Carbon paper for gas diffusion layer of fuel cell and preparation method of carbon paper

By pretreating carbon fibers with boric acid solution during the preparation of carbon paper and combining phenolic resin and graphitization technology, the problem of high resistivity of carbon paper in the fuel cell gas diffusion layer is solved, and carbon paper with low resistivity and high mechanical properties is achieved Preparation improves the polarization performance of fuel cells.

CN119092723APending Publication Date: 2024-12-06GUIZHOU MEILING POWER SUPPLY CO LTD +1

Patent Information

Application Number
CN202411100649.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The carbon paper in the existing fuel cell gas diffusion layer has a high resistivity, which leads to an increase in ohmic impedance and a decrease in polarization performance when the fuel cell is running.

Method used

The chopped carbon fiber is pretreated with boric acid solution, and carbon paper base paper is prepared by wet process, followed by phenolic resin impregnation, hot press curing and carbide graphitization, and boron elements are attached to improve the conductive and mechanical properties of carbon paper.

Benefits of technology

The prepared carbon paper has low resistivity, high strength and good mechanical properties, which helps to reduce the ohmic impedance of the fuel cell and improve polarization performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses carbon paper for a gas diffusion layer of a fuel cell and a preparation method thereof.The preparation method comprises the steps that carbon fibers serve as raw materials, a boric acid solution is adopted for pretreating the carbon fibers, then the carbon fibers are evenly dispersed, then a wet process is adopted for preparing carbon paper body paper, and boron-containing PVA glue is used for sizing before drying in a drying cylinder to prepare the carbon paper body paper; and then preparing the carbon paper by phenolic resin impregnation, hot-pressing curing, carbonization graphitization and other preparation methods. According to the preparation method, the boron element is attached to the carbon fibers in the carbon paper body paper making process in the early stage, boron and boride have the effect of enhancing the carbon fibers and have the effect of catalyzing graphitization in the follow-up process, and preparation of the low-resistivity and high-strength carbon paper is facilitated. The carbon paper for the fuel cell prepared by the preparation method has good controllability in surface properties, mechanical properties, intrinsic indexes and the like, and is beneficial to reducing ohmic impedance of the fuel cell and improving polarization performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells, and in particular relates to carbon paper for a fuel cell gas diffusion layer and a preparation method thereof. Background Art

[0002] Proton exchange membrane fuel cell (PEMFC) is a power generation device that converts chemical energy into electrical energy. It has many advantages such as high power density, high conversion efficiency, fast low-temperature start-up, no electrolyte loss, small size, long life and environmental friendliness. It is the new energy battery type with the highest research popularity and the fastest application progress in recent years. It is considered to be an ideal candidate power source for a series of fixed and mobile applications, such as automobiles, individual combat power supplies and distributed power stations.

[0003] The gas diffusion layer (GDL) is one of the core components of proton exchange membrane fuel cells. It has the following four main functions: first, it supports the proton exchange membrane and the catalyst layer; second, it serves as a channel for the anode and cathode reaction gases to diffuse from the flow field flow channel to the catalyst layer; third, it serves as an electron transmission channel to transmit electrons to the electrode plate; fourth, it discharges the product water from the catalyst layer to the flow field flow channel in a timely manner through capillary effect and concentration diffusion, thereby preventing the electrode from being flooded.

[0004] Carbon paper is made by mixing short carbon fibers and other fibers in a dispersed solution to make a slurry, and then mechanically stirring them to make them evenly interwoven, dehydrating and drying to obtain the carbon paper base. Carbon paper for gas diffusion layer is made through resin impregnation, hot pressing, carbonization and graphitization. The gas diffusion layer has a bulk resistance. At present, all types of gas diffusion layers on the market have a high resistivity. When the fuel cell is running, the ohmic impedance increases, resulting in reduced polarization performance.

[0005] The patent document with publication number CN110512459A discloses a high-performance carbon paper for fuel cells and its preparation method and application. The method comprises the following steps: (1) adding fiber raw materials to water and stirring and mixing uniformly to obtain a mixed slurry I; then sequentially adding surfactant, polyethylene oxide and polyvinyl alcohol solution to the mixed slurry I, stirring uniformly to obtain a mixed slurry II; then the mixed slurry II is made into a wet paper web, dried to obtain a carbon paper precursor; wherein the fiber raw materials include viscose fibers, cellulose nanofibrils and carbon fibers; (2) the carbon paper precursor is impregnated in an ethanol solution of a modified phenolic resin, dried, and a hydrophobic coating is applied on its surface, and then hot pressed and heat treated to obtain a carbon paper for a fuel cell. Boric acid is used in the preparation process of the patent document, but the carbon paper is prepared by mixing phenol, boric acid and acetic acid to obtain a boric acid-cardanol modified phenolic resin, and the preparation method and materials used are different from those of the present application. The lowest resistivity of the reference document is 7.1 mΩ·cm, which is higher than the lowest resistivity of 2.3 mΩ·cm in the embodiment of the present application.

[0006] The patent document with the publication number CN117721667A discloses a carbon paper for proton exchange membrane fuel cells, the raw materials of which include modified polyacrylonitrile-based carbon fibers and modified polyvinyl alcohol; the raw materials of the modified polyacrylonitrile-based carbon fibers include polyacrylonitrile-based carbon fibers, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid; the mass ratio of the polyacrylonitrile-based carbon fibers, phenolic resin and 4-(2-amino-2-formylethyl)benzoic acid is 95-105:5-10:3-7; the raw materials of the modified polyvinyl alcohol include polyvinyl alcohol and ethyl 4-amino-2-methylphenylacetate; the mass ratio of the polyvinyl alcohol to ethyl 4-amino-2-methylphenylacetate is 19-21:1-2. This patent improves the conductivity, mechanical strength and air permeability by linking after esterification reaction to form a large-size space channel and a large π-bond electron cloud, but it is different from the method of reducing the resistivity and improving the mechanical properties by boron element in the present invention. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a carbon paper for a fuel cell gas diffusion layer and a preparation method thereof.

[0008] The present invention is achieved through the following technical solutions.

[0009] The present invention provides a method for preparing carbon paper for a fuel cell gas diffusion layer, comprising the following steps:

[0010] S1: The short-cut carbon fiber is soaked in solution A, the carbon fiber is mixed with the water-soluble fiber, taken out and dispersed by a high-speed disperser, and then papermaking is performed, and an adhesive is applied, and the carbon paper base is made after drying;

[0011] S2: using a dip coating machine to dip the carbon paper base paper into the coating solution B, taking it out and drying it to obtain a preformed paper with resin attached;

[0012] S3: placing the preformed paper with the resin attached in a mold and performing a hot pressing curing process to obtain a hot pressing formed paper;

[0013] S4: subjecting the hot-pressed molded paper to carbonization and graphitization to obtain the carbon paper for the gas diffusion layer.

[0014] Preferably, solution A in step S1 is a boric acid aqueous solution, and the chopped carbon fibers are immersed in a boric acid aqueous solution with a weight percentage concentration of 2-3% for 10-15 hours. After being taken out, the chopped carbon fibers and 70°C water-soluble polyvinyl alcohol fibers are mixed in a ratio of 85%:15%, and paper is made using an inclined wire papermaking machine, and the adhesive is applied by a cylinder sizing device, and the carbon paper base is made after being dried in a drying cylinder.

[0015] Preferably, in step S1, in parts by weight, the adhesive preparation step includes: first dissolving boric acid in hot water at 40 to 60° C. to prepare a boric acid solution with a weight percentage concentration of 1 to 5%, taking 2 to 6 parts of the boric acid solution and adding them to 100 parts of a polyvinyl alcohol aqueous solution with a weight percentage concentration of 2 to 7%, and stirring evenly to prepare an adhesive.

[0016] Preferably, in step S1, the chopped carbon fiber is T700, a polyacrylonitrile-based carbon fiber with a fiber length of 4 to 6 mm and a fiber diameter of 7 to 12 μm, and the weight of the carbon paper base paper is 15 to 35 g / m 2 .

[0017] Preferably, in step S2, solution B is a phenolic resin solution, and the preparation step of the phenolic resin solution includes: mixing 300-400 parts of phenolic resin with 1500-1800 parts of ethanol aqueous solution with a concentration of 30-70% by weight, and preparing the solution after sufficient stirring and dissolution.

[0018] Preferably, in step S2, the speed of the dip coating machine is 2-3 m / min; the oven drying temperature is 85-95° C., and the drying time is 10-20 min; and the resin content in the thermoforming paper is 50-54%.

[0019] Preferably, in step S3, the preformed paper with resin attached is stacked in two layers in a customized mold, and the total weight of the stack is 50-70 g / m 2 , perform hot pressing curing treatment on a hot press machine, perform hot pressing curing treatment for 1 to 3 minutes under the conditions of pressure 1 to 6 MPa and temperature 150 to 200°C, and cool down with the instrument while maintaining the pressure after hot pressing.

[0020] Preferably, in step S4, carbonization and graphitization are performed under vacuum or argon atmosphere protection, the carbonization temperature is 1000-1100° C., the graphitization temperature is 2200-2800° C., and the carbonization and graphitization time is 45-52 hours.

[0021] A carbon paper prepared by the above preparation method.

[0022] Preferably, the gas permeability of the carbon paper is greater than 2000 ml·mm / (cm 2 ·h·mmHg), graphitization degree>65%, porosity≥80%, vertical resistivity≤400mΩ·cm, horizontal resistivity≤2.3mΩ·cm, tensile strength≥25MPa, bending modulus≥10MPa, thickness180~220μm, volume density0.35~0.45g / cm 3 .

[0023] The beneficial effects of the present invention are:

[0024] The present invention uses carbon fiber as raw material, uses boric acid solution to pretreat the carbon fiber, then uniformly disperses the carbon fiber and uses a wet process to prepare carbon paper base paper, and uses boron-containing PVA glue to apply before drying to prepare carbon paper base paper; then it is prepared into carbon paper through phenolic resin impregnation, hot pressing curing, carbonization and graphitization. The preparation method attaches boron elements to carbon fiber in the early carbon paper base papermaking process, and boron and boride have the effect of enhancing carbon fiber and catalyzing graphitization in subsequent processes, which is conducive to the preparation of low resistivity and high strength carbon paper. The surface properties, mechanical properties, intrinsic indicators, etc. of the carbon paper for fuel cells prepared by the preparation method have good controllability, and are helpful to reduce the ohmic impedance of fuel cells and improve polarization performance. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.

[0026] Embodiment 1:

[0027] A method for preparing carbon paper for a fuel cell gas diffusion layer comprises the following steps:

[0028] S1: The short-cut carbon fiber is soaked in solution A, the carbon fiber and the water-soluble fiber are mixed in proportion, taken out and dispersed by a high-speed disperser, and then papermaking is performed, and an adhesive is applied, and the carbon paper base is made after drying;

[0029] S2: using a dip coating machine to dip the carbon paper base paper into the coating solution B, taking it out and drying it to obtain a preformed paper with resin attached;

[0030] S3: placing the preformed paper with the resin attached in a mold and performing a hot pressing curing process to obtain a hot pressing formed paper;

[0031] S4: subjecting the hot-pressed molded paper to carbonization and graphitization to obtain the carbon paper for the gas diffusion layer.

[0032] In the step S1, solution A is a boric acid aqueous solution. The chopped carbon fibers are immersed in a boric acid aqueous solution with a weight percentage concentration of 2-3% for 10 hours. After being taken out, the chopped carbon fibers and 70°C water-soluble polyvinyl alcohol fibers are mixed in a ratio of 85%:15%, and paper is made using an inclined wire papermaking machine. The adhesive is applied by a cylinder sizing device, and the carbon paper base is made after being dried in a drying cylinder.

[0033] In step S1, in parts by weight, the adhesive preparation step includes: dissolving boric acid in hot water at 40°C to prepare a boric acid solution with a weight percentage concentration of 1%, adding 2 parts of the boric acid solution to 100 parts of a polyvinyl alcohol aqueous solution with a weight percentage concentration of 2%, and stirring for 30 minutes to prepare an adhesive.

[0034] In step S1, the chopped carbon fiber is T700, a polyacrylonitrile-based carbon fiber with a fiber length of 4 mm and a fiber diameter of 7 μm, and the weight of the carbon paper base paper is 15 g / m 2 , and cut the carbon paper into 10×10cm 2 .

[0035] In step S2, solution B is a phenolic resin solution, and the preparation step of the phenolic resin solution includes: mixing 300 parts of phenolic resin with 1500 parts of ethanol aqueous solution with a concentration of 30% by weight, and stirring for 30 minutes to dissolve the mixture.

[0036] In the step S2, the speed of the dip coating machine is 2 m / min; the oven drying temperature is 85° C. and the drying time is 10 min; and the resin content in the hot-pressed molding paper is 50%.

[0037] In step S3, the preformed paper with resin attached is stacked in two layers in a customized mold, and the total weight of the stack is 50g / m 2 , hot pressing curing treatment was carried out on a hot press machine at a pressure of 1 MPa and a temperature of 150°C for 1 minute. After hot pressing, the pressure was maintained while the instrument cooled.

[0038] In the step S4, the carbonization and graphitization are carried out under vacuum or argon atmosphere protection, the carbonization temperature is 1000° C., the graphitization temperature is 2200° C., and the carbonization and graphitization time is 45 hours.

[0039] Embodiment 2:

[0040] A method for preparing carbon paper for a fuel cell gas diffusion layer comprises the following steps:

[0041] S1: The short-cut carbon fiber is soaked in solution A, the carbon fiber and the water-soluble fiber are mixed in proportion, taken out and dispersed by a high-speed disperser, and then papermaking is performed, and an adhesive is applied, and the carbon paper base is made after drying;

[0042] S2: using a dip coating machine to dip the carbon paper base paper into the coating solution B, taking it out and drying it to obtain a preformed paper with resin attached;

[0043] S3: placing the preformed paper with the resin attached in a mold and performing a hot pressing curing process to obtain a hot pressing formed paper;

[0044] S4: subjecting the hot-pressed molded paper to carbonization and graphitization to obtain the carbon paper for the gas diffusion layer.

[0045] In the step S1, solution A is a boric acid aqueous solution. The chopped carbon fibers are immersed in a boric acid aqueous solution with a weight percentage concentration of 3% for 15 hours. After being taken out, the chopped carbon fibers and 70°C water-soluble polyvinyl alcohol fibers are mixed in a ratio of 85%:15%, and paper is made using an inclined wire papermaking machine. The adhesive is applied through a cylinder sizing device, and the carbon paper base is made after being dried in a drying cylinder.

[0046] In step S1, in parts by weight, the adhesive preparation step includes: dissolving boric acid in hot water at 60°C to prepare a boric acid solution with a weight percentage concentration of 5%, adding 6 parts of the boric acid solution to 100 parts of a polyvinyl alcohol aqueous solution with a weight percentage concentration of 7%, and stirring for 30 minutes to prepare an adhesive.

[0047] In step S1, the chopped carbon fiber is T700, a polyacrylonitrile-based carbon fiber with a fiber length of 6 mm and a fiber diameter of 12 μm, and the weight of the carbon paper base paper is 35 g / m 2 , and cut the carbon paper into 10×10cm 2 .

[0048] In step S2, solution B is a phenolic resin solution, and the preparation step of the phenolic resin solution includes: mixing 400 parts of phenolic resin with 1800 parts of 70% ethanol aqueous solution by weight, and stirring for 30 minutes to dissolve the mixture.

[0049] In the step S2, the speed of the dip coating machine is 3 m / min; the oven drying temperature is 95° C. and the drying time is 20 min; and the resin content in the hot-pressed molding paper is 54%.

[0050] In step S3, the preformed paper with resin attached is stacked in two layers in a customized mold, and the total weight of the stack is 70g / m 2 , hot pressing curing treatment was carried out on a hot press machine at a pressure of 6 MPa and a temperature of 200°C for 3 minutes. After hot pressing, the pressure was maintained and the instrument was cooled.

[0051] In the step S4, carbonization and graphitization are performed under vacuum or argon atmosphere protection, the carbonization temperature is 1100° C., the graphitization temperature is 2800° C., and the carbonization and graphitization time is 52 hours.

[0052] Embodiment 3:

[0053] A method for preparing carbon paper for a fuel cell gas diffusion layer comprises the following steps:

[0054] S1: The short-cut carbon fiber is soaked in solution A, the carbon fiber and the water-soluble fiber are mixed in proportion, taken out and dispersed by a high-speed disperser, and then papermaking is performed, and an adhesive is applied, and the carbon paper base is made after drying;

[0055] S2: using a dip coating machine to dip the carbon paper base paper into the coating solution B, taking it out and drying it to obtain a preformed paper with resin attached;

[0056] S3: placing the preformed paper with the resin attached in a mold and performing a hot pressing curing process to obtain a hot pressing formed paper;

[0057] S4: subjecting the hot-pressed molded paper to carbonization and graphitization to obtain the carbon paper for the gas diffusion layer.

[0058] In step S1, solution A is a boric acid aqueous solution. The chopped carbon fibers are immersed in a boric acid aqueous solution with a weight percentage concentration of 2.5% for 12 hours. After being taken out, the chopped carbon fibers and 70°C water-soluble polyvinyl alcohol fibers are mixed in a ratio of 85%:15%, and paper is made using an inclined wire papermaking machine. The adhesive is applied by a cylinder sizing device, and the carbon paper base is made after being dried in a drying cylinder.

[0059] In step S1, in parts by weight, the adhesive preparation step includes: dissolving boric acid in hot water at 50°C to prepare a boric acid solution with a weight percentage concentration of 3%, adding 3.5 parts of the boric acid solution to 100 parts of a polyvinyl alcohol aqueous solution with a weight percentage concentration of 4%, and stirring for 30 minutes to prepare an adhesive.

[0060] In step S1, the chopped carbon fiber is T700, a polyacrylonitrile-based carbon fiber with a fiber length of 5 mm and a fiber diameter of 10 μm, and the weight of the carbon paper base paper is 20 g / m 2 , and cut the carbon paper into 10×10cm 2 .

[0061] In step S2, solution B is a phenolic resin solution, and the preparation step of the phenolic resin solution includes: mixing 350 parts of phenolic resin with 1700 parts of 50% ethanol aqueous solution by weight, and stirring for 30 minutes to dissolve the mixture.

[0062] In the step S2, the speed of the dip coating machine is 2.5 m / min; the oven drying temperature is 90° C. and the drying time is 15 min; and the resin content in the hot-pressed molding paper is 52%.

[0063] In step S3, the preformed paper with resin attached is stacked in two layers in a customized mold, and the total weight of the stack is 60g / m 2, hot pressing curing treatment was carried out on a hot press machine at a pressure of 3MPa and a temperature of 180°C for 1.5min. After hot pressing, the pressure was maintained while the instrument cooled.

[0064] In the step S4, carbonization and graphitization are performed under vacuum or argon atmosphere protection, the carbonization temperature is 1066° C., the graphitization temperature is 2500° C., and the carbonization and graphitization time is 48 hours.

[0065] Comparative Example 1:

[0066] The preparation method is basically the same as that of Example 3, except that boric acid is not added during the immersion treatment in solution A and the preparation of the adhesive.

[0067] The performance parameters of the carbon papers prepared in Examples 1 to 3 and Comparative Example 1 are shown in the following table:

[0068] Carbon paper performance parameter table

[0069]

[0070]

[0071] The tensile strength of the carbon paper prepared in Example 3 and Comparative Example 1 was tested. The tensile strength of the carbon paper prepared in Example 3 was 2.8 kN / m, and the tensile strength of the carbon paper prepared in Comparative Example 1 was 2.2 kN / m. The vertical resistivity and horizontal resistivity of Comparative Example 1 were also higher than those of the carbon paper prepared in Examples 1 to 3, and the tensile strength was lower than that of the carbon paper prepared in Examples 1 to 3. It can be seen that the addition of boron has a positive effect on the conductivity and mechanical properties of carbon paper.

Claims

1. A method for preparing carbon paper for a fuel cell gas diffusion layer, characterized in that: The following steps are involved: S1: The short-cut carbon fiber is soaked in solution A, the carbon fiber is mixed with the water-soluble fiber, taken out and dispersed by a high-speed disperser, and then papermaking is performed, and an adhesive is applied, and the carbon paper base is made after drying; S2: using a dip coating machine to dip the carbon paper base paper into the coating solution B, taking it out and drying it to obtain a preformed paper; S3: placing the preformed paper in a mold and performing a hot pressing curing process to obtain a hot pressing formed paper; S4: subjecting the hot-pressed molded paper to carbonization and graphitization to obtain the carbon paper for the gas diffusion layer.

2. The method for preparing a carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In the step S1, solution A is a boric acid aqueous solution. The chopped carbon fibers are immersed in a boric acid aqueous solution with a weight percentage concentration of 2 to 3% for 10 to 15 hours. After being taken out, the chopped carbon fibers and 70°C water-soluble polyvinyl alcohol fibers are mixed in a ratio of 85%:15%, and paper is made using an inclined mesh papermaking machine. The adhesive is applied by a cylinder sizing device, and the carbon paper base is made after being dried in a drying cylinder.

3. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In step S1, in units of parts by weight, the adhesive preparation step includes: first dissolving boric acid in hot water at 40 to 60° C. to prepare a boric acid solution with a weight percentage concentration of 1 to 5%, taking 2 to 6 parts of the boric acid solution and adding it to 100 parts of a polyvinyl alcohol aqueous solution with a weight percentage concentration of 2 to 7%, and stirring evenly to prepare an adhesive.

4. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In step S1, the chopped carbon fiber is T700, a polyacrylonitrile-based carbon fiber with a fiber length of 4 to 6 mm and a fiber diameter of 7 to 12 μm, and the weight of the carbon paper base paper is 15 to 35 g / m 2 .

5. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In step S2, solution B is a phenolic resin solution, and the preparation step of the phenolic resin solution includes: mixing 300-400 parts of phenolic resin with 1500-1800 parts of ethanol aqueous solution with a concentration of 30-70% by weight, and preparing the mixture after sufficient stirring and dissolution.

6. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In the step S2, the speed of the dip coating machine is 2-3 m / min; the oven drying temperature is 85-95° C., and the drying time is 10-20 min; and the resin content in the hot-pressed molding paper is 50-54%.

7. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In step S3, the preformed paper with resin attached is stacked in two layers in a customized mold, and the total weight of the stack is 50-70 g / m 2 , perform hot pressing curing treatment on a hot press machine, perform hot pressing curing treatment for 1 to 3 minutes under the conditions of pressure 1 to 6 MPa and temperature 150 to 200°C, and cool down with the instrument while maintaining the pressure after hot pressing.

8. The method for preparing carbon paper for a fuel cell gas diffusion layer according to claim 1, characterized in that: In the step S4, the carbonization and graphitization are carried out under vacuum or argon atmosphere protection, the carbonization temperature is 1000-1100° C., the graphitization temperature is 2200-2800° C., and the carbonization and graphitization time is 45-52 hours.

9. A carbon paper prepared by the preparation method according to any one of claims 1 to 8.

10. A carbon paper as claimed in claim 9, characterized in that: The gas permeability of the carbon paper is > 2000 ml·mm / (cm 2 ·h·mmHg), graphitization degree>65%, porosity≥80%, vertical resistivity≤400mΩ·cm, horizontal resistivity≤2.3mΩ·cm, tensile strength≥25MPa, bending modulus≥10MPa, thickness180~220μm, volume density0.35~0.45g / cm 3 .

Citation Information

Patent Citations

  • High-performance carbon paper for fuel cell and preparation method and application thereof

    CN110512459A

  • Carbon paper for proton exchange membrane fuel cell and preparation method thereof

    CN117721667A

Cited By

  • Method for preparing carbon paper by blending PVA fiber and carbon fiber into web

    CN120311521A