZndLie) 1-fTMfO2, and the layered structural material with irregular block morphology is prepared by co-precipitation method to reduce the nickel content and improve the capacity and circulation performance.
It reduces material costs, improves discharge g capacity and cycling performance, avoids lattice structure collapse under high SOC, and enhances structural stability and voltage retention.
Smart Images

Figure CN119092657A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a low-nickel and high-capacity sodium ion battery positive electrode material, a preparation method and a sodium ion battery. Background Art
[0002] In recent years, the popularity of new energy vehicles has driven the rapid development of the lithium-ion battery industry. The commercialization of lithium-ion batteries can be traced back to the 1990s. After years of research, lithium-ion batteries have a mature battery technology route. However, with the scarcity of lithium resources and uneven geographical distribution, the price of lithium resources has risen, increasing the manufacturing cost of lithium-ion batteries, seriously restricting its further development. Sodium and lithium belong to the first main group and have similar physical and chemical properties. Sodium ranks sixth in crustal abundance, and its resources are evenly distributed and low in price. It is expected to be widely used in large-scale energy storage and low-speed electric vehicles.
[0003] Sodium-ion batteries are mainly composed of positive electrodes, negative electrodes, electrolytes, diaphragms and auxiliary components. Among them, the positive electrode material is one of the key factors affecting the performance of sodium-ion batteries. The current mainstream positive electrode materials for sodium-ion batteries include layered transition metal oxides, Prussian blue analogs, and polyanion positive electrode materials. Among them, layered transition metal oxide positive electrodes have attracted more and more attention due to their high redox potential, high specific capacity, and low price. At present, the mainstream layered oxide positive electrode material for sodium-ion batteries on the market is the NFM111 system, which has the following problems: First, the relatively high nickel content leads to generally high material costs; second, the NFM111 system materials currently sold on the market can only exert a discharge capacity of 130 to 135 mAh / g in the voltage range of 2.0 to 4.0 V, and when the charging cut-off voltage is 4.1 V and above, an irreversible phase change of P3-O′3 occurs, which seriously affects the cycle performance of the material. Therefore, this system material has no obvious advantages over mature lithium iron phosphate materials and cannot further promote the large-scale market application of sodium-ion batteries. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a low-nickel and high-capacity sodium ion battery positive electrode material, a preparation method and a sodium ion battery which can effectively reduce the nickel content, reduce the material cost, and improve the gram capacity and cycle performance.
[0005] One of the purposes of the present invention is to provide a low-nickel high-capacity sodium ion battery positive electrode material, characterized in that: the chemical formula of the sodium ion battery positive electrode material is Na x (Ni a Fe b Mn c Zn d Lie ) 1-f TM f O2, where 0.5 ≤ x ≤ 1.1, 0 < a < 0.3, 0.2 ≤ b ≤ 0.5, 0.2 ≤ c ≤ 0.5, 0 < d ≤ 0.1, 0 < e ≤ 0.1, 0 ≤ f ≤ 0.1, and a + b + c + d + e = 1. The positive electrode material of this sodium-ion battery has an irregular block morphology and a layered structure.
[0006] The TM includes at least one of the elements Ti, V, Cr, Co, Cu, K, Si, Ta, La, Nb, Y, Zr, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F.
[0007] Preferably, the TM is Zr, Ti, Cu, Al, Mg, Co, and F.
[0008] The chemical formula of the positive electrode material of the sodium-ion battery is Na x (Ni a Fe b Mn c Zn d Li e ) 1-f TM f O2, equivalent to Na x Ni a(1-f) Fe b(1-f) Mn c(1-f) Zn d(1-f) Li e(1-f) TM f O2; The positive electrode material of this sodium-ion battery has an irregular block morphology, a layered structure, and the specific surface area of the positive electrode material of the sodium-ion battery is less than 0.8 m 2 / g;
[0009] And / or, the median particle size D50 of the positive electrode material of the sodium-ion battery is 3.0 - 12.0 μm.
[0010] The second object of the present invention is to provide a preparation method of the above-mentioned low-nickel and high-capacity positive electrode material for a sodium-ion battery, which is characterized in that the method includes the following steps:
[0011] Step 1: Prepare a low-nickel precursor by a co-precipitation method; the chemical formula of the low-nickel precursor is Ni a Fe b Mn c Zn d Li e CO3, Ni a Fe b Mn c Zn d Li e (OH)2 or Nia Fe b Mn c Zn d Li e C2O4, where 0 < a < 0.3, 0.2 ≤ b ≤ 0.5, 0.2 ≤ c ≤ 0.5, 0 < d ≤ 0.1, 0 < e ≤ 0.1, and a + b + c + d + e = 1;
[0012] Step 2: Mix the low-nickel precursor, dopant, and sodium source compound in a stoichiometric ratio, perform drying treatment, then carry out high-temperature sintering. After cooling to room temperature, perform crushing, grinding, and sieving treatments to obtain a low-nickel high-capacity cathode material for sodium-ion batteries; among them, except for the sodium element ratio in the low-nickel high-capacity cathode material for sodium-ion batteries being added according to 0.8 - 1.1 times the theoretical sodium ratio, the usage amounts of other elements are calculated according to the molar ratios of the elements in the chemical formula; the sintering temperature is 850 - 1100 °C, the heat preservation time is 6 - 20 h, the heating rate is 1 - 10 °C / min, and the sintering atmosphere is air or oxygen.
[0013] The chemical formula of the low-nickel precursor is Ni a Fe b Mn c Zn d Li e CO3, Ni a Fe b Mn c Zn d Li e (OH)2 or Ni a Fe b Mn c Zn d Li e C2O4, where 0 < a < 0.3, 0.2 ≤ b ≤ 0.5, 0.2 ≤ c ≤ 0.5, 0 < d ≤ 0.1, 0 < e ≤ 0.1, and a + b + c + d + e = 1.
[0014] The dopant includes one or more compounds containing elements such as Ti, V, Cr, Co, Cu, K, Si, Ta, La, Nb, Y, Zr, Mg, Al, Sn, Ru, Sr, W, Mo, B, F.
[0015] Preferably, the dopant is a compound containing elements such as Zr, Ti, Cu, Co, Mg, Al, F.
[0016] The sodium source compound in Step 2 includes at least one of Na2CO3, NaHCO3, NaOH, Na2O, CH3COONa.
[0017] In Step 1, the preparation of the low-nickel precursor is carried out according to the following steps:
[0018] a. First, prepare sodium hydroxide solution (8 mol / L), lithium hydroxide solution (5 mol / L), ammonia solution (2 mol / L), hydrogen peroxide solution (20 wt%), nickel sulfate, ferrous iron, manganese, zinc mixed salt solution (total metal ion molar concentration 2 mol / L, wherein Ni:Fe:Mn:Zn=a:b:c:d);
[0019] b. Add pure water to the reactor, set the stirring rate to 800 rpm / min and heat to 60°C, while introducing high-purity nitrogen to remove dissolved oxygen in the pure water;
[0020] c. Add the prepared sodium hydroxide solution into the reactor to adjust the pH value to 10.5-11.5;
[0021] d. Simultaneously introduce the prepared ammonia solution, sodium hydroxide solution and mixed salt solution into the reactor, and simultaneously introduce oxygen and nitrogen into the mixed solution. The flow rate of the mixed salt solution is 6-10 L / h, the flow rate of the ammonia solution is 1-1.5 L / h, the flow rate of the sodium hydroxide solution is 1-3 L / h, the flow rate of oxygen is 1-5 L / min, and the flow rate of the inert gas is 15-50 L / min. The pH value is controlled at 10.5-11.5, the coprecipitation reaction time is 10-15 min, and the stirring rate is maintained at 800 rpm / min during the reaction;
[0022] e. Keep the stirring rate, the flow rate of the salt solution and the flow rate of the ammonia solution unchanged, adjust the flow rate of the sodium hydroxide solution, lower the pH value to 10±0.15, and coprecipitate to the target particle size D50 of the precursor particles = 2-8 μm;
[0023] f. After the precursor particles reach the target particle size, the reactor is heated to 70-90° C. in a water bath, and sodium hydroxide solution is continuously introduced until the pH value is 12-13. Hydrogen peroxide solution and lithium hydroxide solution are added to the reactor. The amount of lithium hydroxide solution introduced is based on the molar ratio of the metal elements in the reactor of Ni:Fe:Mn:Zn:Li=a:b:c:d:e, and the amount of hydrogen peroxide solution introduced is based on a mass ratio of 2:1 to the metal elements in the reactor.
[0024] g. The mixture in the reaction kettle was passed into an aging kettle, the temperature was controlled to be 60°C, the stirring rate was adjusted to 400 rpm / min, and the aging time was 10 hours. After aging, the mixture was washed and dried to obtain a precursor of the positive electrode material for a sodium ion battery.
[0025] The third object of the present invention is to provide a method for preparing the low-nickel and high-capacity sodium ion battery positive electrode material, characterized in that the method comprises the following steps:
[0026] The transition metal or non-metallic element compound and the sodium source compound are mixed according to a stoichiometric ratio, dried, and tableted, and then sintered at high temperature. After cooling to room temperature, they are crushed, ground, and sieved to obtain a low-nickel and high-capacity sodium ion battery positive electrode material; wherein, in the low-nickel and high-capacity sodium ion battery positive electrode material, except for the Na element added according to the ratio of 0.8 to 1.1 times the theoretical sodium ratio, the usage of other elements is calculated according to the molar ratio of each element in the chemical formula; the sintering temperature is 850 to 1100°C, the insulation time is 6 to 20h, the heating rate is 1 to 10°C / min, and the sintering atmosphere is air or oxygen.
[0027] The transition metal or non-metal element compound includes at least one of the compounds containing Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Si, Ta, La, Nb, Y, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F elements.
[0028] Preferably, the transition metal or non-metal element compound is a compound containing Ni, Fe, Mn, Zn, Li, Zr, Ti, Cu, Co, Mg, Al, and F elements.
[0029] The sodium source compound includes at least one of Na2CO3, NaHCO3, NaOH, Na2O, and CH3COONa.
[0030] A fourth object of the present invention is to provide a sodium ion battery, characterized in that the positive electrode material of the sodium ion battery is a low-nickel, high-capacity sodium ion battery positive electrode material or a low-nickel, high-capacity sodium ion battery positive electrode material prepared by the above preparation method.
[0031] The beneficial effects of the present invention are:
[0032] 1. This material is prepared by preparing a corresponding low-nickel precursor and mixing it with a dopant-sintering or by a high-temperature solid phase method, which reduces the nickel content in the material components. The raw material cost is lower than that of the NFM111 system, and the lower the nickel content, the lower the cost;
[0033] 2. Zn can induce high potential (about 4.0V, different nickel-containing material systems have different potentials) of Ni 3+ / Ni 4+ or 2- The redox reaction is advanced, so that a higher specific capacity can be obtained at a relatively low upper cut-off voltage, so as to prevent the upper cut-off voltage from being passively increased to achieve a high specific capacity, thereby causing the lattice structure of the material to collapse at a high SOC;
[0034] 3. Zn can reduce Fe in the cycle 3+Irreversible migration to the Na layer improves the voltage drop during cycling;
[0035] 4. Low-valence Zn can control the valence of Mn to a level close to +4, thereby reducing the 3+ The induced Jahn-Teller effect leads to lattice distortion, which improves the cycling performance of the material;
[0036] 5. A small amount of Zn migrates to the Na layer during the cycle, reducing the Na + The lattice changes during the extraction / insertion process improve the structural stability;
[0037] 6. During the charge and discharge process, the Li element undergoes reversible migration from the transition metal layer to the Na layer. After the migration, vacancies are generated in the transition metal layer, forming a Li(Na)-O-□TM or □Na-O-□TM configuration, activating the anion redox reaction and providing more gram capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Ni in Example 1 0.20 Fe 0.35 Mn 0.35 Zn 0.07 Li 0.03 SEM image of (OH)2 precursor sample;
[0039] Figure 2 is Na in Example 1 0.98 Ni 0.20 Fe 0.345 Mn 0.35 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0040] Figure 3 is Na in Example 2 0.98 Ni 0.20 Fe 0.345 Mn 0.35 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0041] Figure 4 is Na in Example 3 1.06 Ni 0.25 Fe 0.325 Mn 0.32 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0042] Figure 5 is Na in Example 4 0.91 Ni 0.15 Fe 0.375 Mn 0.37 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0043] Figure 6 is Na in Example 5 0.83 Ni 0.10 Fe 0.395 Mn 0.40 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0044] Figure 7 is Na in Example 6 1.06 Ni 0.25 Fe 0.325 Mn 0.32 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0045] Figure 8 is Na in Example 7 0.91 Ni 0.15 Fe 0.375 Mn 0.37 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0046] Fig. 9 is Na in Example 8 0.83 Ni 0.10 Fe 0.395 Mn 0.40 Zn 0.07 Li 0.03 Al 0.005 SEM image of O2 sample;
[0047] Fig.10 It is a comparison diagram of the charge and discharge curves of Example 1 and Example 2;
[0048] Fig.11 It is a comparison diagram of the charge and discharge curves of Example 3 and Example 6;
[0049] Fig.12 It is a comparison diagram of the charge and discharge curves of Example 4 and Example 7;
[0050] Fig.13It is a comparison diagram of the charge and discharge curves of Example 5 and Example 8;
[0051] Fig.14 It is a comparison diagram of the charge and discharge curves of Examples 1, 9 and 10;
[0052] Fig.15 It is a comparison chart of the cyclic discharge performance of Examples 1 to 8;
[0053] Fig.16 1 is a comparison chart of the cyclic discharge performance of Examples 1, 9 and 10;
[0054] Fig.17 It is a comparison diagram of the charge and discharge curves of Example 1 and Comparative Examples 1 to 3;
[0055] Fig.18 It is a comparison diagram of the charge and discharge curves of Example 1 and Comparative Example 4;
[0056] Fig.19 It is a comparison chart of the cyclic discharge performance of Example 1 and Comparative Examples 1-4. DETAILED DESCRIPTION
[0057] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0058] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0059] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0060] In the following examples of the present application, important reagents are purchased from Aladdin Chemical Reagent Network, and the reagent purity is analytical grade or battery grade. All performance indicators of the product are strictly measured using precision instruments and standard test methods. The product microstructure and element distribution are analyzed using a field emission scanning electron microscope (SEM) of Zeiss Sigma 300. The sodium ion battery is charged and discharged using a new battery test cabinet, and the capacity, median voltage, etc. of different cycle times are read from the charge and discharge curves.
[0061] Example 1
[0062] In this embodiment, a low-nickel high-capacity sodium ion battery positive electrode material is prepared by preparing a corresponding low-nickel precursor and mixing it with a dopant and sintering it, specifically according to the following steps:
[0063] Step 1: Prepare a low-nickel precursor by coprecipitation method; the chemical formula of the low-nickel precursor is Ni 0.20 Fe 0.35 Mn 0.35 Zn 0.07 Li 0.03 (OH)2;
[0064] Step 2: Mix a low-nickel precursor, a dopant and a sodium source compound according to a stoichiometric ratio, dry the mixture and then sinter at a high temperature. After cooling to room temperature, crush, grind and sieve the mixture to obtain a low-nickel and high-capacity sodium ion battery positive electrode material. In the low-nickel and high-capacity sodium ion battery positive electrode material, except for the addition of Na element according to 1.03 times the theoretical sodium ratio, the amounts of other elements are calculated according to the molar ratio of each element in the chemical formula. The sintering temperature is 1020° C., the holding time is 12 h, the heating rate is 2° C. / min, and the sintering atmosphere is air.
[0065] Specifically, the preparation of the low nickel precursor in step 1 is carried out according to the following steps:
[0066] a. First, prepare sodium hydroxide solution (8 mol / L), lithium hydroxide solution (5 mol / L), ammonia solution (2 mol / L), hydrogen peroxide solution (20 wt%), nickel sulfate, ferrous iron, manganese, zinc mixed salt solution (total metal ion molar concentration 2 mol / L, wherein Ni:Fe:Mn:Zn=20:35:35:7) respectively;
[0067] b. Add pure water to the reactor, set the stirring rate to 800 rpm / min and heat to 60°C, while introducing high-purity nitrogen to remove dissolved oxygen in the pure water;
[0068] c. Add the prepared sodium hydroxide solution into the reactor to adjust the pH value to 11;
[0069] d. Simultaneously introduce the prepared ammonia solution, sodium hydroxide solution and mixed salt solution into the reactor, and simultaneously introduce oxygen and nitrogen into the mixed solution. The flow rate of the mixed salt solution is 8 L / h, the flow rate of the ammonia solution is 1 L / h, the flow rate of the sodium hydroxide solution is 2 L / h, the flow rate of the oxygen is 3 L / min, and the flow rate of the inert gas is 30 L / min. The pH value is controlled at 11, the coprecipitation reaction time is 15 min, and the stirring rate is maintained at 800 rpm / min during the reaction;
[0070] e. Keep the stirring rate, the flow rate of the salt solution and the flow rate of the ammonia solution unchanged, adjust the flow rate of the sodium hydroxide solution, lower the pH value to 10±0.15, and coprecipitate to the target particle size D50 of the precursor particles = 5±2.0 μm;
[0071] f. After the precursor particles reach the target particle size, the reactor is heated to 80° C. in a water bath, and sodium hydroxide solution is continuously introduced until the pH value reaches 12. Hydrogen peroxide solution and lithium hydroxide solution are added to the reactor. The amount of lithium hydroxide solution introduced is according to the molar ratio of the metal elements in the reactor of Ni:Fe:Mn:Zn:Li=20:35:35:7:3, and the amount of hydrogen peroxide solution introduced is according to the mass ratio of the metal elements in the reactor of 2:1.
[0072] g. The mixture in the reaction kettle was passed into the aging kettle, the temperature was controlled at 60°C, the stirring rate was adjusted to 400 rpm / min, and the aging time was 10 hours. After aging, washing and drying were performed to obtain a precursor of the positive electrode material for a sodium ion battery. The corresponding microscopic morphology is as follows: Figure 1 shown.
[0073] The chemical formula of the product prepared in this example is Na 0.98 Ni 0.20 Fe 0.345 Mn 0.35 Zn 0.07 Li 0.03 Al 0.005 O2, SEM analysis of the product, from Figure 2 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 1 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.53 m 2 / g, the median particle size D50 of the sodium ion battery positive electrode material is 5.61μm, and Li(Na)-O-□TM or □Na-O-□TM configuration (□ represents vacancies) can be formed during the charge and discharge process, which activates the anion redox reaction and provides more gram capacity.
[0074] The low-nickel high-capacity sodium ion battery positive electrode material prepared in this embodiment is used as the positive electrode, the metal sodium sheet is used as the negative electrode, the glass fiber membrane is used as the separator, and the NaPF6 / propylene carbonate mixed solution is used as the electrolyte. A sodium ion battery is assembled and a charge and discharge test is performed. The current density is 15mA / g and the voltage range is 2-4V. The charge and discharge curve is as shown in FIG. Fig.10 As shown, the discharge capacity is 152.05 mAh / g, the 5C rate discharge capacity retention rate is 74.96%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 95.23%. Fig.15 .
[0075] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0076] Example 2
[0077] In this embodiment, a low-nickel and high-capacity sodium ion battery positive electrode material is prepared by a high-temperature solid phase method, which is specifically carried out in the following steps:
[0078] The oxides, hydroxides or carbonates containing nickel, iron, manganese, zinc, lithium and aluminum elements are mixed with the sodium source compound Na2CO3 in a stoichiometric ratio, dried, pressed into tablets, and then sintered at high temperature. After cooling to room temperature, they are crushed, ground and sieved to obtain a low-nickel and high-capacity sodium ion battery positive electrode material; wherein, in the low-nickel and high-capacity sodium ion battery positive electrode material, except for the Na element added according to 1.03 times the theoretical sodium ratio, the usage of other elements is calculated according to the molar ratio of each element in the chemical formula; the sintering temperature is 1020°C, the insulation time is 12h, the heating rate is 2°C / min, and the sintering atmosphere is air.
[0079] The chemical formula of the product prepared in this example is Na 0.98 Ni 0.20 Fe 0.345 Mn 0.35 Zn 0.07 Li 0.03 Al 0.005 O2, SEM analysis of the product, from Figure 3 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 2 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.56 m 2 / g, the median particle size D50 of the sodium ion battery positive electrode material is 5.67μm, and Li(Na)-O-□TM or □Na-O-□TM configuration (□ represents vacancies) can be formed during the charge and discharge process, which activates the anion redox reaction and provides more gram capacity.
[0080] According to the method of Example 1, the sodium ion battery prepared in this example was subjected to charge and discharge tests at a current density of 15 mA / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.10 As shown, the discharge capacity is 150.35 mAh / g, the 5C rate discharge capacity retention rate is 74.32%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 95.08%. Fig.15 .
[0081] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0082] Example 3
[0083] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the low-nickel precursor prepared in step 1 is different. The chemical formula of the low-nickel precursor in this embodiment is Ni 0.25 Fe 0.33 Mn 0.32 Zn 0.07 Li 0.03 (OH)2. The other process conditions are the same.
[0084] The product prepared in this example has the molecular formula of Na 1.06 Ni 0.25 Fe 0.325 Mn 0.32 Zn 0.07 Li 0.03 Al 0.005 O2, SEM analysis was performed, from Figure 4 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 3 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.46 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 7.67μm.
[0085] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.11 As shown, the discharge capacity is 151.16 mAh / g, the 5C rate discharge capacity retention rate is 71.32%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 94.68%. Fig.15 .
[0086] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0087] Example 4
[0088] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the low-nickel precursor prepared in step 1 is different. The chemical formula of the low-nickel precursor in this embodiment is Ni 0.15 Fe 0.38 Mn 0.37 Zn 0.07 Li 0.03 (OH)2. The other process conditions are the same.
[0089] The product prepared in this example has the molecular formula of Na 0.91 Ni 0.15 Fe 0.375 Mn 0.37 Zn 0.07 Li 0.03 Al 0.005 O2, SEM analysis was performed on it, from Figure 5 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 4 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.51 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 6.70 μm.
[0090] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.12 As shown, the discharge capacity is 140.71 mAh / g, the 5C rate discharge capacity retention rate is 76.01%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 95.66%. Fig.15 .
[0091] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0092] Example 5
[0093] The preparation process of this embodiment is basically the same as that of embodiment 1, except that the low-nickel precursor prepared in step 1 is different. The chemical formula of the low-nickel precursor in this embodiment is Ni 0.10 Fe 0.40 Mn 0.40 Zn 0.07 Li 0.03 (OH)2. The other process conditions are the same.
[0094] The product prepared in this example has the molecular formula of Na 0.83 Ni 0.10 Fe 0.395 Mn 0.40 Zn 0.07 Li 0.03 Al0.005 O2, SEM analysis was performed on it, from Figure 6 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 5 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.58 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 4.56μm.
[0095] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.13 As shown, the discharge capacity is 130.01 mAh / g, the 5C rate discharge capacity retention rate is 77.31%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 95.82%. Fig.15 .
[0096] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0097] Example 6
[0098] The preparation process of this embodiment is basically the same as that of embodiment 2. The only difference is that 1.06 Ni 0.25 Fe 0.325 Mn 0.3 2Zn 0.07 Li 0.03 Al 0.005 O2 was added in a stoichiometric ratio. The other process conditions were the same.
[0099] The product prepared in this example was subjected to SEM analysis. Figure 7 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 6 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.44 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 7.74μm.
[0100] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.11 As shown, the discharge capacity is 150.86 mAh / g, the 5C rate discharge capacity retention rate is 69.92%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 94.14%. Fig.15 .
[0101] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0102] Example 7
[0103] The preparation process of this embodiment is basically the same as that of embodiment 2. The only difference is that 0.91 Ni 0.15 Fe 0.375 Mn 0.3 7Z 0.07 Li 0.03 Al 0.005 O2 was added in a stoichiometric ratio. The other process conditions were the same.
[0104] The product prepared in this example was subjected to SEM analysis. Figure 8 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 7 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.50 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 6.53 μm.
[0105] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.12 As shown, the discharge capacity is 139.22 mAh / g, the 5C rate discharge capacity retention rate is 74.22%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 95.49%. Fig.15 .
[0106] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0107] Example 8
[0108] The preparation process of this embodiment is basically the same as that of embodiment 2. The only difference is that 0.83 Ni 0.10 Fe 0.395 Mn 0.4 0Z 0.07 Li 0.03 Al 0.005 O2 was added in a stoichiometric ratio. The other process conditions were the same.
[0109] The product prepared in this example was subjected to SEM analysis. Fig. 9 It can be seen that the low-nickel and high-capacity sodium ion battery positive electrode material prepared in Example 8 has an irregular block morphology and a layered structure. The specific surface area of the sodium ion battery positive electrode material is 0.60 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 4.45 μm.
[0110] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.13 As shown, the discharge capacity is 127.32 mAh / g, the 5C rate discharge capacity retention rate is 76.02%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 96.02%. Fig.15 .
[0111] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0112] Example 9
[0113] The preparation process of this embodiment is basically the same as that of embodiment 1, except that TM is Mg.
[0114] The rest of the process conditions are the same.
[0115] The specific surface area of the sodium ion battery positive electrode material prepared in this embodiment is 0.52m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 5.83 μm.
[0116] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.14 As shown, the discharge capacity is 148.24 mAh / g, the 5C rate discharge capacity retention rate is 74.34%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 94.29%. Fig.16 .
[0117] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0118] Example 10
[0119] The preparation process of this embodiment is basically the same as that of embodiment 1, except that TM is Ti. The other process conditions are the same.
[0120] The specific surface area of the sodium ion battery positive electrode material prepared in this embodiment is 0.54m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 5.63μm.
[0121] The sodium ion battery prepared in this example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.14As shown, the discharge capacity is 146.41 mAh / g, the 5C rate discharge capacity retention rate is 75.18%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 94.40%. Fig.16 .
[0122] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment is listed in the following Table 1.
[0123] Comparative Example 1
[0124] The difference between this comparative example and Example 1 is that according to Na 0.91 Ni 0.20 Fe 0.365 Mn 0.36 Zn 0.07 Al 0.005 O2 was added in a stoichiometric ratio. The other process conditions were the same.
[0125] The specific surface area of the sodium ion battery positive electrode material prepared in this comparative example is 0.53 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 5.64μm.
[0126] The sodium ion battery prepared in this comparative example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.17 As shown, the discharge capacity is 142.26 mAh / g, the 5C rate discharge capacity retention rate is 77.48%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 94.88%. Fig.19 .
[0127] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this comparative example is listed in Table 1 below.
[0128] Comparative Example 2
[0129] The difference between this comparative example and Example 1 is that according to Na 0.88 Ni 0.20 Fe 0.385 Mn 0.38 Li 0.03 Al 0.005 O2 was added in a stoichiometric ratio. The other process conditions were the same.
[0130] The specific surface area of the sodium ion battery positive electrode material prepared in this comparative example is 0.54 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 5.64μm.
[0131] The sodium ion battery prepared in this comparative example was subjected to charge and discharge tests with a current density of 15 mAh / g and a voltage range of 2 to 4 V. The charge and discharge curves are shown in FIG. Fig.17 As shown, the discharge capacity is 138.03 mAh / g, the 5C rate discharge capacity retention rate is 78.79%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 97.08%. Fig.19 .
[0132] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this comparative example is listed in Table 1 below.
[0133] Comparative Example 3
[0134] The difference between this comparative example and Example 1 is that according to Na 0.8 Ni 0.20 Fe 0.395 Mn 0.40 Al 0.005 O2 was added in a stoichiometric ratio. The other process conditions were the same.
[0135] The specific surface area of the sodium ion battery positive electrode material prepared in this comparative example is 0.52 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 5.61 μm.
[0136] The sodium ion battery prepared in this comparative example was subjected to charge and discharge tests. The current density was 15 mAh / g and the voltage range was 2 to 4 V. The charge and discharge curves were as follows: Fig.17 As shown, the discharge capacity is 130.49 mAh / g, the 5C rate discharge capacity retention rate is 82.27%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 97.33%. Fig.19 .
[0137] The median voltage of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this comparative example is listed in Table 1 below.
[0138] Comparative Example 4
[0139] This comparison is the mainstream NaNi in the NFM111 system. 1 / 3 Fe 1 / 3 Mn 1 / 3 O2. It is prepared by the following method:
[0140] By NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The other process conditions are the same as those in Example 1.
[0141] The specific surface area of the sodium ion battery positive electrode material prepared in this comparative example is 0.49 m 2 / g, and the median particle size D50 of the sodium ion battery positive electrode material is 5.70 μm.
[0142] The sodium ion battery prepared in this comparative example was subjected to charge and discharge tests. The current density was 15 mAh / g and the voltage range was 2 to 4 V. The charge and discharge curves were as follows: Fig.18 As shown, the discharge capacity is 134.35 mAh / g, the 5C rate discharge capacity retention rate is 87.51%, and after 50 cycles at 1C (150 mA / g), the discharge capacity retention rate is 96.19%. Fig.19 .
[0143] The median voltage and compaction density of the low-nickel and high-capacity sodium ion battery positive electrode material prepared in this embodiment are listed in Table 1 below.
[0144] Table 1 Performance of prepared positive electrode materials
[0145]
[0146]
[0147] By comparing Example 1, Example 2 and Comparative Example 4, it can be seen that the present application can prepare low-nickel and high-capacity sodium ion battery positive electrode materials by preparing a corresponding low-nickel precursor and mixing with a dopant-sintering or by a high-temperature solid phase method. The positive electrode materials prepared in Example 1 and Example 2 reduce the nickel content in the material components, and the raw material cost is lower than that of the NFM111 system, and the lower the nickel content, the lower the cost; Figures 10 to 13 and Fig.15 It can be seen that the sodium ion battery layered oxide positive electrode material prepared by mixing and sintering the corresponding low-nickel precursor and dopant has a relatively higher discharge capacity, rate performance and cycle stability, indicating that the sample synthesized by this preparation method has better structural stability.
[0148] By comparing Example 1, Example 3, Example 4 and Example 5, it can be seen that the preparation of low-nickel precursors with different structures has a certain influence on the performance of the finally prepared positive electrode material. When the chemical formula of the low-nickel precursor is Ni 0.20 Fe 0.35 Mn 0.35 Zn 0.07 Li 0.03 (OH)2, the prepared positive electrode material is relatively superior to the products prepared in other embodiments in terms of structure and performance. From the perspective of gram capacity, Ni and Fe are the main elements that provide charge compensation, so Example 3Na 1.06 Ni 0.25 Fe0.325 Mn 0.32 Zn 0.07 Li 0.03 Al 0.005 The O2 sample has the highest charge capacity, but its Mn content is slightly lower than that of Example 1Na 0.98 Ni 0.20 Fe 0.345 Mn 0.35 Zn 0.07 Li 0.03 Al 0.005 The O2 sample has a slightly inferior structural stability to that of the Example 1 sample, so it does not show a higher discharge gram capacity than that of Example 1, and its cycle performance is lower than that of Example 1. Due to the lower nickel content, the charge gram capacity of Examples 4 and 5 is lower than that of Examples 1 and 3. Although they have relatively better structural stability, the discharge gram capacity is limited by the charge gram capacity and remains at a lower level.
[0149] By comparing Example 1 and Examples 6 to 10, it can be seen that the positive electrode material of Example 1 is better than that of the other examples. By comparing Example 1 with Comparative Examples 1, 2, and 3, it can be seen that the gram capacity of the sample doped with Zn or Li alone or not doped with either of them is larger than that of the sample co-doped with Zn and Li. The reason is that Zn can induce Ni with high potential (about 4.0V, different nickel-containing material systems have different potentials) 3+ / Ni 4+ or 2- The redox reaction of Zn can be advanced, so that a higher gram capacity can be obtained at a relatively low upper cut-off voltage, so as to prevent the passive increase of the upper cut-off voltage to achieve high gram capacity, thereby causing the lattice structure of the material to collapse at high SOC; Zn can reduce the Fe 3+ The irreversible migration to the Na layer improves the voltage drop during the cycle; the low-valence Zn can control the valence state of Mn to a level close to +4, thereby reducing the 3+ The lattice distortion caused by the Jahn-Teller effect improves the cycling performance of the material; a small amount of Zn migrates to the Na layer during the cycle, reducing the Na + The lattice changes during the extraction / insertion process improve the structural stability; the Li element undergoes reversible migration from the transition metal layer to the Na layer during the charge and discharge process, and after the migration, vacancies are generated in the transition metal layer, forming a Li(Na)-O-□TM or □Na-O-□TM configuration, activating the anion redox reaction and providing more gram capacity. Compared with the mainstream NFM111 system in Comparative Example 4, it can be seen that the performance of the sample in Example 1 is significantly better than that of the NFM111 sample.
[0150] The above examples are for the purpose of illustrating the embodiments disclosed by the present invention and are not to be construed as limitations of the present invention. In addition, the various modifications listed herein and the variations of methods and compositions in the invention are obvious to those skilled in the art without departing from the scope and spirit of the present invention. Although the present invention has been specifically described in conjunction with various specific preferred embodiments of the present invention, it should be understood that the present invention should not be limited to these specific embodiments. In fact, various modifications obvious to those skilled in the art as described above to obtain the invention should be included within the scope of the present invention.
Claims
1. A low-nickel, high-capacity sodium ion battery positive electrode material, characterized in that: The chemical formula of the positive electrode material of the sodium-ion battery is Na x (Ni a Fe b Mn c Zn d Li e ) 1-f TM f O2, where 0.5 ≤ x ≤ 1.1, 0 < a < 0.3, 0.2 ≤ b ≤ 0.5, 0.2 ≤ c ≤ 0.5, 0 < d ≤ 0.1, 0 < e ≤ 0.1, 0 ≤ f ≤ 0.1, a + b + c + d + e = 1. The positive electrode material of the sodium-ion battery has an irregular block morphology and a layered structure.
2. The low-nickel and high-capacity sodium ion battery positive electrode material according to claim 1, characterized in that: The TM includes at least one of elements Ti, V, Cr, Mn, Fe, Co, Ni, Cu, K, Ta, La, Nb, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F.
3. The low-nickel and high-capacity sodium ion battery positive electrode material according to claim 2, characterized in that: The positive electrode material of the sodium ion battery has an irregular block morphology and a layered structure, and the specific surface area of the positive electrode material of the sodium ion battery is less than 0.8 m 2 / g; And / or, the median particle size D50 of the positive electrode material of the sodium ion battery is 3.0 - 12.0 μm.
4. A low-nickel, high-capacity sodium ion battery positive electrode material as claimed in any one of claims 1 to 3, characterized in that: The preparation method includes the following steps: Step 1: Prepare a low-nickel precursor by a coprecipitation method: The chemical formula of the low-nickel precursor is Ni a Fe b Mn c Zn d Li e CO3, Ni a Fe b Mn c Zn d Li e (OH)2 or Ni a Fe b Mn c Zn d Li e C2O4, 0 < a < 0.3, 0.2 ≤ b ≤ 0.5, 0.2 ≤ c ≤ 0.5, 0 < d ≤ 0.1, 0 < e ≤ 0.1, and a + b + c + d + e = 1; Step 2: Mix the low-nickel precursor, the dopant, and the sodium source compound in a stoichiometric ratio, perform drying treatment, then carry out high-temperature sintering, cool to room temperature, and then perform crushing, grinding, and sieving treatments to obtain a low-nickel high-capacity positive electrode material for a sodium ion battery; wherein, in the low-nickel high-capacity positive electrode material for a sodium ion battery, except that the Na element ratio is added according to 0.8 - 1.1 times the theoretical sodium addition, the usage amounts of other elements are calculated according to the molar ratios of the respective elements in the chemical formula; the sintering temperature is 850 - 1100 °C, the heat preservation time is 6 - 20 h, the heating rate is 1 - 10 °C / min, and the sintering atmosphere is air or oxygen.
5. The method for preparing a low-nickel and high-capacity sodium ion battery positive electrode material according to claim 4, characterized in that: The dopant includes one or more of compounds containing Ti, V, Cr, Co, Cu, K, Si, Ta, La, Nb, Y, Zr, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F.
6. The method for preparing a low-nickel and high-capacity sodium ion battery positive electrode material according to claim 4, characterized in that: The sodium source compound includes at least one of Na2CO3, NaHCO3, NaOH, Na2O, and CH3COONa.
7. A low-nickel high-capacity sodium ion battery positive electrode material as claimed in any one of claims 1 to 3, characterized in that: The preparation method includes the following steps: Mix the transition metal or non-metal element compound and the sodium source compound in a stoichiometric ratio, perform drying and tabletting treatments, then carry out high-temperature sintering, cool to room temperature, and then perform crushing, grinding, and sieving treatments to obtain a low-nickel high-capacity positive electrode material for a sodium ion battery; wherein, in the low-nickel high-capacity positive electrode material for a sodium ion battery, except that the Na element ratio is added according to 0.8 - 1.1 times the theoretical sodium addition, the usage amounts of other elements are calculated according to the molar ratios of the respective elements in the chemical formula; the sintering temperature is 850 - 1100 °C, the heat preservation time is 6 - 20 h, the heating rate is 1 - 10 °C / min, and the sintering atmosphere is air or oxygen.
8. The method for preparing a low-nickel and high-capacity sodium ion battery positive electrode material according to claim 7, characterized in that: The transition metal or non-metal element compound includes at least one of compounds containing elements Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Li, K, Si, Ta, La, Nb, Y, Zr, Zn, Mg, Al, Sn, Ru, Sr, W, Mo, B, and F.
9. The method for preparing a low-nickel and high-capacity sodium ion battery positive electrode material according to claim 7, characterized in that: The sodium source compound includes at least one of Na2CO3, NaHCO3, NaOH, Na2O, and CH3COONa.
10. A sodium ion battery, characterized in that: The positive electrode material of the sodium ion battery is the low-nickel high-capacity positive electrode material described in any one of claims 1 - 3 or the low-nickel high-capacity positive electrode material prepared by the preparation method described in any one of claims 4 - 9.
Citation Information
Cited By
Sodium-ion battery positive electrode material precursor as well as preparation method and application thereof
CN119306265A
Oxide-doped sodium ion battery high-voltage positive electrode material and preparation method thereof
CN119873903A
A doped oxide sodium-ion battery high-voltage positive electrode material and a preparation method thereof
CN119873903B
High-capacity sodium-ion battery positive electrode material as well as preparation method and application thereof
CN120978060A