Semi-solid battery, energy storage device and electric equipment

By forming a composite electrolyte layer of polymer electrolyte and fiber on the surface of the electrode sheet, the problem of low cycling performance of semi-solid battery is solved, higher ionic conductivity and mechanical strength are achieved, and the overall performance of lithium-ion semi-solid battery is improved. .

CN119092707AActive Publication Date: 2024-12-06XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411178512.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The cycling performance of semi-solid state batteries is low and it is difficult to meet the needs of actual application.

Method used

The composite electrolyte layer is formed on the surface of the electrode sheet, and the layer contains polymer electrolyte and polymer fibers. The polymer fibers are distributed between the electrolytes to form a micro-curved structure, which improves the amorphous area and mechanical properties of the electrolyte, and regulates the composite electrolyte layer. The thickness is to improve ionic conductivity and liquid retention capacity.

Benefits of technology

It significantly improves the cycling performance of lithium-ion semi-solid state batteries, reduces the risk of lithium dendrites and internal short circuits, maintains high liquid retention and tensile strength, and improves the capacity retention and energy efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092707A_ABST
    Figure CN119092707A_ABST
Patent Text Reader

Abstract

The invention provides a semi-solid-state battery, an energy storage device and electric equipment, the semi-solid-state battery comprises an electrode pole piece, the electrode pole piece comprises a current collector and an active material layer, at least one surface of the electrode pole piece comprises a composite electrolyte layer, the composite electrolyte layer comprises a polymer electrolyte and polymer fibers, the polymer fibers are distributed among the polymer electrolytes, and the single-sided thickness of the composite electrolyte layer is 50-100 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a semi-solid battery, an energy storage device and an electrical equipment. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight. They are widely used in various fields such as energy storage, portable electronic devices and electric vehicles.

[0003] Semi-solid electrolytes are a type of electrolyte between liquid electrolytes and pure solid electrolytes. Semi-solid batteries developed based on semi-solid electrolytes have better safety performance, but the cycle performance still needs to be improved. How to improve the cycle performance of semi-solid batteries has become a technical problem that needs to be solved urgently. Summary of the invention

[0004] In order to solve the above technical problems, the present application discloses a semi-solid-state battery, an energy storage device and an electrical equipment to improve the cycle performance of the semi-solid-state battery.

[0005] In the first aspect, the present application provides a semi-solid-state battery, comprising an electrode plate, wherein the electrode plate comprises a current collector and an active material layer, wherein at least one surface of the electrode plate comprises a composite electrolyte layer, wherein the composite electrolyte layer comprises a polymer electrolyte and polymer fibers, wherein the polymer fibers are distributed between the polymer electrolyte, and the single-sided thickness of the composite electrolyte layer is 50 μm to 100 μm.

[0006] In some embodiments of the present application, the composite electrolyte layer is a multilayer structure, each layer in the multilayer structure is a composite electrolyte sublayer formed by the polymer electrolyte and the polymer fiber, and multiple composite electrolyte sublayers are stacked to form the composite electrolyte layer.

[0007] In some embodiments of the present application, the number of layers of the multilayer structure in the composite electrolyte layer is 1 to 3.

[0008] In some embodiments of the present application, the polymer fiber forms a polymer fiber layer, and the polymer fiber layer is embedded in the composite electrolyte layer.

[0009] In some embodiments of the present application, the single-side thickness of the polymer fiber layer is 5 μm to 10 μm.

[0010] In some embodiments of the present application, in the composite electrolyte layer, the ionic conductivity of the polymer electrolyte is 13×10 -4 S / cm~16×10 -4 S / cm.

[0011] In some embodiments of the present application, the electrode plates include a positive electrode plate and a negative electrode plate, and a side of the positive electrode plate having the composite electrolyte layer is arranged opposite to a side of the negative electrode plate having the composite electrolyte layer.

[0012] In some embodiments of the present application, the first polymer material in the polymer electrolyte includes at least one of polyethylene oxide, polymethyl methacrylate, polyacrylonitrile, polyvinylidene fluoride, polypropylene carbonate and polycyanoacrylate.

[0013] In some embodiments of the present application, the second polymer material in the polymer fiber includes at least one of polylactic acid, polycarbonate, polyethylene and polycaprolactone.

[0014] In a second aspect, the present application provides an energy storage device, comprising a housing and at least one semi-solid-state battery as described in the first aspect, wherein the semi-solid-state battery is accommodated in the housing.

[0015] In a third aspect, the present application provides an electrical device, comprising the energy storage device described in the second aspect, wherein the energy storage device supplies power to the electrical device.

[0016] Compared with the prior art, this application has at least the following beneficial effects:

[0017] The present application provides a semi-solid battery, energy storage device and electrical equipment, wherein the semi-solid battery comprises an electrode plate, the electrode plate comprises a current collector and an active material layer, at least one surface of the electrode plate comprises a composite electrolyte layer, the composite electrolyte layer comprises a polymer electrolyte and a polymer fiber, the polymer fiber is distributed between the polymer electrolyte, the single-sided thickness of the composite electrolyte layer is 50 μm to 100 μm, wherein the polymer electrolyte is separated into a large number of micro-bend structures by the polymer fiber, such micro-bend structures are conducive to increasing the amorphous area of ​​the polymer electrolyte and improving the ionic conductivity of the polymer electrolyte; and the polymer fiber improves the mechanical properties of the composite electrolyte layer, effectively reducing the formation of lithium dendrites and the risk of internal short circuit; and the polymer fiber also has an adsorption effect on the polymer electrolyte, improving the liquid retention capacity of the polymer electrolyte. The lithium ion semi-solid battery of the present application has the above structure, and the thickness of the composite electrolyte layer is regulated within the scope of the present application, which is conducive to reducing the ionic conductivity while maintaining a high liquid retention rate and tensile strength, so that the cycle performance of the lithium ion semi-solid battery is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0019] Figure 1 This is a schematic diagram of the structure of an electrode plate according to an embodiment of the present application;

[0020] Figure 2 This is a schematic diagram of the structure of an electrode sheet according to another embodiment of the present application;

[0021] Figure 3 A schematic diagram of the structure of a composite electrolyte layer according to an embodiment of the present application;

[0022] Figure 4 This is a schematic diagram of the structure of an electrode sheet according to another embodiment of the present application;

[0023] Figure 5 A schematic diagram of the structure of a household energy storage system according to an implementation scheme of the present application;

[0024] Figure 6 A schematic diagram of the structure of an energy storage system according to an implementation scheme of the present application.

[0025] Explanation of the accompanying drawings: 1-energy storage device, 2-electric energy conversion device, 3-first user load, 4-second user load, 10-electrode plate, 11-current collector, 12-active material layer, 13-composite electrolyte layer, 131-polymer electrolyte, 132-polymer fiber, 133-composite electrolyte sublayer, 400-energy storage system, 410-high voltage cable, 420-first electric energy conversion device, 430-second electric energy conversion device. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0027] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings. These terms are mainly used to better describe the present application and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific orientation, or to be constructed and operated in a specific orientation.

[0028] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.

[0029] In addition, the terms "installed", "set", "provided with", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0030] In addition, the terms "first", "second", etc. are mainly used to distinguish different devices, elements or components (the specific types and structures may be the same or different), and are not used to indicate or imply the relative importance and quantity of the indicated devices, elements or components. Unless otherwise specified, "plurality" means two or more.

[0031] It should be noted that, in the content of the present application, lithium-ion semi-solid-state batteries are used as an example of semi-solid-state batteries to explain the present application, but the semi-solid-state batteries of the present application are not limited to lithium-ion semi-solid-state batteries.

[0032] The present application provides a semi-solid-state battery, such as Figure 1 As shown, the semi-solid battery includes an electrode plate 10, the electrode plate includes a current collector 11 and an active material layer 12, and at least one surface of the electrode plate includes a composite electrolyte layer 13, specifically, the composite electrolyte layer can be located on the surface of the active material layer. The composite electrolyte layer includes a polymer electrolyte 131 and polymer fibers 132, the polymer fibers are distributed between the polymer electrolytes, and the single-sided thickness of the composite electrolyte layer is 50μm to 100μm. For example, the single-sided thickness of the composite electrolyte layer is 50μm, 60μm, 70μm, 80μm, 90μm or 100μm.

[0033] The inventors have found that the conduction of lithium ions in polymer electrolytes mainly includes the coordination process and dissociation process of lithium ions and oxygen functional groups. Due to the action of the electric field, lithium ions and oxygen functional groups are continuously coordinated and dissociated, and are rapidly conducted with the thermal motion of the polymer chain segments. The conduction of lithium ions mainly includes the local movement within and between the chains of the polymer chain segments, and the migrating ions include ions and ion clusters. The migration rate of lithium ions in the amorphous phase is much higher than the migration rate in the crystalline phase, and the ionic conductivity in the amorphous phase is usually 2 to 3 orders of magnitude higher. Based on the above findings, in the electrode pole piece of the semi-solid battery of the present application, the polymer electrolyte is separated into a large number of micro-bend structures by polymer fibers, which is conducive to increasing the area of ​​the amorphous region of the polymer electrolyte, thereby facilitating the improvement of the ionic conductivity of the polymer electrolyte and improving the migration rate of lithium ions; and the polymer fibers improve the mechanical properties of the composite electrolyte layer, effectively reducing the formation of lithium dendrites and the risk of internal short circuits; and the polymer fibers also have an adsorption effect on the polymer electrolyte, improving the liquid retention capacity of the polymer electrolyte. The inventors also found that the thickness of the composite electrolyte layer should not be too small or too large. When the thickness of the composite electrolyte layer is too small (for example, less than 50 μm), the liquid retention capacity of the polymer electrolyte decreases, and at the same time, the mechanical strength of the composite electrolyte layer decreases significantly, resulting in a decrease in the mechanical strength of the electrode plate, which is not conducive to improving the cycle performance of the lithium-ion semi-solid battery; when the thickness of the composite electrolyte layer is too large (for example, greater than 100 μm), the ionic conductivity decreases significantly, which is also not conducive to improving the cycle performance of the lithium-ion semi-solid battery. The lithium-ion semi-solid battery of the present application has the above structure, and the thickness of the composite electrolyte layer is adjusted within the scope of the present application, which is conducive to reducing the ionic conductivity while maintaining a high liquid retention rate and tensile strength, so that the cycle performance of the lithium-ion semi-solid battery is improved.

[0034] In the present application, at least one surface of the electrode plate includes a composite electrolyte layer, such as Figure 1 As shown, the composite electrolyte layer 13 may be included on one surface of the electrode plate; or Figure 2 As shown, both surfaces of the electrode plate include a composite electrolyte layer 13 .

[0035] In some embodiments of the present application, Figure 3 As shown, the composite electrolyte layer 13 can be a multilayer structure, each layer in the multilayer structure is a composite electrolyte sublayer 133 formed by a polymer electrolyte and a polymer fiber, and multiple composite electrolyte sublayers are stacked to form a composite electrolyte layer. The composite electrolyte layer of the present application can be a single-layer structure; or, the composite electrolyte layer can be a multilayer structure, which is conducive to enhancing the mechanical strength of the composite electrolyte layer and preventing lithium dendrites from piercing the composite electrolyte layer and causing internal short circuits.

[0036] In some embodiments of the present application, the number of layers of the multilayer structure in the composite electrolyte layer is 1 to 3, for example, the number of layers of the multilayer structure is 1, 2 or 3. This is beneficial to enhancing the mechanical strength of the composite electrolyte layer, preventing lithium dendrites from piercing the composite electrolyte layer and causing internal short circuits, while reducing ionic conductivity and internal resistance, which is beneficial to improving the capacity, capacity retention rate and energy efficiency of lithium-ion semi-solid batteries.

[0037] In some embodiments of the present application, the polymer fibers form a polymer fiber layer, and the polymer fiber layer is embedded in the composite electrolyte layer. In this way, the polymer fiber layer in the composite electrolyte layer can be fully distributed between the polymer electrolytes, which is beneficial to improve the ionic conductivity of the polymer electrolyte.

[0038] In some embodiments of the present application, the single-side thickness of the polymer fiber layer is 5 μm to 10 μm, for example, the single-side thickness is 5 μm, 7 μm, 9 μm or 10 μm. By adjusting the single-side thickness of the polymer fiber layer within the above range, it is beneficial to obtain a polymer fiber layer with good liquid retention capacity and mechanical strength.

[0039] In some embodiments of the present application, in the composite electrolyte layer, the ionic conductivity of the polymer electrolyte is 13×10 -4 S / cm~16×10 -4 S / cm. For example, the ionic conductivity of polymer electrolytes is 13×10 -4 S / cm, 14×10 -4 S / cm, 15×10 -4 S / cm or 16×10 -4 S / cm, with excellent ionic conductivity.

[0040] In some embodiments of the present application, Figure 4 As shown, the electrode plates include a positive electrode plate and a negative electrode plate, and the positive electrode plate has a side with a composite electrolyte layer 13 and the negative electrode plate has a side with a composite electrolyte layer 13. In this way, it is beneficial to obtain the lithium ion semi-solid battery of the present application. Figure 4 In the embodiment, when the upper electrode plate is a positive electrode plate, the lower electrode plate can be a negative electrode plate; when the upper electrode plate is a negative electrode plate, the lower electrode plate can be a positive electrode plate. There is no special limitation in this application.

[0041] In some embodiments of the present application, the first polymer material in the polymer electrolyte includes at least one of polyethylene oxide (PEO), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polypropylene carbonate (PPC) and polycyanoacrylate (PCA).

[0042] In some embodiments of the present application, the second polymer material in the polymer fiber includes at least one of polylactic acid (PLA), polycarbonate (PC), polyethylene (PE) and polycaprolactone (PCL).

[0043] The present application has no particular restrictions on the preparation method of the composite electrolyte layer, as long as the composite electrolyte layer of the present application can be obtained. Exemplarily, the composite electrolyte layer can be prepared by the following preparation steps:

[0044] Preparation of polymer electrolyte glue: a first polymer material and a first solvent are mixed in a mass ratio of 1:8 to 1:10, and stirred to form a first glue; wherein the first solvent can be selected from at least one of deionized water, ethanol, ethyl acetate, isopropanol, N,N-dimethylformamide, cyclohexane, N-methylpyrrolidone, and tetrahydrofuran; then a photocuring agent is added to the first glue and stirred evenly to obtain a second glue, wherein the content of the photocuring agent in the second glue is 0.3wt% to 0.6wt%; then a liquid electrolyte is added to the second glue and stirred evenly to obtain a polymer electrolyte glue, wherein the content of the liquid electrolyte in the polymer electrolyte glue is 8wt% to 12wt%;

[0045] Preparation of electrospinning solution: mixing the second polymer material and the second solvent at a mass ratio of 1:15 to 1:25, and stirring evenly to obtain an electrospinning solution; the second solvent can be selected from at least one of methanol, ether, acetone, propanol, methyl acetate, N,N-dimethylformamide, dimethyl sulfoxide, and tetrahydrofuran;

[0046] Preparation of composite electrolyte layer:

[0047] Step S1, coating the surface of the active material layer of the electrode plate with a polymer electrolyte glue to form a polymer electrolyte coating, and then spraying the electrospinning solution on the surface of the polymer electrolyte coating through an electrospinning device to form polymer fibers, the polymer fibers are infiltrated by the uncured polymer electrolyte coating and embedded in the polymer electrolyte coating to form an initial structure of the composite electrolyte layer;

[0048] Step S2, placing the electrode plate with the initial structure of the composite electrolyte layer obtained in step S1 under a light source for irradiation for 60s to 120s, and the polymer electrolyte coating in the initial structure of the composite electrolyte layer is cured after being exposed to light to form the composite electrolyte layer structure of the present application.

[0049] In an optional embodiment, step S1 can be repeated to obtain a multi-layer composite electrolyte layer initial structure, and then uniformly photocured, which is beneficial to improve the interface contact effect between layers; in another optional embodiment, after obtaining a layer of composite electrolyte layer initial structure, the composite electrolyte layer initial structure can be photocured separately, which is beneficial to more accurately control the thickness of the composite electrolyte layer.

[0050] The present application has no particular restrictions on liquid electrolytes, and those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, after mixing at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl propionate (EP), propyl propionate (PP), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate (VC) or fluoroethylene carbonate (FEC) in a certain mass ratio or volume ratio to obtain a non-aqueous organic solvent, add a lithium salt to dissolve and mix evenly. The present application has no restrictions on the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include LiPF 6 , LiBF 4 、LiAsF 6 、LiClO 4 、LiB(C 6 H 5 ) 4 、LiCH 3 SO 3 、LiCF 3 SO 3 、LiN(SO 2 CF 3 ) 2 、LiC(SO 2 CF 3 ) 3 、LiSiF 6 At least one of lithium bis(oxalatoborate) (LiBOB) or lithium difluoroborate. The present application has no particular limitation on the concentration of the lithium salt in the liquid electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt is 1.0 mol / L to 2.0 mol / L.

[0051] The thickness of the polymer fiber layer generally increases with the spraying time and / or spraying amount of electrospinning. The thickness of the polymer fiber layer can be adjusted by regulating the spraying time and / or spraying amount during electrospinning, and the present application has no particular limitation.

[0052] It can be understood that the thickness of the composite electrolyte layer is mainly affected by the thickness of the polymer electrolyte coating. Based on this, the present application can control the thickness of the polymer electrolyte coating by adjusting the coating amount of the polymer electrolyte glue, thereby adjusting the thickness of the composite electrolyte layer.

[0053] The photocuring agent of the present application can be at least one of 2,4,6-trimethylbenzoyl ethyl phosphate, 4-dimethylamino-ethyl benzoate, 1-hydroxy-cycloethyl-phenyl ketone, and 2-hydroxy-2-methyl-1-phenyl-1-propanone. Photocuring has the advantages of simple reaction equipment, short reaction time, and good controllability. When preparing the composite electrolyte layer structure, the initial structure of the composite electrolyte layer can be cured by the photocuring method.

[0054] The semi-solid battery of the present application includes a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet generally includes a positive current collector and a positive active material layer. The positive active material layer can be arranged on one surface in the thickness direction of the positive current collector, or on two surfaces in the thickness direction of the positive current collector. In the present application, the positive active material layer is arranged on the surface of the positive current collector, that is, the positive active material layer can be arranged in a partial area of ​​one surface of the positive current collector, or in the entire area of ​​one surface of the positive current collector. The present application has no special restrictions on the positive current collector, as long as the purpose of the present application can be achieved, for example, it can include but is not limited to aluminum foil, aluminum alloy foil or composite current collector. In the present application, there is no special restriction on the thickness of the positive current collector, as long as the purpose of the present application can be achieved, for example, the thickness is 8μm to 13μm. The single-sided thickness of the positive active material layer of the present application can be 100μm to 200μm.

[0055] In the present application, the positive electrode active material layer includes a positive electrode active material. The present application has no particular limitation on the positive electrode active material as long as the purpose of the present application can be achieved. For example, it may include at least one of lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide and lithium iron manganese phosphate.

[0056] In the present application, the positive electrode active material layer may also include a positive electrode binder. The present application has no particular limitation on the positive electrode binder as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of fluorine-containing resins, polypropylene resins, fiber-type binders, rubber-type binders or polyimide-type binders.

[0057] The negative electrode sheet generally includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer can be arranged on one surface or both surfaces in the thickness direction of the negative electrode current collector. In the present application, the negative electrode active material layer is arranged on the surface of the negative electrode current collector, that is, the negative electrode active material layer can be arranged in a partial area of ​​one surface of the negative electrode current collector, or can be arranged in the entire area of ​​one surface of the negative electrode current collector. The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, it can include but is not limited to copper foil, copper alloy foil, nickel foil or composite current collector, etc. In the present application, there is no special restriction on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness is 4μm to 12μm. The single-sided thickness of the negative electrode active material layer of the present application can be 70μm to 200μm.

[0058] In the present application, the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode active material is not particularly limited as long as the purpose of the present application can be achieved, for example, it may include at least one of artificial graphite, natural graphite, mesophase carbon microbeads, silicon, and silicon carbon.

[0059] In the present application, the negative electrode active material layer may further include a negative electrode binder. The present application has no particular restrictions on the negative electrode binder, as long as the purpose of the present application can be achieved, for example, it may include at least one of acrylate, polyamide, polyimide, polyamideimide, polyvinylidene fluoride (PVDF), styrene-butadiene rubber, sodium alginate, polyvinyl alcohol, polytetrafluoroethylene, and sodium carboxymethyl cellulose.

[0060] The lithium-ion semi-solid battery of the present application also includes a shell, and the present application has no particular limitation on the shell, and those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved. For example, the shell may include an aluminum-plastic film.

[0061] The present application does not particularly limit the preparation method of the semi-solid battery, and a preparation method known in the art can be selected as long as the purpose of the present application can be achieved. For example, the preparation method of the lithium-ion semi-solid battery includes but is not limited to the following steps: stacking the positive electrode sheet and the negative electrode sheet in order, and placing the side of the positive electrode sheet with the composite electrolyte layer opposite to the side of the negative electrode sheet with the composite electrolyte layer, and winding and folding the sheet as needed to obtain a bare cell with a wound structure, and placing the bare cell in a packaging bag to obtain a lithium-ion semi-solid battery.

[0062] The present application also provides an energy storage device, comprising a housing and at least one semi-solid-state battery in any of the above embodiments, wherein the lithium-ion semi-solid-state battery is contained in the housing. The energy storage device having the semi-solid-state battery has excellent performance, which is beneficial to the use of the energy storage device. By containing the semi-solid-state battery in the housing, the fixation and protection of the semi-solid-state battery can be increased, thereby improving the service life of the energy storage device. It is understandable that the energy storage device may have one or more semi-solid-state batteries, and when the energy storage device contains multiple semi-solid-state batteries, the multiple semi-solid-state batteries may be connected in at least one of parallel and series connection.

[0063] The present application also provides an electrical device, including the energy storage device in the above-mentioned implementation scheme, which is conducive to improving the product competitiveness and performance of the electrical device. In an optional implementation scheme, the electrical device includes an electrical device body, and the energy storage device is used to supply power to the electrical device body. In an optional implementation scheme, the electrical device body includes a positive electrode of the device and a negative electrode of the device, and the positive electrode plate of the lithium-ion semi-solid battery in the energy storage device is used to electrically connect to the device positive electrode of the electrical device body, and the negative electrode plate of the lithium-ion semi-solid battery in the energy storage device is used to electrically connect to the device negative electrode of the electrical device body to supply power to the electrical device.

[0064] The electrical equipment of the present application may include but is not limited to: containers, household energy storage systems, battery vehicles, electric vehicles, ships, spacecraft, electric toys and electric tools, etc., wherein spacecrafts include airplanes, rockets, space shuttles and spacecrafts, etc., electric toys include fixed or mobile electric toys, such as electric car toys, electric ship toys and electric airplane toys, etc., and electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.

[0065] See also Figure 5 , Figure 5 This is a schematic diagram of the structure of a household energy storage system according to an implementation scheme of the present application, and the present application Figure 5 The implementation plan is described using a household energy storage scenario in user-side energy storage as an example, but the energy storage device of the present application is not limited to the household energy storage scenario.

[0066] The present application provides a household energy storage system, which includes an energy conversion device 2 (photovoltaic panel), a first user load 3 (street lamp), a second user load 4 (such as air conditioner and other household appliances), and an energy storage device 1. The energy storage device 1 is a small energy storage box that can be mounted on an outdoor wall by wall hanging. Specifically, the photovoltaic panel can convert solar energy into electrical energy during the period of low electricity prices. The energy storage device 1 is used to store the electrical energy and supply it to street lamps and household appliances for use during the peak electricity prices, or to supply power when the power grid is out of power / power outage.

[0067] See also Figure 6 , Figure 6 This is a schematic diagram of the structure of an energy storage system 400 according to an implementation scheme of the present application, and the present application Figure 6 The implementation plan is described using the shared energy storage scenario on the generation / distribution side as an example, and the energy storage device 1 of the present application is not limited to the energy storage scenario on the generation / distribution side.

[0068] The present application provides an energy storage system 400, which includes: a high-voltage cable 410, a first electric energy conversion device 420, a second electric energy conversion device 430 and an energy storage device 1 provided in the present application. In the case of power generation, the first electric energy conversion device 420 and the second electric energy conversion device 430 are used to convert other forms of energy into electric energy, which are connected to the high-voltage cable 410 and supplied to the power distribution network for use. When the power load is low and the first electric energy conversion device 420 and the second electric energy conversion device 430 generate excess power, the excess power is stored in the energy storage device 1, thereby reducing the wind and solar power abandonment rates and improving the problem of new energy power generation and consumption. When the power load is high, the power grid issues an instruction to transmit the power stored in the energy storage device 1 in conjunction with the high-voltage cable 410 in a grid-connected mode to the power consumption side, thereby providing peak shaving, frequency regulation, standby and other services for the power grid operation, giving full play to the peak shaving role of the power grid, promoting peak shaving and valley filling of the power grid, and alleviating the power supply pressure of the power grid.

[0069] Optionally, the first electric energy conversion device 420 and the second electric energy conversion device 430 can convert at least one of solar energy, light energy, wind energy, thermal energy, tidal energy, biomass energy and mechanical energy into electric energy.

[0070] The number of energy storage devices 1 can be multiple, and multiple energy storage devices 1 are connected in series or in parallel. Multiple energy storage devices 1 are supported and electrically connected by isolation plates (not shown). In this embodiment, "multiple" refers to two or more. An energy storage box can also be provided outside the energy storage device 1 to accommodate the energy storage device 1.

[0071] Optionally, the energy storage device 1 may include but is not limited to a battery module, a battery pack, a battery system, etc. Among them, the battery module may be a battery module formed by connecting multiple lithium-ion semi-solid batteries of the present application in series / parallel, the battery pack may include multiple lithium-ion semi-solid batteries of the present application, and the battery system may be a charging and discharging system including the lithium-ion semi-solid battery or battery pack of the present application.

[0072] The actual application form of the energy storage device 1 provided in the embodiment of the present application may be, but is not limited to, the listed products, and may also be other application forms. The embodiment of the present application does not strictly limit the application form of the energy storage device 1. The embodiment of the present application only takes the energy storage device 1 as a multi-core battery as an example for explanation. When the energy storage device 1 is a single battery, the energy storage device 1 may be at least one of a cylindrical battery, a square battery, and the like.

[0073] Example

[0074] Hereinafter, the embodiments of the present application will be described in more detail with reference to preparation examples, examples and comparative examples. Various tests and evaluations were performed according to the following methods.

[0075] Example 1

[0076] <Preparation of polymer electrolyte gel>

[0077] The first polymer material (PEO and PMMA are mixed in a mass ratio of 1:1) is mixed with the first solvent N-methylpyrrolidone (NMP) in a mass ratio of 1:10, and stirred to form a first glue solution, and then a photocuring agent is added to the first glue solution and stirred evenly to obtain a second glue solution, and the content of the photocuring agent in the second glue solution is 0.5wt%; then a liquid electrolyte is added to the second glue solution and stirred evenly to obtain a polymer electrolyte glue solution, and the content of the liquid electrolyte in the polymer electrolyte glue solution is 10wt%. The preparation process of the liquid electrolyte is as follows: in an argon atmosphere glove box with a moisture content of ≤1ppm, ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) are mixed in a mass ratio of 1:1:1, and then lithium salt LiPF is added. 6 And dissolved in the above solvent, mixed evenly to obtain the electrolyte. Among them, LiPF 6 The molar concentration in the electrolyte is 1 mol / L.

[0078] <Preparation of electrospinning solution>

[0079] The second polymer material PLA and the second solvent N,N-dimethylformamide are mixed at a mass ratio of 1:20 and stirred evenly to obtain an electrospinning solution.

[0080] <Preparation of positive electrode sheet>

[0081] The positive electrode active material lithium iron phosphate (LiFePO 4 ), conductive carbon black (Super-P), and binder PVDF are mixed in a mass ratio of 97:0.7:2.3; then NMP is added as a solvent to prepare a positive electrode slurry with a solid content of 60wt%, and stirred evenly, and then the positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 85°C; then, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode active material layer. Among them, the single-sided thickness of the positive electrode active material layer is 100μm;

[0082] The polymer electrolyte gel is coated on one surface of the above-mentioned positive electrode active material layer to form a polymer electrolyte coating, and then the electrostatic spinning liquid is sprayed on the surface of the polymer electrolyte coating by an electrostatic spinning device to form polymer fibers. After the polymer fibers are infiltrated by the uncured polymer electrolyte coating and embedded in the polymer electrolyte coating, the initial structure of the composite electrolyte layer is formed; then the positive electrode sheet with the initial structure of the composite electrolyte layer is placed under a light source for irradiation for 60 seconds, and the polymer electrolyte coating in the initial structure of the composite electrolyte layer is cured after being exposed to light to form a composite electrolyte layer; then, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a composite electrolyte layer on both sides. The single-sided thickness of the composite electrolyte layer is 50μm, and the single-sided thickness of the polymer fiber layer is 5μm.

[0083] <Preparation of negative electrode sheet>

[0084] The negative electrode active material artificial graphite, conductive carbon black (Super-P), thickener carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96.5:0.5:1:2, and deionized water is added to prepare a negative electrode slurry with a solid content of 50wt%, and stirred evenly. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 85°C; then, the above steps are repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of a negative electrode active material layer. Among them, the single-sided thickness of the negative electrode active material layer is 70μm;

[0085] The polymer electrolyte glue is coated on one surface of the above-mentioned negative electrode active material layer to form a polymer electrolyte coating, and then the electrostatic spinning liquid is sprayed on the surface of the polymer electrolyte coating by an electrostatic spinning device to form polymer fibers. After the polymer fibers are infiltrated by the uncured polymer electrolyte coating and embedded in the polymer electrolyte coating, the initial structure of the composite electrolyte layer is formed; then the negative electrode sheet with the initial structure of the composite electrolyte layer is placed under a light source for irradiation for 60 seconds, and the polymer electrolyte coating in the initial structure of the composite electrolyte layer is cured after being exposed to light to form a composite electrolyte layer; then, the above steps are repeated on the other surface of the copper foil to obtain a negative electrode sheet with a composite electrolyte layer on both sides. The single-sided thickness of the composite electrolyte layer is 50μm, and the single-sided thickness of the polymer fiber layer is 5μm.

[0086] <Preparation of lithium-ion semi-solid batteries>

[0087] The positive electrode sheets and negative electrode sheets prepared as above are stacked in order, and the side of the positive electrode sheet with the composite electrolyte layer is arranged opposite to the side of the negative electrode sheet with the composite electrolyte layer, and assembled into a button battery. The specific assembly order from bottom to top is negative electrode shell → negative electrode sheet → diaphragm → positive electrode sheet → gasket → spring → positive electrode shell. The assembled button battery is subjected to packaging, standing, formation and other processes to obtain a button lithium ion semi-solid battery. The shell size of the button battery used is 2430 model, the positive electrode sheet size is 14 mm in diameter, the negative electrode sheet size is 16 mm in diameter, and the diaphragm size is 19 mm in diameter.

[0088] Embodiment 2 to Embodiment 5

[0089] Except that the single-side thickness of the composite electrolyte layer is adjusted according to Table 1 in <Preparation of positive electrode sheet> and <Preparation of negative electrode sheet>, the rest is the same as Example 1.

[0090] Embodiment 6 to Embodiment 7

[0091] Except that the single-side thickness of the polymer fiber layer is adjusted according to Table 1 in <Preparation of positive electrode sheet> and <Preparation of negative electrode sheet>, the rest is the same as Example 5.

[0092] Embodiment 8~embodiment 10

[0093] Except that the types of the first polymer material and the second polymer material are adjusted according to Table 2 in <Preparation of positive electrode sheet> and <Preparation of negative electrode sheet>, the rest is the same as Example 5.

[0094] Embodiment 11

[0095] Except that <Preparation of positive electrode sheet> and <Preparation of negative electrode sheet> are different from those in Example 5, the rest are the same as those in Example 5.

[0096] <Preparation of positive electrode sheet>

[0097] The positive electrode active material lithium iron phosphate (LiFePO 4 ), conductive carbon black (Super-P), and binder PVDF are mixed in a mass ratio of 97:0.7:2.3; then N-methylpyrrolidone (NMP) is added as a solvent to prepare a positive electrode slurry with a solid content of 60wt%, and stirred evenly, and then the positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 85°C; then, the above steps are repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided positive electrode active material layer. Among them, the single-sided thickness of the positive electrode active material layer is 100μm;

[0098] Step 1: Apply the polymer electrolyte glue on one surface of the above-mentioned positive electrode active material layer to form a polymer electrolyte coating, and then spray the electrospinning liquid on the surface of the polymer electrolyte coating through an electrospinning device to form polymer fibers. After the polymer fibers are infiltrated by the uncured polymer electrolyte coating and embedded in the polymer electrolyte coating, the initial structure of the first composite electrolyte sublayer is formed, and the single-sided thickness of the polymer fiber layer in the structure is 5μm; repeat the above step 1 to form the initial structure of the second composite electrolyte sublayer, and the single-sided thickness of the polymer fiber layer in the structure is 5μm; Step 2: Place the obtained positive electrode plate under a light source for irradiation for 60s, and the polymer electrolyte coating in the first composite electrolyte sublayer and the second composite electrolyte sublayer is cured after being exposed to light to form a composite electrolyte layer with a multilayer structure. Afterwards, repeat the above steps 1 and 2 on the other surface of the aluminum foil to obtain a positive electrode plate with a composite electrolyte layer on both sides. Among them, the total single-sided thickness of the composite electrolyte layer is 100μm, and the total single-sided thickness of the polymer fiber layer is 10μm.

[0099] <Preparation of negative electrode sheet>

[0100] The negative electrode active material artificial graphite, conductive carbon black (Super-P), thickener carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96.5:0.5:1:2, and deionized water is added to prepare a negative electrode slurry with a solid content of 50wt%, and stirred evenly. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 85°C; then, the above steps are repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of a negative electrode active material layer. Among them, the single-sided thickness of the negative electrode active material layer is 70μm;

[0101] Step 1', apply the polymer electrolyte glue on one surface of the above-mentioned negative electrode active material layer to form a polymer electrolyte coating, and then spray the electrospinning liquid on the surface of the polymer electrolyte coating through an electrospinning device to form polymer fibers. After the polymer fibers are infiltrated by the uncured polymer electrolyte coating and embedded in the polymer electrolyte coating, the initial structure of the first composite electrolyte sublayer is formed, and the single-sided thickness of the polymer fiber layer in the structure is 5μm; repeat the above step 1' to form the initial structure of the second composite electrolyte sublayer, and the single-sided thickness of the polymer fiber layer in the structure is 5μm; step 2', place the obtained negative electrode plate under a light source for irradiation, the irradiation time is 60s, and the polymer electrolyte coating in the first composite electrolyte sublayer and the second composite electrolyte sublayer is cured after being exposed to light to form a composite electrolyte layer with a multi-layer structure. Afterwards, repeat the above steps 1' and 2' on the other surface of the aluminum foil to obtain a negative electrode plate with a composite electrolyte layer on both sides. Among them, the total thickness of the single side of the composite electrolyte layer is 100μm, and the total thickness of the single side of the polymer fiber layer is 10μm.

[0102] Comparative Example 1

[0103] The process is the same as Example 1 except that in <Preparation of Positive Electrode Plate> and <Preparation of Negative Electrode Plate>, electrospinning solution is not sprayed on the surface of the polymer electrolyte coating, that is, the formed electrolyte layer does not contain polymer fibers.

[0104] Comparative Example 2

[0105] The above process is the same as Example 3 except that in the steps of <Preparation of Positive Electrode Plate> and <Preparation of Negative Electrode Plate>, electrospinning solution is not sprayed on the surface of the polymer electrolyte coating, that is, the formed electrolyte layer does not contain polymer fibers.

[0106] Comparative Example 3

[0107] The above process is the same as Example 5 except that in the steps of <Preparation of Positive Electrode Plate> and <Preparation of Negative Electrode Plate>, electrospinning solution is not sprayed on the surface of the polymer electrolyte coating, that is, the formed electrolyte layer does not contain polymer fibers.

[0108] Comparative Example 4 to Comparative Example 5

[0109] Except that the single-side thickness of the composite electrolyte layer is adjusted according to Table 1 in <Preparation of positive electrode sheet> and <Preparation of negative electrode sheet>, the rest is the same as Example 1.

[0110] Table 1 Relevant preparation parameters of Examples 1 to 7 and Comparative Examples 1 to 5

[0111]

[0112] Note: In Table 1, “ / ” indicates that there is no relevant preparation parameter.

[0113] Table 2 Relevant preparation parameters of Example 5, Example 8 to Example 10

[0114] First polymer material type Second polymer material type Example 5 PEO:PMMA=1:1 PLA Example 8 PAN:PVDF=1:1 PE Example 9 PPC:PCA=1:1 PC Example 10 PEO:PMMA=1:3 PLA

[0115] Test methods and equipment:

[0116] Ionic conductivity test:

[0117] In an argon atmosphere glove box, the gel polymer electrolyte was assembled into a simulated button cell of stainless steel / polymer electrolyte / stainless steel structure. After standing for 12 hours, the electrochemical impedance spectroscopy (EIS) test was carried out using the Princeton electrochemical test system. The test frequency range was 0.1 Hz to 10 kHz and the excitation voltage was 5 mV. The ionic conductivity δ of the polymer electrolyte was calculated according to formula (1), where l is the thickness of the polymer electrolyte membrane, S is the area of ​​the polymer electrolyte membrane, and Re is the bulk resistance of the polymer electrolyte membrane.

[0118] δ=l / (Re·S) (1)

[0119] Liquid retention rate test:

[0120] In an argon atmosphere glove box, the polymer electrolyte was coated on a flat glass plate at different thicknesses, and then cured by light to form a semi-solid electrolyte film layer, which was weighed and recorded as m. 1 ; Then keep it in a dry culture dish for 7 days and weigh it again, recorded as m 2 , liquid retention rate = (m 2 / m 1 )×100%.

[0121] Tensile strength test:

[0122] The cured polymer electrolyte membrane (thickness of 50 μm) was cut into strips of 7 cm in length and 2.5 cm in width using a dumbbell-shaped cutter. The strips were subjected to a tensile test using a universal material testing machine at a tensile speed of 10 mm / min. The ratio of the maximum force F that the strip bears when it is broken during the tensile process to the original cross-sectional area S of the strip is called the tensile strength σ (as shown in formula (2)), in MPa.

[0123] σ=F / S (2)

[0124] Cycle retention test:

[0125] The button-type lithium-ion semi-solid batteries prepared in each embodiment and comparative example were subjected to constant current charge and discharge tests at 0.1 times (C) and 1C (1C = 160 mA / g), respectively, with a charging voltage of 2.5V to 4.2V, and the capacity retention rate after the cycle was calculated. The capacity retention rate calculation formula is: 200 times (cls) cycle capacity retention rate = (discharge capacity after the 200th cycle / discharge capacity of the first cycle) × 100%.

[0126] Table 3 Performance data of each embodiment and comparative example

[0127]

[0128] In combination with Table 1 and Table 3, it can be seen from Example 1 and Comparative Example 1, Example 3 and Comparative Example 2, and Example 5 and Comparative Example 3 that when there is no polymer fiber in the electrolyte layer (for example, Comparative Examples 1 to Comparative Examples 3), that is, the lithium ion semi-solid battery does not have the composite electrolyte layer of the present application, the ionic conductivity, liquid retention rate and tensile strength performance of Comparative Examples 1 to Comparative Examples 3 are significantly low, resulting in the 0.1C cycle discharge capacity retention rate and 1C cycle discharge capacity retention rate of the battery being significantly low; while the lithium ion semi-solid battery of Example 1 of the present application has a composite electrolyte layer, and its ionic conductivity, liquid retention rate and tensile strength are significantly improved compared with Comparative Example 1, thereby significantly improving the 0.1C cycle discharge capacity retention rate and 1C cycle discharge capacity retention rate; similarly, the cycle performance of the lithium ion semi-solid batteries of Examples 3 and 5 of the present application is also significantly improved compared with Comparative Examples 2 and Comparative Example 3, respectively.

[0129] The single-sided thickness of the composite electrolyte layer and the single-sided thickness of the polymer fiber layer in the electrode plate will usually also affect the performance of the lithium-ion semi-solid-state battery. It can be seen from Examples 1 to 7 that, on the basis of having the composite electrolyte layer structure of the present application, by regulating the above parameters within the scope of the present application, it is beneficial to improve the ionic conductivity while maintaining a high liquid retention rate and tensile strength, thereby improving the cycle performance of the lithium-ion semi-solid-state battery.

[0130] It can be seen from Example 1 and Comparative Examples 4 to 5 that when the thickness of the single-sided composite electrolyte layer in the electrode plate is too thin (such as Comparative Example 4), the ionic conductivity, liquid retention rate and tensile strength performance of the lithium-ion semi-solid-state battery are low, resulting in significantly low 0.1C cycle discharge capacity retention rate and 1C cycle discharge capacity retention rate of the battery. This may be due to the fact that the composite electrolyte layer is too thin, and the storage space for the liquid in the polymer electrolyte is insufficient, resulting in excessive consumption of the electrolyte, and the mechanical strength of the composite electrolyte layer is reduced. The reduction in strength will further lead to a reduction in the inhibitory effect on interfacial lithium precipitation, and there is a risk of piercing the electrolyte layer and causing a short circuit. risk; when the single-sided thickness of the composite electrolyte layer in the electrode pole piece is too thick (for example, in Comparative Example 5), although the lithium-ion semi-solid-state battery has a high tensile strength, the ionic conductivity is significantly low, resulting in low 0.1C cycle discharge capacity retention rate and 1C cycle discharge capacity retention rate of the battery. This may be due to the excessive thickness of the composite electrolyte layer, which increases the internal impedance of the composite electrolyte layer and affects the battery cycle performance; by regulating the single-sided thickness of the composite electrolyte layer in the electrode pole piece within the scope of this application, it is beneficial to reduce the ionic conductivity while maintaining a high liquid retention rate and tensile strength, so that the lithium-ion semi-solid-state battery exhibits excellent cycle performance.

[0131] The type of the first polymer material and the type of the second polymer material will usually also affect the local performance of the lithium-ion semi-solid-state battery. It can be seen from Examples 5 and 8 to 10 that, on the basis of having the composite electrolyte layer structure of the present application, by regulating the above parameters within the scope of the present application, it is beneficial to improve the ionic conductivity while maintaining a high liquid retention rate and tensile strength, thereby improving the cycle performance of the lithium-ion semi-solid-state battery.

[0132] It can be seen from Example 11 and Example 5 that the ionic conductivity, liquid retention rate and tensile strength of the lithium ion semi-solid battery with a multilayer structure are further improved, so that the cycle performance of the lithium ion semi-solid battery is further improved.

[0133] The above is a detailed introduction to a semi-solid-state battery, energy storage device and electrical equipment disclosed in the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solutions and core invention points of the embodiments of the present application. At the same time, for general technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A semi-solid-state battery, characterized in that: The invention comprises an electrode plate, wherein the electrode plate comprises a current collector and an active material layer, wherein: At least one surface of the electrode plate comprises a composite electrolyte layer, wherein the composite electrolyte layer comprises a polymer electrolyte and polymer fibers, wherein the polymer fibers are distributed between the polymer electrolytes, and the single-side thickness of the composite electrolyte layer is 50 μm to 100 μm.

2. The semi-solid-state battery according to claim 1, characterized in that: The composite electrolyte layer is a multi-layer structure, each layer in the multi-layer structure is a composite electrolyte sub-layer formed by the polymer electrolyte and the polymer fiber, and a plurality of composite electrolyte sub-layers are stacked to form the composite electrolyte layer.

3. The semi-solid-state battery according to claim 2, characterized in that: The number of layers of the multilayer structure in the composite electrolyte layer is 1 to 3.

4. The semi-solid-state battery according to claim 1, characterized in that: The polymer fibers form a polymer fiber layer, and the polymer fiber layer is embedded in the composite electrolyte layer.

5. The semi-solid-state battery according to claim 4, characterized in that: The single-side thickness of the polymer fiber layer is 5 μm to 10 μm.

6. The semi-solid-state battery according to claim 1, characterized in that: In the composite electrolyte layer, the ionic conductivity of the polymer electrolyte is 13×10 -4 S / cm~16×10 -4 S / cm.

7. The semi-solid-state battery according to claim 1, characterized in that: The electrode plates include a positive electrode plate and a negative electrode plate, and a surface of the positive electrode plate having the composite electrolyte layer is arranged opposite to a surface of the negative electrode plate having the composite electrolyte layer.

8. The semi-solid-state battery according to claim 1, characterized in that: The first polymer material in the polymer electrolyte includes at least one of polyethylene oxide, polymethyl methacrylate, polyacrylonitrile, polyvinylidene fluoride, polypropylene carbonate and polycyanoacrylate.

9. The semi-solid-state battery according to claim 1, characterized in that: The second polymer material in the polymer fiber includes at least one of polylactic acid, polycarbonate, polyethylene and polycaprolactone.

10. An energy storage device, characterized in that: The invention comprises a casing and at least one semi-solid-state battery according to any one of claims 1 to 9, wherein the semi-solid-state battery is accommodated in the casing.

11. An electrical device, characterized in that: It includes the energy storage device as described in claim 10, and the energy storage device supplies power to the electrical equipment.

Citation Information

Patent Citations

  • Composite solid electrolyte membrane with multilayer structure, preparation method thereof and solid-state battery

    CN110581314A

  • Method for preparing polyurethane-based composite electrolyte membrane and polyurethane-based composite electrolyte membrane

    CN113394446A

  • Fibrous composite solid electrolyte as well as preparation method and application thereof

    CN116093418A

  • Lithium polymer battery with a crosslinked electrolyte