Special material for bipolar plate of liquid flow energy storage battery and preparation method of special material
By depositing nanosilicon on the graphite surface and mixing it with other materials, pressurized refining and preparing special materials for bipolar plates for liquid flow energy storage batteries, the problem of difficult to take into account both the conductivity and mechanical strength of carbon plastic composite bipolar plates is achieved. Synergistic efficiency of high conductivity and high mechanical strength.
Patent Information
- Application Number
- CN202411165254.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
AI Technical Summary
While improving mechanical strength, the existing carbon plastic composite bipolar plates are difficult to take into account both the conductive properties, and the graphite brittleness and the excessive resin content lead to the problem of reduced conductivity.
Nanosilicon is deposited on the surface of the scale graphite and mixed with silane coupling agent, polysulfone, cyanate resin, carbon material and plasticizer. After pressurization, the special material for liquid flow energy storage battery bipolar plate is prepared. , improve conductive properties and mechanical strength.
The mechanical strength of graphite is effectively improved, and the conductive properties are maintained by combining the deposited nano-silicon with polysulfone and cyanate resin, achieving synergistic efficiency of high conductivity and high mechanical strength.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy materials and relates to a special material for bipolar plates of a liquid flow energy storage battery and a preparation method thereof. Background Art
[0002] Vanadium battery, whose full name is Vanadium Redox Flow Battery (VRB), is a redox battery in which the active material is in a circulating liquid state.
[0003] As a multifunctional key component in the all-vanadium liquid flow battery system, the bipolar plate can collect and conduct the current generated during the battery charging and discharging process, provide effective mechanical support for the membrane and electrode, connect multiple single cells and prevent the mixing of positive and negative electrode electrolytes and direct contact of the electrodes, which has a significant impact on the energy efficiency of the battery stack. Therefore, ideal bipolar plate materials usually need to have good conductivity, electrochemical stability, corrosion resistance and certain mechanical strength, but it is often difficult to take all these characteristics into account. Bipolar plate materials are mainly divided into three types according to the composition of the materials: metal bipolar plates, graphite bipolar plates and carbon-plastic composite bipolar plates. Graphite materials have good conductivity, lower density and better corrosion resistance than metal materials, and are currently the most widely used materials in liquid flow batteries. However, the processing performance of graphite bipolar plates is poor, requiring more stringent processing technology and higher costs, so carbon-plastic composite bipolar plates have attracted the attention of the battery industry. Carbon-plastic composite bipolar plates are generally composed of conductive fillers and polymer resins, where the conductive material is generally various graphites, and the polymer resin can be selected from thermosetting resins or thermoplastic resins. At present, the main contradiction faced by carbon-plastic composite bipolar plates is that the graphite itself is very brittle and has insufficient mechanical strength, so resin needs to be added for reinforcement. However, excessive resin content will lead to a decrease in the conductivity of the bipolar plate. Therefore, how to develop a carbon composite bipolar plate with high conductivity and high mechanical strength has become a hot topic in current research. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a special material for bipolar plates of liquid flow energy storage batteries and a preparation method thereof.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] The first aspect of the present invention provides a method for preparing a special material for bipolar plates of a liquid flow energy storage battery, comprising the following steps:
[0007] (1) depositing nano-silicon on the surface of flake graphite to obtain flake graphite with deposited nano-silicon;
[0008] (2) mixing the flake graphite with deposited nano-silicon, a silane coupling agent, polysulfone, and a cyanate resin, stirring for the first time, and then adding the carbon material and the plasticizer, stirring for the second time, to obtain a coating mixture;
[0009] (3) The coated mixture is pressurized, kneaded, and solidified to obtain a special material for bipolar plates of liquid flow energy storage batteries.
[0010] Preferably, in step (1), the method for depositing nano-silicon is:
[0011] The flake graphite is placed in a chemical vapor deposition furnace, evacuated to a vacuum state, filled with inert protective gas at a rate of 10-100L / h, heated to 400-1000°C at a rate of 1-15°C / min, and after heating to the set temperature, silicon source gas is filled at a rate of 10-100L / h. The program insulation time is 0.5-10h, the silicon source gas pipeline is closed, and the automatic cooling program is entered. After cooling to room temperature, it is taken out to obtain flake graphite with deposited nano-silicon.
[0012] Preferably, the D50 particle size of the flake graphite is 1-500 μm, the silicon source gas is one or more of monosilane, dichlorodimethylsilane, dichlorosilane, trichlorosilane, and silicon tetrachloride, and the inert protective gas is one or more of nitrogen, helium, xenon, radon, neon, and argon.
[0013] Preferably, in step (2), the weight ratio of the flake graphite for depositing nano-silicon, the silane coupling agent, the polysulfone, the cyanate resin, the carbon material and the plasticizer is: (45-70): (0.5-5): (15-20): (15-20): (0.5-5): (0.5-5), and the plasticizer is a polyolefin elastomer.
[0014] Preferably, the silane coupling agent includes one or more of 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane and 3-(2,3-epoxypropyloxy)propyltrimethoxysilane; and the carbon material is composed of carbon nanotubes, superconducting carbon black and graphene in a weight ratio of 1:1:1.
[0015] Preferably, the first stirring condition is: stirring at 200-550 r / min for 2-5 min; the second stirring condition is: stirring at 600-950 r / min for 5-10 min.
[0016] Preferably, in step (3), the conditions for pressure mixing are: 5-12 MPa, 12-15 min;
[0017] The granulation method is as follows: the material obtained by internal mixing is extruded into a 48:1 twin-screw extruder, the temperature of the first zone of the twin-screw extruder is 140-150°C, the temperature of the second zone is 150-160°C, the temperature of the third zone is 160-170°C, the temperature of the fourth zone, the fifth zone, the sixth zone, the seventh zone, and the eighth zone are all set to 180-190°C, the temperature of the ninth zone is 160-170°C, the temperature of the tenth zone is 150-160°C, the temperature of the eleventh zone is 140-150°C, the temperature of the twelfth zone is 150-160°C, and the temperature of the die head is 210-220°C.
[0018] The second aspect of the present invention provides a special material for bipolar plates of liquid flow energy storage batteries prepared by the above preparation method.
[0019] A third aspect of the present invention provides a bipolar plate for a liquid flow energy storage battery, which is made of the above-mentioned special material for bipolar plates of liquid flow energy storage batteries.
[0020] Beneficial effects of the present invention:
[0021] (1) The present invention deposits nano-silicon materials on the surface of graphite and prepares special materials for bipolar plates of liquid flow energy storage batteries, which can effectively make up for the disadvantage of large brittleness of graphite itself. In addition, the graphite after deposition of nano-silicon materials is combined with polysulfone and cyanate resin to maintain the conductive properties of the materials, thus playing a synergistic effect.
[0022] (2) The present invention adopts a two-step method, firstly mixing and stirring graphite and a coupling agent, so that the coupling agent is fully and evenly coated on the surface of the powder, which plays a better coupling role and improves the physical and mechanical properties of the product. DETAILED DESCRIPTION
[0023] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0024] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.
[0025] In the following examples and comparative examples, the flake graphite used was purchased from Qingdao Mingrun Chenyue Graphite Co., Ltd.;
[0026] 3-Aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and 3-(2,3-epoxypropyloxy)propyltrimethoxysilane were purchased from Shandong Sike New Materials Co., Ltd.;
[0027] Polysulfone was purchased from Solvay, USA, with the brand name Udel P3500;
[0028] The cyanate resin is specifically bisphenol E cyanate resin, CAS number is 47073-92-7;
[0029] The polyolefin elastomer is specifically Vistamaxx 6102 propylene-based elastomer, purchased from ExxonMobil Corporation;
[0030] Carbon nanotubes were industrial-grade multi-walled carbon nanotubes purchased from Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, Chengdu;
[0031] The superconducting carbon black model is AC-80, purchased from Shanghai Yutong Chemical Technology Co., Ltd.;
[0032] Graphene was purchased from Aladdin Reagents.
[0033] Example 1: Preparation of special materials for bipolar plates of liquid flow energy storage batteries.
[0034] (1) The flake graphite is placed in a chemical vapor deposition furnace, evacuated to a vacuum state, and nitrogen is introduced at a rate of 50 L / h. The temperature is raised to 600°C at a rate of 7°C / min. After the temperature reaches the set temperature, monosilane is introduced at a rate of 50 L / h. The program insulation time is 5 hours, and the silicon source gas pipeline is closed. The automatic cooling program is entered, and the temperature is taken out after it drops to room temperature to obtain flake graphite with deposited nanosilicon.
[0035] (2) mixing the nano-silicon deposited flake graphite, 3-aminopropyltriethoxysilane, polysulfone, and cyanate resin, stirring at 300 r / min for 3 min, then adding the carbon material and the polyolefin elastomer, stirring at 700 r / min for 8 min, to obtain a coating mixture;
[0036] The weight ratio of nano-silicon deposited flake graphite, 3-aminopropyltriethoxysilane, polysulfone, cyanate resin, carbon material and polyolefin elastomer is 50:2:18:18:2:2, and the carbon material is composed of carbon nanotubes, superconducting carbon black and graphene in a weight ratio of 1:1:1;
[0037] (3) The coating mixture was placed in an internal mixer and mixed at 1.2 MPa for 13 min. The mixed material was extruded into a 48:1 twin-screw extruder and granulated to obtain a bipolar plate material.
[0038] The twin-screw extruder was set as follows: the temperature of the first zone was 140°C, the second zone was 150°C, the third zone was 160°C, the temperatures of the fourth zone, the fifth zone, the sixth zone, the seventh zone, and the eighth zone were all set to 180°C, the ninth zone was 160°C, the tenth zone was 150°C, the eleventh zone was 140°C, the twelfth zone was 150°C, and the head temperature was 210°C.
[0039] Example 2: Preparation of special materials for bipolar plates of liquid flow energy storage batteries.
[0040] (1) The flake graphite is placed in a chemical vapor deposition furnace, evacuated to a vacuum state, filled with helium at a rate of 10 L / h, and heated to 400°C at a rate of 1°C / min. After heating to the set temperature, silicon tetrachloride is filled at a rate of 10 L / h, and the program insulation time is 0.5 h. The silicon source gas pipeline is closed, and the automatic cooling program is entered. After cooling to room temperature, it is taken out to obtain flake graphite with deposited nano-silicon.
[0041] (2) mixing the nano-silicon deposited flake graphite, 3-mercaptopropyltrimethoxysilane, a silane coupling agent, polysulfone, and a cyanate resin, stirring at 200 r / min for 2 min, then adding the carbon material and the polyolefin elastomer, stirring at 600 r / min for 5 min, to obtain a coating mixture;
[0042] The weight ratio of nano-silicon deposited flake graphite, 3-mercaptopropyltrimethoxysilane, polysulfone, cyanate resin, carbon material and polyolefin elastomer is 45:0.5:15:15:0.5:0.5, and the carbon material is composed of carbon nanotubes, superconducting carbon black and graphene in a weight ratio of 1:1:1;
[0043] (3) The coating mixture was placed in an internal mixer and mixed at 0.8 MPa for 12 min. The mixed material was extruded into a 48:1 twin-screw extruder and granulated to obtain a bipolar plate material.
[0044] The twin-screw extruder was set as follows: the temperature of the first zone was 150°C, the second zone was 160°C, the third zone was 170°C, the temperatures of the fourth zone, the fifth zone, the sixth zone, the seventh zone, and the eighth zone were all set to 190°C, the ninth zone was 170°C, the tenth zone was 160°C, the eleventh zone was 150°C, the twelfth zone was 160°C, and the head temperature was 220°C.
[0045] Example 3: Preparation of special materials for bipolar plates of liquid flow energy storage batteries.
[0046] (1) Placing flake graphite in a chemical vapor deposition furnace, evacuating to a vacuum state, charging neon gas at a rate of 100 L / h, heating to 1000°C at a rate of 1-15°C / min, and after heating to the set temperature, charging dichlorosilane at a rate of 100 L / h, and keeping the temperature for 10 hours. Closing the silicon source gas pipeline, entering the automatic cooling program, and taking it out after cooling to room temperature, flake graphite with deposited nano-silicon is obtained.
[0047] (2) mixing the nano-silicon deposited flake graphite, 3-(methacryloyloxy)propyltrimethoxysilane, polysulfone, and cyanate resin, stirring at 550 r / min for 5 min, then adding the carbon material and the polyolefin elastomer, stirring at 950 r / min for 10 min, to obtain a coating mixture;
[0048] The weight ratio of nano-silicon deposited flake graphite, 3-(methacryloyloxy)propyltrimethoxysilane, polysulfone, cyanate resin, carbon material and polyolefin elastomer is 70:5:20:20:5:5, and the carbon material is composed of carbon nanotubes, superconducting carbon black and graphene in a weight ratio of 1:1:1;
[0049] (3) The coating mixture was placed in an internal mixer and mixed at 1.2 MPa for 15 min. The mixed material was extruded into a 48:1 twin-screw extruder and granulated to obtain a bipolar plate material.
[0050] The twin-screw extruder was set as follows: the temperature of the first zone was 145°C, the second zone was 155°C, the third zone was 165°C, the temperatures of the fourth zone, the fifth zone, the sixth zone, the seventh zone, and the eighth zone were all set to 185°C, the ninth zone was 165°C, the tenth zone was 155°C, the eleventh zone was 145°C, the twelfth zone was 155°C, and the head temperature was 215°C.
[0051] Comparative Example 1: Preparation of special materials for bipolar plates of liquid flow energy storage batteries.
[0052] The bipolar plate of the liquid flow energy storage battery was prepared according to the method of Example 1, except that: polysulfone was not used in this comparative example, and nano-silicon was not deposited on the flake graphite, as follows:
[0053] (1) flake graphite, monoalkoxy titanate, and cyanate resin were mixed, stirred at 300 r / min for 3 min, and then carbon material and polyolefin elastomer were added, and stirred at 700 r / min for 8 min to obtain a coating mixture;
[0054] The weight ratio of the flake graphite for depositing nano-silicon, the coupling agent, the cyanate resin, the carbon material and the polyolefin elastomer is 50:2:18:18:2:2, and the carbon material is composed of carbon nanotubes, superconducting carbon black and graphene in a weight ratio of 1:1:1;
[0055] (2) The coating mixture was placed in an internal mixer and mixed at 1.0 MPa for 13 min. The mixed material was extruded into a 48:1 twin-screw extruder and granulated to obtain a bipolar plate special material.
[0056] The twin-screw extruder was set as follows: the temperature of the first zone was 140°C, the second zone was 150°C, the third zone was 160°C, the temperatures of the fourth zone, the fifth zone, the sixth zone, the seventh zone, and the eighth zone were all set to 180°C, the ninth zone was 160°C, the tenth zone was 150°C, the eleventh zone was 140°C, the twelfth zone was 150°C, and the head temperature was 210°C.
[0057] Comparative Example 2: Preparation of special materials for bipolar plates of liquid flow energy storage batteries.
[0058] The special material for bipolar plates of liquid flow energy storage batteries was prepared according to the method of Example 1, except that polysulfone was not used in this comparative example.
[0059] Comparative Example 3: Preparation of special materials for bipolar plates of liquid flow energy storage batteries.
[0060] The special material for bipolar plates of liquid flow energy storage batteries was prepared according to the method of Example 1, except that: the flake graphite of this comparative example did not deposit nano-silicon.
[0061] Test Example 1: Mechanical Properties Test
[0062] (1) Test method:
[0063] The bipolar plate materials prepared in Example 1 and Comparative Examples 1-3 were placed in a flat vulcanizer and hot pressed for 20 minutes at 200° C. and 10 MPa to produce bipolar plates, which were then tested for bending strength in accordance with GB / T 20042.6-2011.
[0064] The test method is as follows:
[0065] Several 10×1cm specimens were cut as test specimens, the specimen detection gauge length was limited to 60mm, a three-point bending test was performed at a running rate of 2mm / min, and the arithmetic mean of 5 valid samples was selected as the final test result.
[0066] (2) Test results:
[0067] Table 1: Bending strength of bipolar plates
[0068] Flexural strength(MPa) Example 1 31 Comparative Example 1 13 Comparative Example 2 21 Comparative Example 3 16
[0069] It can be seen from the data in the above table that the bipolar plate provided by the present invention has a high bending strength, indicating that it has a high mechanical strength, and the graphite after the deposition of nano-silicon material is combined with polysulfone and cyanate resin to play a synergistic role.
[0070] Test Example 2: Conductive Performance Test
[0071] (1) Test method:
[0072] On the basis of Experimental Example 1, the conductivity and contact resistance of the bipolar plates prepared with the special materials of Example 1 and Comparative Examples 1-3 were measured.
[0073] The test method of conductivity is: use a dual-electric four-probe measuring instrument to measure the volume resistivity of each sample. The instrument test range is 1μA~100mA, and the conductivity value is the reciprocal of the volume resistivity. Each sample is tested for five data values in different areas, and the average value of the above five data is taken as the test result of a single sample. The final result is the average value of three groups of parallel samples.
[0074] The contact resistance is determined by referring to the method described in the master's thesis "Preparation and Performance Study of Graphite_Polyimide-Polyetheretherketone Resin Composite Bipolar Plates for PEMFC".
[0075] (2) Test results:
[0076] Table 2: Bipolar plate conductivity
[0077] Conductivity (S / cm) <![CDATA[Contact resistance (mΩ·cm 2 )]]> Example 1 152 18.8 Comparative Example 1 124 26.4 Comparative Example 2 133 21.6 Comparative Example 3 109 29.4
[0078] It can be seen from the above table that the bipolar plate of Example 1 has the highest conductivity and the lowest contact resistance, which means that the bipolar plate has good electrical conductivity and high mechanical strength.
[0079] The above description is only a preferred embodiment of the present invention and is not intended to limit the implementation and application of the present invention. Any modifications, equivalent substitutions, etc. made in the implementation and application within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a special material for bipolar plates of liquid flow energy storage batteries, It is characterized in that The following steps are involved: (1) depositing nano-silicon on the surface of flake graphite to obtain flake graphite with deposited nano-silicon; (2) mixing the flake graphite with deposited nano-silicon, a silane coupling agent, polysulfone, and a cyanate resin, stirring for the first time, and then adding the carbon material and the plasticizer, stirring for the second time, to obtain a coating mixture; (3) The coated mixture is pressurized, kneaded, and granulated to obtain a special material for bipolar plates of liquid flow energy storage batteries.
2. The preparation method according to claim 1, It is characterized in that In step (1), the method for depositing nano-silicon is: The flake graphite is placed in a chemical vapor deposition furnace, evacuated to a vacuum state, filled with inert protective gas at a rate of 10-100L / h, heated to 400-1000°C at a rate of 1-15°C / min, and after heating to the set temperature, silicon source gas is filled at a rate of 10-100L / h. The program insulation time is 0.5-10h, the silicon source gas pipeline is closed, and the automatic cooling program is entered. After cooling to room temperature, it is taken out to obtain flake graphite with deposited nano-silicon.
3. The preparation method according to claim 1 or 2, It is characterized in that The D50 particle size of the flake graphite is 1-500 μm, the silicon source gas is one or more of monosilane, dichlorodimethylsilane, dichlorosilane, trichlorosilane, and silicon tetrachloride, and the inert protective gas is one or more of nitrogen, helium, xenon, radon, neon, and argon.
4. The preparation method according to claim 1, It is characterized in that In step (2), the weight ratio of the flake graphite for depositing nano-silicon, the silane coupling agent, the polysulfone, the cyanate resin, the carbon material and the plasticizer is (45-70): (0.5-5): (15-20): (15-20): (0.5-5): (0.5-5), and the plasticizer is a polyolefin elastomer.
5. The preparation method according to claim 4, It is characterized in that The silane coupling agent includes one or more of 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane and 3-(2,3-epoxypropyloxy)propyltrimethoxysilane; the carbon material is composed of carbon nanotubes, superconducting carbon black and graphene in a weight ratio of 1:1:
1.
6. The preparation method according to claim 1, It is characterized in that The conditions for the first stirring are: stirring at 200-550 r / min for 2-5 min; the conditions for the second stirring are: stirring at 600-950 r / min for 5-10 min.
7. The preparation method according to claim 1, It is characterized in that In step (3), the conditions of pressure mixing are: 5-12 MPa, 12-15 min; The granulation method is as follows: the material obtained by internal mixing is extruded into a 48:1 twin-screw extruder, the temperature of the first zone of the twin-screw extruder is 140-150°C, the temperature of the second zone is 150-160°C, the temperature of the third zone is 160-170°C, the temperature of the fourth zone, the fifth zone, the sixth zone, the seventh zone, and the eighth zone are all set to 180-190°C, the temperature of the ninth zone is 160-170°C, the temperature of the tenth zone is 150-160°C, the temperature of the eleventh zone is 140-150°C, the temperature of the twelfth zone is 150-160°C, and the temperature of the die head is 210-220°C.
8. Special material for bipolar plates of liquid flow energy storage batteries prepared by the preparation method described in claims 1-7.
9. A bipolar plate for a liquid flow energy storage battery, It is characterized in that Made of the special material for bipolar plates of liquid flow energy storage batteries as claimed in claim 8.