Positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
By forming a surface modification layer containing Al and Sr on the lithium transition metal composite oxide, the problem of structural instability of the lithium transition metal composite oxide under high Ni content is solved, and the stability and high capacity characteristics of the battery capacity are achieved.
Patent Information
- Application Number
- CN202411048745.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-07-28
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing nonaqueous electrolyte secondary batteries, the layered structure of lithium transition metal composite oxide is unstable under high Ni content, resulting in the gradually decreasing battery capacity during charging and discharging.
The lithium transition metal composite oxide and the surface modification layer are used to combine the lithium transition metal composite oxide. The surface modification layer contains Al and Sr. The surface structure of the lithium transition metal composite oxide is stabilized through the synergistic effect of Al and Sr, inhibit the electrolyte reaction, and maintain the stability of the layered structure. sex.
It effectively suppresses the reduction of battery capacity during charging and discharging, and improves the high capacity characteristics of the battery.
Smart Images

Figure BDA0004974263470000171 
Figure HDA0004974263480000011
Abstract
Description
[0001] This application is a divisional application of an application filed on July 28, 2020, with application number 202080059907.9 and invention name “Positive electrode active material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery”. Technical Field
[0002] The present application relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery. Background Art
[0003] In recent years, as a high-output, high-capacity secondary battery, a nonaqueous electrolyte secondary battery having a positive electrode, a negative electrode and a nonaqueous electrolyte, which allows lithium ions to move between the positive electrode and the negative electrode for charge and discharge, has been widely used. From the viewpoints of low resistance and high capacity of the battery, the characteristics of the positive electrode active material contained in the positive electrode of the battery are sought to be improved.
[0004] For example, Patent Document 1 discloses a positive electrode active material, which is a lithium transition metal composite oxide having a layered structure and containing Mn, Ni, Co, Sr and Mo. By setting the Mo content to 0.1 mol% to 1.5 mol% and the Mo / Sr content ratio to 0.5 to 2.0 in terms of molar ratio, high capacity can be achieved and charge and discharge cycle characteristics can be improved.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent No. 5245210 Summary of the invention
[0008] However, for the lithium transition metal composite oxide contained in the positive electrode active material, a design of increasing the content of Ni in order to obtain a high discharge capacity is considered. However, when the ratio of Ni to the total molar number of metal elements other than Li is 80 mol% or more, the layered structure of the lithium transition metal composite oxide sometimes becomes unstable, and the battery capacity decreases with charging and discharging. The technology of Patent Document 1 does not take into account the reduction of the battery capacity of the battery with a high Ni content rate accompanied by charging and discharging, and there is still room for improvement.
[0009] Therefore, an object of the present application is to provide a positive electrode active material in which the ratio of Ni to the total molar number of metal elements other than Li is 80 mol % or more and in which a decrease in battery capacity accompanying charge and discharge can be suppressed.
[0010] A positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present application is characterized in that it comprises a lithium transition metal composite oxide and a surface modification layer, wherein the lithium transition metal composite oxide contains at least Al and 80 mol % or more of Ni relative to the total molar number of metal elements other than Li, and the surface modification layer is formed on the surface of primary particles of the lithium transition metal composite oxide and contains at least Sr.
[0011] A nonaqueous electrolyte secondary battery as one embodiment of the present application is characterized by comprising a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode includes the positive electrode active material.
[0012] According to the positive electrode active material for a nonaqueous electrolyte secondary battery as one embodiment of the present application, a high-capacity nonaqueous electrolyte secondary battery capable of suppressing a decrease in battery capacity associated with charge and discharge can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment.
[0014] Description of Reference Numerals
[0015] 10 Non-aqueous electrolyte secondary battery
[0016] 11 Positive electrode
[0017] 12 Negative electrode
[0018] 13 Divider
[0019] 14 Electrode body
[0020] 15 Battery housing
[0021] 16 Outer packaging cans
[0022] 17 Sealing body
[0023] 18, 19 Insulation board
[0024] 20 positive electrode tab
[0025] 21. Negative electrode tab
[0026] 22 Groove
[0027] 23 Base Plate
[0028] 24 Lower valve plug
[0029] 25 Insulation parts
[0030] 26 Upper valve plug
[0031] 27 Cover
[0032] 28 Gasket
[0033] 30 Positive electrode collector
[0034] 31. Positive electrode active material layer
[0035] 40 Negative electrode collector
[0036] 41 Negative electrode active material layer DETAILED DESCRIPTION
[0037] There are transition metal layers such as Ni, Li layers, and oxygen layers in the layered structure of the lithium transition metal composite oxide, and the charge and discharge reaction of the battery is carried out by the reversible entry and exit of Li ions present in the Li layer. Here, in the lithium transition metal composite oxide contained in the positive electrode active material, when the ratio of Ni relative to the total molar number of metal elements other than Li is 80 mol% or more, when the battery is charged, a large amount of Li ions are separated from the Li layer, so the layered structure sometimes becomes unstable. On the surface of the lithium transition metal composite oxide where the layered structure becomes unstable, a metamorphic layer is formed due to the reaction with the electrolyte. Since the structural changes of the lithium transition metal composite oxide further occur from the metamorphic layer as the starting point, the battery capacity gradually decreases with charging and discharging. However, as a positive electrode active material for a non-aqueous electrolyte secondary battery in one form of the present application, by containing a specified amount of Al and Sr, the reaction with the electrolyte at the surface is suppressed due to the synergistic effect of Al and Sr, and then, the surface structure is stabilized, so that the battery capacity reduction associated with charging and discharging can be suppressed. It is speculated that since Al does not change its oxidation number during charge and discharge, its presence in the transition metal layer stabilizes the structure of the transition metal layer. It is also speculated that Sr can change the surface state of the lithium transition metal composite oxide due to the interaction of electrons.
[0038] Hereinafter, an example of an embodiment of the non-aqueous electrolyte secondary battery described in the present application is described in detail. Hereinafter, a cylindrical battery in which a wound electrode body is contained in a cylindrical battery case is exemplified, but the electrode body is not limited to a wound type, and can be a laminated type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one through a separator. In addition, the battery case is not limited to a cylindrical shape, and can be, for example, a square, a coin shape, etc., or a battery case consisting of a laminated sheet comprising a metal layer and a resin layer.
[0039] Figure 1 FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1As shown in the example, the nonaqueous electrolyte secondary battery 10 includes an electrode body 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 has a winding structure in which the positive electrode 11 and the negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 is composed of an outer can 16 with a bottomed cylindrical shape and a sealing body 17 that seals the opening of the outer can 16.
[0040] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one size larger than the positive electrode 11. That is, the negative electrode 12 is formed longer in the length direction and the width direction (short side direction) than the positive electrode 11. The two separators 13 are formed to be at least one size larger than the positive electrode 11, for example, arranged in a manner of clamping the positive electrode 11.
[0041] The non-aqueous electrolyte secondary battery 10 includes insulating plates 18 and 19 disposed above and below the electrode body 14, respectively. Figure 1 In the example shown, the positive electrode tab 20 mounted on the positive electrode 11 extends toward the sealing body 17 through the through hole of the insulating plate 18, and the negative electrode tab 21 mounted on the negative electrode 12 extends toward the bottom side of the outer can 16 through the outer side of the insulating plate 19. The positive electrode tab 20 is connected to the lower surface of the bottom plate 23 of the sealing body 17 by welding or the like, and the cover 27 of the sealing body 17 electrically connected to the bottom plate 23 becomes the positive terminal. The negative electrode tab 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 becomes the negative terminal.
[0042] The outer can 16 is, for example, a metal container in a cylindrical shape with a bottom. A gasket 28 is provided between the outer can 16 and the sealing body 17, and the internal space of the battery case 15 is sealed. The outer can 16 has a groove portion 22 for supporting the sealing body 17, for example, formed by pressurizing the side portion from the outside. The groove portion 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and the sealing body 17 is supported by its upper surface.
[0043] The sealing body 17 has a structure in which a bottom plate 23, a lower valve plug 24, an insulating component 25, an upper valve plug 26 and a cover body 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating component 25 are electrically connected to each other. The lower valve plug 24 and the upper valve plug 26 are connected to each other at their respective central portions, and an insulating component 25 is sandwiched between their respective edge portions. If the internal pressure of the battery rises due to abnormal heat release, the lower valve plug 24 is deformed and broken in a manner that pushes the upper valve plug 26 toward the cover body 27 side, thereby blocking the circuit between the lower valve plug 24 and the upper valve plug 26. If the internal pressure rises further, the upper valve plug 26 breaks and gas is discharged from the opening of the cover body 27.
[0044] The positive electrode 11 , the negative electrode 12 , the separator 13 , and the nonaqueous electrolyte constituting the nonaqueous electrolyte secondary battery 10 , particularly the positive electrode active material contained in the positive electrode active material layer 31 constituting the positive electrode 11 , will be described in detail below.
[0045] [positive electrode]
[0046] The positive electrode 11 has a positive electrode collector 30 and a positive electrode active material layer 31 formed on both sides of the positive electrode collector 30. The positive electrode collector 30 can use a foil of a metal such as aluminum or aluminum alloy that is stable within the potential range of the positive electrode 11, a thin film having the metal configured on the surface, etc. The positive electrode active material layer 31 contains a positive electrode active material, a conductive material, and a binding material. The thickness of the positive electrode active material layer 31 is, for example, 10 μm to 150 μm on one side of the positive electrode collector 30. The positive electrode 11 can be made by coating a positive electrode slurry containing a positive electrode active material, a conductive material, and a binding material on the surface of the positive electrode collector 30, and after drying the coating, compressing it to form the positive electrode active material layer 31 on both sides of the positive electrode collector 30.
[0047] As the conductive material contained in the positive electrode active material layer 31, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binding material contained in the positive electrode active material layer 31, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. These resins can be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc.
[0048] The positive electrode active material contains a lithium transition metal composite oxide and a surface modification layer formed on the surface of the primary particles of the lithium transition metal composite oxide. The lithium transition metal composite oxide contains at least Al and Ni in a proportion of 80 mol% or more relative to the total molar amount of metal elements other than Li. By setting the proportion of Ni relative to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide to 80 mol% or more, a battery with a high capacity can be obtained.
[0049] The lithium transition metal composite oxide has a layered structure. Examples of the layered structure of the lithium transition metal composite oxide include a layered structure belonging to the space group R-3m, a layered structure belonging to the space group C2 / m, etc. Among these, from the viewpoints of high capacity and stability of the crystal structure, etc., a layered structure belonging to the space group R-3m is preferred.
[0050] The proportion of Ni relative to the total molar amount of metal elements other than Li in the lithium transition metal composite oxide is preferably 90 mol% or more. Thereby, a battery with an even higher capacity can be obtained.
[0051] The lithium transition metal composite oxide can be represented by the general formula Li a Ni x Al y Co z M w O 2-b (wherein, 0.95 < a < 1.05, 0.8 ≤ x ≤ 0.96, 0 < y ≤ 0.10, 0 ≤ z ≤ 0.15, 0 ≤ w ≤ 0.1, 0 ≤ b < 0.05, x + y + z + w = 1; M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn). It should be noted that the positive electrode active material may contain a lithium transition metal composite oxide or other compounds other than those represented by the above general formula within the scope not impairing the object of the present application. The molar fraction of the metal elements contained in the whole particles of the lithium transition metal composite oxide is measured by inductively coupled plasma (ICP) emission spectrometry.
[0052] a representing the proportion of Li in the lithium transition metal composite oxide preferably satisfies 0.95 ≤ a < 1.05, and more preferably satisfies 0.97 ≤ a ≤ 1.03. When a is less than 0.95, the battery capacity sometimes decreases compared with the case where a satisfies the above range. When a is 1.05 or more, more Li compounds are added compared with the case where a satisfies the above range, and thus it is sometimes uneconomical from the viewpoint of production cost.
[0053] The proportion y of Al relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide preferably satisfies 0 < y ≤ 0.10, more preferably 0.03 ≤ y ≤ 0.07. Since Al does not change its oxidation number during charge and discharge, it can be considered that the structure of the transition metal layer is stabilized by including Al in the transition metal layer. On the other hand, when y > 0.10, Al impurities are generated, resulting in a decrease in battery capacity. Al can be uniformly dispersed, for example, within the layered structure of the lithium transition metal composite oxide, or can be present in a part of the layered structure.
[0054] Co and M (M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn) are optional components. The proportions z and w of Co and M relative to the total molar number of metal elements other than Li in the lithium transition metal composite oxide preferably satisfy 0 ≤ z ≤ 0.15 and 0 ≤ w ≤ 0.1, respectively. Since Co is expensive, from the viewpoint of manufacturing cost, it is preferable to suppress the Co content rate.
[0055] The lithium transition metal composite oxide is, for example, secondary particles aggregated from a plurality of primary particles. The particle diameter of the primary particles constituting the secondary particles is, for example, 0.05 μm to 1 μm. The particle diameter of the primary particles is measured in the form of the diameter of the circumscribed circle in the particle image observed by a scanning electron microscope (SEM). A surface modification layer exists on the surface of the primary particles. In other words, the surface modification layer exists on the surface of the secondary particles of the lithium transition metal composite oxide or at the interface where the primary particles contact each other.
[0056] The lithium transition metal composite oxide is particles having a volume-based median particle diameter (D50) of, for example, 3 μm to 30 μm, preferably 5 μm to 25 μm, and particularly preferably 7 μm to 15 μm. D50 refers to the particle diameter at which the cumulative frequency in the volume-based particle size distribution reaches 50% starting from the smaller particle diameter side, and is also referred to as the median diameter. The particle size distribution of the lithium transition metal composite oxide can be measured using a laser diffraction type particle size distribution measuring device (for example, manufactured by MICROTRAC-BELL Corporation, MT3000II) with water as the dispersion medium.
[0057] The lithium transition metal composite oxide has a surface layer existing from the surface to the inner side and a main body portion existing on the inner side of the surface layer. The thickness of the surface layer is, for example, 1 nm to 5 nm.
[0058] The ratio of Al in the surface layer relative to the total molar number of metal elements other than Li is 1.3 times or more of the ratio of Al in the main body relative to the total molar number of metal elements other than Li. Thus, the structure of the surface layer is more stabilized than the main body, and therefore, the reduction in battery capacity associated with charge and discharge can be suppressed by the synergistic effect with the surface modification layer described later. It should be noted that the ratio of Al in the surface layer relative to the total molar number of metal elements other than Li can be set to, for example, less than 4 times the ratio of Al in the main body relative to the total molar number of metal elements other than Li.
[0059] The surface modification layer contains at least Sr. The surface modification layer may contain, for example, Sr or a compound containing Sr. As a compound containing Sr, SrO2 can be exemplified. The surface modification layer may further contain at least one selected from Al or a compound containing Al, and a compound containing Sr and Al. As a compound containing Al, Al2O3 can be exemplified. In addition, as a compound containing Sr and Al, SrAlO4 can be exemplified. The surface modification layer may further contain Li. Li present on the surface of the lithium transition metal composite oxide described later may be contained in the surface modification layer.
[0060] The ratio of Al to the total number of moles of metal elements other than Li in the surface modification layer may be greater than the ratio of Al to the total number of moles of metal elements other than Li in the bulk of the lithium transition metal composite oxide.
[0061] Furthermore, the ratio of Al to the total molar number of metal elements other than Li in the surface modification layer is preferably 1.9 times or more the ratio of Al to the total molar number of metal elements other than Li in the main body of the lithium transition metal composite oxide.
[0062] The ratio of Sr in the surface modification layer can be 0.05 mol % to 0.25 mol % relative to the total molar number of metal elements other than Li in the surface modification layer. Within this range, the surface state of the lithium transition metal composite oxide can be changed by the interaction of electrons.
[0063] The thickness of the surface modification layer is, for example, 0.1 nm to 2 nm. Within this range, the reaction with the electrolyte on the surface of the lithium transition metal composite oxide can be suppressed, and thus the reduction in battery capacity accompanying charge and discharge can be suppressed through a synergistic effect with the surface layer.
[0064] The amount of Li remaining on the surface of the lithium transition metal composite oxide (hereinafter sometimes referred to as the residual Li amount) can be set to 0.03 wt% to 0.08 wt%. The Li present on the surface of the lithium transition metal composite oxide includes: Li contained in the surface modification layer, and Li present in a form such as a Li compound on the surface modification layer but not contained in the surface modification layer.
[0065] The positive electrode active material is dispersed in water and dissolved, and the residual Li amount can be quantitatively determined by titration. The specific measurement method is as follows.
[0066] (1) 1 g of the positive electrode active material is added to 30 ml of pure water, and the mixture is stirred to prepare a suspension in which the active material is dispersed in water.
[0067] (2) The suspension was filtered, and pure water was added to adjust the volume to 70 ml to obtain a filtrate containing Li dissolved from the active material.
[0068] (3) While measuring the pH of the filtrate, hydrochloric acid was added dropwise to the filtrate, and the amount of Li dissolved in the filtrate was calculated from the amount of hydrochloric acid consumed (titration) until the first inflection point (near pH 8) and the second inflection point (near pH 4) of the pH curve.
[0069] For example, from the perspective of increasing the capacity of the battery and effectively suppressing the reduction in charge and discharge cycle characteristics, the content of the lithium transition metal composite oxide in the positive electrode active material is preferably 90 mass % or more, more preferably 99 mass % or more relative to the total mass of the positive electrode active material.
[0070] In addition, the positive electrode active material of the present embodiment may include other lithium transition metal composite oxides in addition to the lithium transition metal composite oxide of the present embodiment. As other lithium transition metal composite oxides, for example, lithium transition metal composite oxides having a Ni content of 0 mol% or more and less than 85 mol% may be listed.
[0071] Next, an example of a method for producing a positive electrode active material including a lithium transition metal composite oxide and a surface modification layer will be described.
[0072] The method for producing a positive electrode active material, for example, comprises the following steps: a first step of obtaining a composite oxide containing Ni, Al and an optional metal element; a second step of mixing the composite oxide obtained in the first step with a lithium compound to obtain a mixture; and a third step of calcining the mixture. The composition and thickness of the surface layer and the surface modification layer in the finally obtained positive electrode active material are adjusted by controlling, for example, the mixing ratio of the raw materials in the second step, the calcination temperature and time in the third step, etc.
[0073] In the first step, for example, by stirring a solution of a metal salt containing Ni, Al and an optional metal element (Co, Mn, Fe, etc.), while dropping an alkaline solution such as sodium hydroxide, the pH is adjusted to the alkaline side (e.g., 8.5 to 12.5), so that a composite hydroxide containing Ni, Al and an optional metal element is precipitated (coprecipitated), and the composite hydroxide is calcined to obtain a composite oxide containing Ni, Al and an optional metal element. The calcination temperature is not particularly limited, for example, in the range of 300° C. to 600° C.
[0074] In the second step, the composite oxide, lithium compound and strontium compound obtained in the first step are mixed to obtain a mixture. Examples of lithium compounds include Li2CO3, LiOH, Li2O2, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, and LiF. Examples of strontium compounds include Sr(OH)2, Sr(OH)2·8H2O, SrO, SrCo3, SrSO4, and Sr(NO3)2. Regarding the mixing ratio of the composite oxide obtained in the first step and the lithium compound, from the viewpoint of facilitating the adjustment of the above parameters to the above specified ranges, it is preferably set to a ratio in the range of 1:0.98 to 1:1.1 in terms of the molar ratio of the metal element other than Li:Li. In addition, regarding the mixing ratio of the composite oxide obtained in the first step and the strontium compound, from the viewpoint of easily adjusting the above parameters to the above specified range, it is preferably set to a ratio in the range of 1:0.0005 to 1:0.0018, for example, the molar ratio of the metal element other than Li:Sr. In the second step, when the composite oxide, lithium compound and strontium compound obtained in the first step are mixed, other metal raw materials may be added as needed. Other metal raw materials are oxides of metal elements other than the metal elements constituting the composite oxide obtained in the first step, etc.
[0075] In the third step, the mixture obtained in the second step is calcined at a specified temperature and time to obtain the positive electrode active material described in this embodiment. The calcination of the mixture in the third step, for example, has the following multi-stage calcination steps: a first calcination step, calcining to a first set temperature of 450°C or more and 680°C or less at a first heating rate in a calcination furnace under an oxygen gas flow; and a second calcination step, calcining the calcined product obtained by the above-mentioned first calcination step in a calcination furnace under an oxygen gas flow at a second heating rate to a second set temperature of more than 680°C and less than 800°C. Here, the first heating rate is in the range of 1.5°C / min or more and 5.5°C / min or less, and the second heating rate is slower than the first heating rate, and is in the range of 0.1°C / min or more and 3.5°C / min or less. Through this multi-stage calcination, for the positive electrode active material of the present embodiment finally obtained, the composition and thickness parameters of the surface layer and the surface modification layer can be adjusted to the above-mentioned specified range. It should be noted that if the first heating rate and the second heating rate are within the above-mentioned specified range, multiple temperatures can be set in each temperature zone. From the viewpoint of adjusting the above-mentioned parameters of the lithium transition metal composite oxide to the above-mentioned specified range, the holding time of the first set temperature in the first sintering process is preferably 0 hours or more and 5 hours or less, and more preferably 0 hours or more and 3 hours or less. The holding time of the first set temperature refers to the time for maintaining the first set temperature after the first set temperature is reached. From the viewpoint of adjusting the above-mentioned parameters of the lithium transition metal composite oxide to the above-mentioned specified range, the holding time of the second set temperature in the second sintering process is preferably 1 hour or more and 10 hours or less, and more preferably 1 hour or more and 5 hours or less. The holding time of the second set temperature refers to the time for maintaining the second set temperature after the second set temperature is reached. When sintering the mixture, from the viewpoint of adjusting the above-mentioned parameters to the above-mentioned specified range, for example, it can be carried out in an oxygen gas flow with an oxygen concentration of 60% or more, and the flow rate of the oxygen gas flow is set to 1 hour per 10 cm 3 The firing furnace is in the range of 0.2 mL / min to 4 mL / min and is 0.3 L / min or more per 1 kg of the mixture.
[0076] The molar fraction of the metal element contained in the positive electrode active material obtained as described above is measured by inductively coupled plasma (ICP) emission spectrometry, and can be expressed as Li a Ni x Al y Co z M w Sr α O 2-b(wherein, 0.95 < a < 1.05, 0.8 ≤ x ≤ 0.96, 0 < y ≤ 0.10, 0 ≤ z ≤ 0.15, 0 ≤ w ≤ 0.1, 0.05 ≤ α ≤ 0.18, 0 ≤ b < 0.05, x + y + z + w = 1; M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn). It should be noted that Sr is not dissolved in the lithium transition metal composite oxide, but is contained in the surface modification layer existing on the surface of the lithium transition metal composite oxide. In addition, a part of Al may be contained in the surface modification layer.)
[0077] In addition, the composition of the interior and surface layer of the lithium transition metal composite oxide in the positive electrode active material, and the composition of the surface modification layer can be determined by analyzing the ratio of Ni, Co, Al, and M at each part of the cross-section of the primary particles of the positive electrode active material using energy dispersive X-ray spectroscopy (TEM-EDX). It should be noted that since the surface modification layer is thinner than the spot diameter of the irradiated electron beam, it can be considered that the composition of the surface modification layer is affected by the composition of the adjacent surface layer. Even if Ni, Co, and Mn are detected in the measurement result of the surface layer, Ni, Co, and M do not actually exist in the surface layer. In addition, as in the case of α above, the addition amount of Sr is small, so although it is possible to confirm the presence or absence, it cannot be quantitatively measured.
[0078] [Negative electrode]
[0079] The negative electrode 12 has a negative electrode current collector 40 and a negative electrode active material layer 41 formed on both surfaces of the negative electrode current collector 40. The negative electrode current collector 40 can use a foil of a metal such as copper or a copper alloy that is stable within the potential range of the negative electrode 12, a thin film having the metal disposed on the surface layer, etc. The negative electrode active material layer 41 contains a negative electrode active material and a binder. The thickness of the negative electrode active material layer 41 is, for example, 10 μm to 150 μm on one side of the negative electrode current collector 40. The negative electrode 12 can be produced by coating a negative electrode slurry containing a negative electrode active material, a binder, etc. on the surface of the negative electrode current collector 40, drying the coating film, and then performing rolling to form the negative electrode active material layer 41 on both surfaces of the negative electrode current collector 40.
[0080] As the negative electrode active material contained in the negative electrode active material layer 41, any material that can reversibly occlude and release lithium ions is not particularly limited, and carbon materials such as graphite are usually used. The graphite can be any of natural graphite such as flake graphite, massive graphite, and earthy graphite; artificial graphite such as massive artificial graphite and graphitized mesophase carbon microbeads. In addition, as the negative electrode active material, metals that alloy with Li such as Si and Sn can be used; metal compounds containing Si, Sn, etc., lithium titanium composite oxides, etc. In addition, materials provided with a carbon coating film on them can be used. For example, SiO xa Si-containing compound represented by (0.5 ≤ x ≤ 1.6) or a Si-containing compound such as a Si-containing compound in which Si fine particles are dispersed in a lithium silicate phase represented by (0 < y < 2) is used in combination with graphite. 2y SiO (2+y) a Si-containing compound represented by (0 < y < 2) is used in combination with graphite.
[0081] Similar to the case of the positive electrode 11, the binder contained in the negative electrode active material layer 41 can be a fluororesin such as PTFE or PVdF, PAN, polyimide, an acrylic resin, a polyolefin, etc., and styrene-butadiene rubber (SBR) is preferably used. In addition, the negative electrode active material layer 41 can contain CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc.
[0082] [Separator]
[0083] The separator 13 can be, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include a microporous film, a woven fabric, a non-woven fabric, etc. As the material of the separator, polyolefins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 can be a single-layer structure or can have a laminated structure. In addition, a resin layer having high heat resistance such as an aromatic polyamide resin, a filler layer containing an inorganic compound filler, etc. can be provided on the surface of the separator 13.
[0084] [Non-aqueous electrolyte]
[0085] The non-aqueous electrolyte contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. As the non-aqueous solvent, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and a mixed solvent of two or more of these can be used. The non-aqueous solvent can contain a halogen-substituted product obtained by substituting at least a part of the hydrogen in these solvents with a halogen atom such as fluorine. As the halogen-substituted product, fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC); fluorinated chain carbonates; fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP), etc. can be cited.
[0086] Examples of the above esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate; cyclic carboxylic acid esters such as γ-butyrolactone (GBL), γ-valerolactone (GVL); chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), ethyl propionate (EP), etc.
[0087] Examples of the above-mentioned ethers include cyclic ethers such as 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-epoxybutane, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, crown ether, etc.; chain ethers such as 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc.
[0088] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborate, lithium lower aliphatic carboxylate, borate salts such as Li2B4O7, Li(B(C2O4)F2), etc.; imide salts such as LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2){l, m are integers of 0 or more}, etc. The lithium salts can be used alone or in combination of multiple kinds. Among these, from the viewpoints of ionic conductivity, electrochemical stability, etc., LiPF6 is preferably used. The concentration of the lithium salt is, for example, 0.8 mol to 1.8 mol per 1 L of the non-aqueous solvent. In addition, vinylene carbonate, propanesultone-based additives can be further added.
[0089] Examples
[0090] Hereinafter, the present application will be further described by way of examples and comparative examples, but the present application is not limited to the following examples.
[0091] [Production of positive electrode active material]
[0092] <Example 1>
[0093] The [Ni 0.82 Al 0.05 Co 0.13 The composite hydroxide represented by ](OH)2 was calcined at 500°C for 8 hours to obtain a composite oxide (Ni 0.82 Al 0.05 Co 0.13 O2). LiOH, Sr(OH)2 and the above composite oxide were mixed in such a way that the molar ratio of the total amount of Li, Ni, Al and Co to Sr reached 1.03:1:0.0005 to obtain a mixture. Under an oxygen gas flow with an oxygen concentration of 95% (per 10 cm 3 The mixture was calcined from room temperature to 650°C at a heating rate of 2.0°C / min, and then calcined from 650°C to 780°C at a heating rate of 0.5°C / min. The calcined product was washed with water to remove impurities to obtain a positive electrode active material. The composition of the positive electrode active material obtained above was measured using an ICP emission spectrometer (manufactured by Thermo Fisher Scientific, trade name "iCAP6300"), and the composition was LiNi 0.82 Al 0.05 Co 0.13 Sr 0.0005 O2 was used as the positive electrode active material of Example 1.
[0094] <Comparative Example 1>
[0095] LiOH and composite oxide (Ni 0.82 Al 0.05 Co 0.13 O2) was mixed in a manner such that the molar ratio of Li to the total amount of Ni, Al and Co reached 1.03:1 to obtain a mixture. Except for this, the same operation as in Example 1 was performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.82 Al 0.05 Co 0.13 O2 was used as the positive electrode active material of Comparative Example 1.
[0096] <Example 2>
[0097] Use [Ni 0.87 Al 0.04 Co 0.09 ](OH)2 to obtain a composite hydroxide (Ni 0.87 Al 0.04 Co 0.09O2), LiOH, Sr(OH)2 and the composite oxide are mixed in a manner such that the molar ratio of the total amount of Li, Ni, Al and Co to Sr reaches 1.03:1:0.001 to obtain a mixture. Except for this, the same operation as in Example 1 is performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.87 Al 0.04 Co 0.09 Sr 0.001 O2 was used as the positive electrode active material in Example 2.
[0098] <Comparative Example 2>
[0099] LiOH and composite oxide (Ni 0.87 Al 0.04 Co 0.09 O2) was mixed in a manner such that the molar ratio of Li to the total amount of Ni, Al and Co reached 1.03:1 to obtain a mixture. Except for this, the same operation as in Example 2 was performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.87 Al 0.04 Co 0.09 O2 was used as the positive electrode active material of Comparative Example 2.
[0100] <Example 3>
[0101] Use [Ni 0.92 Al 0.05 Co 0.01 Mn 0.02 ](OH)2 to obtain a composite hydroxide (Ni 0.92 Al 0.05 Co 0.01 Mn 0.02 O2), LiOH, Sr(OH)2 and the composite oxide are mixed in a manner such that the molar ratio of the total amount of Li, Ni, Al, Co and Mn to Sr reaches 1.03:1:0.0007 to obtain a mixture. Except for this, the same operation as in Example 1 is performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.92 Al 0.05 Co 0.01 Mn 0.02 Sr 0.0007 O2 was used as the positive electrode active material in Example 3.
[0102] <Comparative Example 3>
[0103] LiOH and composite oxide (Ni 0.92 Al 0.05 Co 0.01 Mn 0.02O2) was mixed in a manner such that the molar ratio of Li to the total amount of Ni, Al, Co and Mn reached 1.03:1 to obtain a mixture. Except for this, the same operation as in Example 3 was performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.92 Al 0.05 Co 0.01 Mn 0.02 O2 was used as the positive electrode active material of Comparative Example 3.
[0104] <Example 4>
[0105] Use [Ni 0.91 Al 0.05 Mn 0.04 ](OH)2 to obtain a composite hydroxide (Ni 0.91 Al 0.05 Mn 0.04 O2), LiOH, Sr(OH)2 and the composite oxide are mixed in a manner such that the total amount of Li, Ni, Al and Mn and Sr have a molar ratio of 1.03:1:0.0015 to obtain a mixture. Except for this, the same operation as in Example 1 is performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.91 Al 0.05 Mn 0.04 Sr 0.0015 O2 was used as the positive electrode active material of Example 4.
[0106] <Comparative Example 4>
[0107] LiOH and composite oxide (Ni 0.91 Al 0.05 Mn 0.04 O2) was mixed in a manner such that the molar ratio of Li to the total amount of Ni, Al and Mn reached 1.03:1 to obtain a mixture. Except for this, the same operation as in Example 4 was performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.91 Al 0.05 Mn 0.04 O2 was used as the positive electrode active material of Comparative Example 4.
[0108] <Example 5>
[0109] Use [Ni 0.92 Al 0.06 Mn 0.02 ](OH)2 to obtain a composite hydroxide (Ni 0.92 Al 0.06 Mn 0.02O2), LiOH, Sr(OH)2 and the composite oxide are mixed in a manner such that the total amount of Li, Ni, Al and Mn and Sr have a molar ratio of 1.03:1:0.0018 to obtain a mixture. Except for this, the same operation as in Example 1 is performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.92 Al 0.06 Mn 0.02 Sr 0.0018 O2 was used as the positive electrode active material of Example 5.
[0110] <Comparative Example 5>
[0111] LiOH and composite oxide (Ni 0.92 Al 0.06 Mn 0.02 O2) was mixed in a manner such that the molar ratio of Li to the total amount of Ni, Al and Mn reached 1.03:1 to obtain a mixture. Except for this, the same operation as in Example 5 was performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.92 Al 0.06 Mn 0.02 O2 was used as the positive electrode active material of Comparative Example 5.
[0112] <Comparative Example 6>
[0113] Use [Ni 0.60 Co 0.21 Mn 0.19 ](OH)2 to obtain a composite hydroxide (Ni 0.60 Co 0.21 Mn 0.19 O2), LiOH, Sr(OH)2 and the composite oxide are mixed in a manner such that the total amount of Li, Ni, Co and Mn and Sr have a molar ratio of 1.03:1:0.001 to obtain a mixture. Except for this, the same operation as in Example 1 is performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.60 Co 0.21 Mn 0.19 Sr 0.001 O2 was used as the positive electrode active material of Comparative Example 6.
[0114] <Comparative Example 7>
[0115] LiOH and composite oxide (Ni 0.60 Co 0.21 Mn 0.19O2) was mixed in a manner such that the molar ratio of Li to the total amount of Ni, Co and Mn reached 1.03:1 to obtain a mixture. Except for this, the same operation as in Comparative Example 6 was performed to obtain a positive electrode active material. The composition of the obtained positive electrode active material is LiNi 0.60 Co 0.21 Mn 0.19 O2 was used as the positive electrode active material of Comparative Example 7.
[0116] The positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 to 7 were subjected to TEM-EDX measurement, and the internal and surface layers of the lithium transition metal composite oxide and the surface modification layer were analyzed for composition. Since Sr cannot be quantified, its presence or absence is analyzed based on the presence or absence of the peak. In addition, the residual Li amount of the positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 to 7 was measured. The results are shown in Table 1.
[0117] [Table 1]
[0118]
[0119] In Examples 1 to 5, the Al content of the surface modification layer is greater than the Al content of the main body and the Al content of the surface layer. On the other hand, in Comparative Examples 1 to 5, such a tendency is not observed. In Examples 1 to 5, the Al content in the surface modification layer is greater than that in the surface layer, and Al exists in the surface modification layer, but in Comparative Examples 1 to 5, the Al content of the surface modification layer and the surface layer is the same, so it is affected by the composition of the adjacent surface layer, and it can be considered that there is no Al in the surface modification layer. In addition, in Examples 1 to 5 and Comparative Example 6 to which Sr is added, Sr is only detected in the surface modification layer, and is not detected in the surface layer and the main body. It should be noted that in any sample, the composition of the surface modification layer is affected by the composition of the adjacent surface layer, and it can be considered that Ni, Co and Mn are not present in the surface modification layer. In addition, only residual Li is detected in any sample.
[0120] Next, using the positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 to 7, test cells were prepared as follows.
[0121] [Production of positive electrode]
[0122] According to the positive electrode active material of Examples 1 to 5 and Comparative Examples 1 to 7, 91 parts by mass, 7 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder are mixed, and mixed with N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode slurry. Next, the slurry is applied to a positive electrode collector formed of an aluminum foil with a thickness of 15 μm. After the coating is dried, the coating is rolled using a calendering roller and cut into a specified electrode size to obtain a positive electrode having a positive electrode composite material layer formed on both sides of the positive electrode core. It should be noted that an exposed portion exposed on the surface of the positive electrode core is provided on a portion of the positive electrode. The other embodiments and comparative examples are also operated in the same way to make a positive electrode.
[0123] [Production of negative electrode]
[0124] Natural graphite is used as the negative electrode active material. The negative electrode active material, sodium carboxymethyl cellulose (CMC-Na) and styrene-butadiene rubber (SBR) are mixed in an aqueous solution at a solid content mass ratio of 100:1:1 to prepare a negative electrode composite material slurry. The negative electrode composite material slurry is applied to both sides of a negative electrode core formed by copper foil, and after the coating film is dried, the coating film is rolled using a calendering roller and cut into a specified electrode size to obtain a negative electrode having a negative electrode composite material layer formed on both sides of the negative electrode core. It should be noted that an exposed portion exposed on the surface of the negative electrode core is provided on a portion of the negative electrode.
[0125] [Preparation of non-aqueous electrolyte]
[0126] Ethylene carbonate (EC), ethyl methyl carbonate (MEC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent at a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0127] [Production of test battery cells]
[0128] An aluminum lead was installed on the exposed portion of the positive electrode containing the positive electrode active material of Examples 1 to 5 and Comparative Examples 1 to 7, and a nickel lead was installed on the exposed portion of the negative electrode, and the positive electrode and the negative electrode were wound into a spiral shape with a polyolefin separator interposed therebetween to prepare a wound electrode body. The electrode body was housed in an outer package, and after the non-aqueous electrolyte was injected, the opening of the outer package was sealed to obtain a test battery cell.
[0129] [Evaluation of capacity maintenance rate]
[0130] The following cycle test was performed on batteries fabricated by assembling positive electrodes containing the positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 to 7. The discharge capacity at the 1st cycle and the discharge capacity at the 100th cycle in the cycle test were determined, and the capacity retention rate was calculated by the following formula.
[0131] Capacity retention rate (%) = (discharge capacity at the 100th cycle ÷ discharge capacity at the 1st cycle) × 100
[0132] <Cyclic test>
[0133] The test battery cell was charged at a constant current of 0.5 It at a temperature of 45°C until the battery voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 1 / 50 It. Thereafter, the battery was discharged at a constant current of 0.5 It until the battery voltage reached 2.5 V. This charge and discharge cycle was repeated 100 times.
[0134] The capacity retention rates of Examples 1 to 5 and Comparative Examples 1 to 7 are shown in Tables 2 to 7, respectively. The residual Li amount is also described in Tables 2 to 7. The capacity retention rate of the test cell of Example 1 shown in Table 2 is a relative retention rate with the capacity retention rate of the test cell of Comparative Example 1 being 100%.
[0135] The capacity maintenance rate of the test battery cell of Example 2 shown in Table 3 is a relative maintenance rate, with the capacity maintenance rate of the test battery cell of Comparative Example 2 being 100%.
[0136] The capacity maintenance rate of the test battery cell of Example 3 shown in Table 4 is a relative maintenance rate, with the capacity maintenance rate of the test battery cell of Comparative Example 3 being 100%.
[0137] The capacity maintenance rate of the test battery cell of Example 4 shown in Table 5 is a relative maintenance rate, with the capacity maintenance rate of the test battery cell of Comparative Example 4 being 100%.
[0138] The capacity maintenance rate of the test battery cell of Example 5 shown in Table 6 is a relative maintenance rate, with the capacity maintenance rate of the test battery cell of Comparative Example 5 being 100%.
[0139] The capacity maintenance rate of the test battery cell of Comparative Example 7 shown in Table 7 is a relative maintenance rate, with the capacity maintenance rate of the test battery cell of Comparative Example 6 being 100%.
[0140] [Table 2]
[0141] Capacity maintenance rate (%) Example 1 101.2 Comparative Example 1 100
[0142] [Table 3]
[0143] Capacity maintenance rate (%) Example 2 101.3 Comparative Example 2 100
[0144] [Table 4]
[0145] Capacity maintenance rate (%) Example 3 101.2 Comparative Example 3 100
[0146] [Table 5]
[0147] Capacity maintenance rate (%) Example 4 101.5 Comparative Example 4 100
[0148] [Table 6]
[0149] Capacity maintenance rate (%) Example 5 101.7 Comparative Example 5 100
[0150] [Table 7]
[0151] Capacity maintenance rate (%) Comparative Example 6 100 Comparative Example 7 100
[0152] Any of Tables 2 to 6 shows that the capacity maintenance rate of the embodiment containing Sr in the surface modification layer is higher than that of the comparative example in which the surface modification layer does not contain Sr. It should be noted that it can be inferred that the surface layer contains more Al than the main body, and further, a part of Al is contained in the surface modification layer. In Table 7, both Comparative Examples 6 and 7 are lithium transition metal composite oxides that do not contain Al, so the capacity maintenance rate does not change due to whether Sr is added.
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium transition metal composite oxide and a surface modification layer, The lithium transition metal composite oxide contains at least Al and 80 mol % or more of Ni relative to the total molar number of metal elements other than Li, The surface modification layer is formed on the surface of the primary particles of the lithium transition metal composite oxide and contains at least Sr and Al. The lithium transition metal composite oxide is represented by the general formula Li a Ni x Al y Co z M w O 2-b wherein 0.95 < a < 1.05, 0.8 ≤ x ≤ 0.96, 0 < y ≤ 0.10, 0 ≤ z ≤ 0.15, 0 ≤ b < 0.05, and x + y + z + w = 1; M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn.
2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The lithium transition metal composite oxide has a surface layer and a main body. The surface layer exists from the surface to the inner side, and the main body exists on the inner side of the surface layer. The ratio of Al in the surface modification layer to the total number of moles of metal elements other than Li is greater than the ratio of Al in the main body to the total number of moles of metal elements other than Li.
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 2, wherein The ratio of Al in the surface layer to the total number of moles of metal elements other than Li is 1.3 times or more the ratio of Al in the main body to the total number of moles of metal elements other than Li.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The ratio of Sr in the surface modification layer is 0.05 mol % to 0.25 mol % relative to the total molar number of metal elements excluding Li in the surface modification layer.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The ratio of Ni to the total number of moles of metal elements other than Li in the lithium transition metal composite oxide is 90 mol % or more.
6. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The amount of Li remaining on the surface of the lithium transition metal composite oxide is 0.03 wt % to 0.08 wt %.
7. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, The positive electrode comprises the positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 6.