Fuel cell barrier layer slurry and preparation method thereof
By adding organic compound powder to the GDC slurry to form a slurry of organic phase, inorganic phase and additive phase, the problem that the GDC layer cannot be sintered and dense, and the performance of the fuel cell is improved.
Patent Information
- Application Number
- CN202411270120.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
In the existing fuel cell processes, the GDC layer cannot be sintered and densely sintered at a temperature below 1250°C, resulting in a degradation of fuel cell performance.
Add organic compound powders such as gadolinium oxalate, cerium oxalate, cerium oleate, and cerium citrate to the GDC slurry to form a slurry of organic phase, inorganic phase and additive phase, and pass through polymer polymers, organic solvents and organic aids The combination of agents improves sintering activity and forms a dense sintering structure.
Effectively reduce the thickness of the GDC layer, improve the performance of the fuel cell, realize the dense sintering of the GDC layer, and improve the overall performance of the fuel cell.
Smart Images

Figure CN119092766A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, in particular to a fuel cell barrier layer slurry and a preparation method thereof. Background Art
[0002] Solid oxide fuel cell sheets are composed of anode materials, electrolyte materials, barrier materials and cathode materials. The barrier material is composed of gadolinium oxide (chemical formula is Ga2O3) and cerium oxide (chemical formula is CeO2), referred to as GDC, and the barrier layer is also called the GDC layer.
[0003] When making a fuel cell, the cathode layer and electrolyte layer are first made by tape casting, and then the cathode layer and electrolyte layer are laminated by pressure and sintered at 1400°C to form a half-cell. Then, the GDC layer slurry is printed on the half-cell by screen printing and sintered at 1250°C or lower to fix the GDC layer on the half-cell.
[0004] Due to the process limitations of fuel cells, the sintering temperature of the GDC layer is required to be lower than 1250°C, as shown in the patent application with publication number CN117790853A. However, the melting points of gadolinium oxide and cerium oxide are 2330°C and 2397°C respectively, and they cannot be sintered to a dense state at this temperature. The only way to improve the reaction of the GDC layer and the half-cell during sintering is to increase the thickness, but this will reduce the performance of the fuel cell. Summary of the invention
[0005] In view of the problem that the GDC layer of the current fuel cell cannot be sintered densely under the existing process, which affects the performance of the fuel cell, the present invention provides a fuel cell barrier layer slurry and a preparation method thereof. By adding organic compound powders such as gadolinium oxalate, cerium oxalate, cerium oleate, cerium citrate, and gadolinium spray acid to the GDC slurry, the sintering activity of the GDC powder can be greatly improved, a dense sintered structure can be formed, the thickness of the GDC layer can be reduced, and the performance of the fuel cell can be improved, which can effectively solve the problem that the GDC layer cannot be sintered densely under the existing process.
[0006] To achieve the above object, the present invention provides the following technical solution: a fuel cell barrier layer slurry, comprising an organic phase, an inorganic phase and an additive phase, characterized in that: The weight percentages of the organic phase, inorganic phase and additive phase are as follows: Organic phase 15~50%, inorganic phase 50~75%, additive phase 0.5~10%; The organic phase includes a high molecular polymer, an organic solvent and an organic additive, and the weight percentage of the high molecular polymer, the organic solvent and the organic additive is as follows: High molecular polymer 5~30%, organic solvent 20~95%, organic additive 15% and below; The additive phase is an organic compound of gadolinium and cerium.
[0007] Preferably, the weight percentage composition of the organic phase, the inorganic phase and the additive phase is: 30-40% organic phase, 55-65% inorganic phase, and 5-10% additive phase.
[0008] Preferably, the weight percentage composition of the high molecular polymer, organic solvent and organic additive is: 5-15% of the high molecular polymer, 80-95% of the organic solvent and 5-10% of the organic additive.
[0009] The high molecular polymer includes but is not limited to polymethacrylate, polyvinyl alcohol, polyvinyl butyral, ethyl cellulose, nitrocellulose, polyvinyl pyrrolidone, alkyd resin, rosin resin. The organic solvent includes but is not limited to tributyl citrate, trioctyl acetyl citrate, pentanediol, terpineol, diethylene glycol monomethyl ether, diethylene glycol monomethyl ether acetate, butyl acetate. The organic additive includes but is not limited to lecithin, silane coupling agent, titanate coupling agent, polyamide wax, polyacrylic acid, octadecylamine, stearate, 1,4-butyrolactone, sodium lauryl sulfate, methylpentyl alcohol, oleyl amino oleate.
[0010] Preferably, the inorganic phase includes gadolinium oxide, cerium oxide or a mixture of the two in different proportions.
[0011] Preferably, the additive phase includes one or more of gadolinium oxalate, gadopentane acid, cerium oleate, cerium citrate, cerium oxalate, gadolinium stearate, cerium stearate, gadolinium laurate, etc. The present invention includes but is not limited to the above-mentioned gadolinium and cerium organic compounds, and organic compounds that can be decomposed to form nano-gadolinium oxide and cerium oxide during sintering have this effect.
[0012] The present invention also provides another technical solution: a method for preparing a fuel cell barrier layer slurry, the steps of which are as follows: 1) Preparation of organic phase: Heat and dissolve the polymer in an organic solvent according to the weight percentage composition, then add an organic additive, stir with a stirrer until the polymer is completely dissolved, and cool to obtain an organic phase.
[0013] 2) Preparation of slurry: The organic phase, the inorganic phase and the additive phase are mixed evenly using a stirrer according to the weight percentage composition, and then fully ground using a three-roll mill to a fineness of 3 μm or less to obtain a slurry.
[0014] Preferably, in step 1), the organic solvent is first added to the container in proportion, and then the high molecular polymer is added under stirring conditions, dissolved in the organic solvent at 80-85° C., and finally the organic auxiliary agent is added; the mixture is stirred until transparent and then cooled to obtain an organic phase.
[0015] Preferably, in step 2), the mass ratio of gadolinium oxide to cerium oxide in the inorganic phase is (1-3):(7-9).
[0016] Preferably, in step 2), the additive phase accounts for 5-8% of the total weight.
[0017] The principle of the present invention is: during sintering, the organic compound powder generates corresponding oxide nano powder by decomposition, and this powder can effectively promote sintering and improve sintering density due to its large specific surface area and low activation energy. If the addition method of organic compound is not adopted, and nano oxide powder is directly added, it will be difficult to ensure the dispersion and uniform distribution of nano powder, and slurry production will be difficult. Moreover, the prepared nano powder will produce agglomeration phenomenon after preparation due to its large specific surface area. Even if the agglomeration is opened, substances will be adsorbed on the powder surface to reduce the surface energy, and the sintering activity will be correspondingly reduced. The above-mentioned disadvantages can be avoided by adopting the method of adding organic compound to decompose nano powder during sintering.
[0018] Compared with the prior art, the present invention has the following advantages and effects: the present invention adds gadolinium and cerium organic compound additive phases, which can be decomposed into nanoparticles uniformly distributed in the inorganic phase during sintering, thereby reducing the sintering activation energy of the GDC layer and forming a denser sintering structure, thereby reducing the thickness of the GDC layer and improving the performance of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is an electron microscope image of the slurry obtained in Example 1 of the present invention after sintering.
[0020] Figure 2 This is an electron microscope image of the slurry obtained in Example 2 of the present invention after sintering.
[0021] Figure 3 This is an electron microscope image of the slurry obtained in Example 3 of the present invention after sintering.
[0022] Figure 4 This is an electron microscope image of the slurry obtained in Example 4 of the present invention after sintering. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work based on the embodiments of the present invention shall fall within the scope of protection of the present invention.
[0024] Example 1.
[0025] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Ethyl cellulose, organic solvent and lecithin are prepared in a weight percentage ratio of 10:85:5, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then ethyl cellulose is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally lecithin is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0026] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 35:65:0, wherein the inorganic phase is gadolinium oxide and cerium oxide, and the gadolinium oxide:cerium oxide = 1:9 (mass ratio); then the slurry is fully ground by rolling with a three-roll mill to a fineness of less than 3μm to obtain a slurry. The porosity is measured to be 38% and the open circuit voltage (V) is 0.64.
[0027] Example 2.
[0028] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Ethyl cellulose, organic solvent and lecithin are prepared in a weight percentage ratio of 10:85:5, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then ethyl cellulose is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally lecithin is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0029] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 35:63:2, wherein the inorganic phase is gadolinium oxide and cerium oxide, gadolinium oxide: cerium oxide = 1:9 (mass ratio), and the additive phase is gadolinium oxalate; then the slurry is fully ground with a three-roll mill to a fineness of less than 3μm to obtain a slurry. The porosity is measured to be 29% and the open circuit voltage (V) is 0.68.
[0030] Example 3.
[0031] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Ethyl cellulose, organic solvent and lecithin are prepared in a weight percentage ratio of 10:85:5, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then ethyl cellulose is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally lecithin is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0032] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 35:60:5, wherein the inorganic phase is gadolinium oxide and cerium oxide, gadolinium oxide: cerium oxide = 1:9 (mass ratio), and the additive phase is gadolinium oxalate; then the slurry is fully ground with a three-roll mill to a fineness of less than 3μm to obtain a slurry. The porosity is measured to be 8% and the open circuit voltage (V) is 0.97.
[0033] Example 4.
[0034] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Ethyl cellulose, organic solvent and lecithin are prepared in a weight percentage ratio of 10:85:5, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then ethyl cellulose is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally lecithin is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0035] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 35:57:8, wherein the inorganic phase is gadolinium oxide and cerium oxide, gadolinium oxide: cerium oxide = 1:9 (mass ratio), and the additive phase is gadolinium oxalate; then, the slurry is fully ground by rolling with a three-roll mill to a fineness of less than 3μm to obtain a slurry. The porosity is measured to be 3%, and the open circuit voltage (V) is 0.99.
[0036] Example 5.
[0037] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Ethyl cellulose, organic solvent and lecithin are prepared in a weight percentage ratio of 10:85:5, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then ethyl cellulose is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally lecithin is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0038] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 35:57:8, wherein the inorganic phase is gadolinium oxide and cerium oxide, gadolinium oxide: cerium oxide = 1:9 (mass ratio), and the additive phase is cerium oxalate; then, the slurry is fully ground with a three-roll mill to a fineness of less than 3μm to obtain a slurry. The porosity is measured to be 3%, and the open circuit voltage (V) is 1.02.
[0039] Example 6.
[0040] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Ethyl cellulose, organic solvent and lecithin are prepared in a weight percentage ratio of 10:85:5, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then ethyl cellulose is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally lecithin is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0041] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 35:57:8, wherein the inorganic phase is gadolinium oxide and cerium oxide, gadolinium oxide: cerium oxide = 1:9 (mass ratio), and the additive phase is gadolinium oxalate and cerium oxalate, gadolinium oxalate: cerium oxalate = 1:1; then the slurry is fully ground with a three-roll mill to a fineness of less than 3μm to obtain a slurry. The porosity is measured to be 6% and the open circuit voltage (V) is 0.99.
[0042] Example 7.
[0043] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: polyvinyl butyral, organic solvent and 1,4-butyrolactone are prepared in a weight percentage ratio of 5:90:5, wherein pentanediol in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and trioctyl acetyl citrate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then polyvinyl butyral is added under stirring conditions, dissolved in the organic solvent at 80°C, and finally 1,4-butyrolactone is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0044] (2) Preparation of slurry: The organic phase, the inorganic phase, and the additive phase are uniformly mixed in a weight percentage of 25:65:10, wherein the inorganic phase is cerium oxide and the additive phase is gadolinium oxalate; then the slurry is fully ground by a three-roll mill to a fineness of less than 3 μm to obtain a slurry. The porosity is measured to be 3% and the open circuit voltage (V) is 0.99.
[0045] Example 8.
[0046] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Nitrocellulose, organic solvent and polyamide wax are prepared in a weight percentage ratio of 30:55:15, wherein butyl acetate in the organic solvent accounts for 45% of the total weight of the organic carrier, tributyl citrate accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, the solvent is placed in a container according to the proportion, and then nitrocellulose is added under stirring conditions, dissolved in the organic solvent at 85°C, and finally the polyamide wax is added. Stir until the mixture is transparent and then cool to obtain an organic phase.
[0047] (2) Preparation of slurry: The organic phase, inorganic phase and additive phase are uniformly mixed in a weight percentage of 50:45:5, wherein the inorganic phase is gadolinium oxide and cerium oxide, gadolinium oxide: cerium oxide = 5:9 (mass ratio), and the additive phase is cerium oxalate; then, the slurry is fully ground by a three-roll mill to a fineness of less than 3 μm to obtain a slurry. The porosity is measured to be 8%, and the open circuit voltage (V) is 0.98.
[0048] Example 9.
[0049] This embodiment provides a technical solution: a fuel cell barrier layer slurry and a preparation method thereof, which are as follows: (1) Preparation of organic phase: Prepare polymethacrylate, organic solvent and methyl amyl alcohol in a weight percentage of 20:68:12, wherein terpineol in the organic solvent accounts for 45% of the total weight of the organic carrier, diethylene glycol monomethyl ether accounts for 20% of the total weight of the organic carrier, and diethylene glycol monomethyl ether acetate accounts for 20% of the total weight of the organic carrier. First, put the solvent in a container according to the proportion, then add polymethacrylate under stirring, dissolve it in the organic solvent at 85°C, and finally add methyl amyl alcohol. Stir until the mixture is transparent and then cool it to obtain an organic phase.
[0050] (2) Preparation of slurry: The organic phase, the inorganic phase and the additive phase are uniformly mixed in a weight percentage of 24:70:6, wherein the inorganic phase is gadolinium oxide, the additive phase is gadolinium oxalate and cerium oxalate, and the ratio of gadolinium oxalate to cerium oxalate is 1:2; then the slurry is fully ground with a three-roll mill to a fineness of less than 3 μm to obtain a slurry. The porosity is measured to be 6% and the open circuit voltage (V) is 0.99.
[0051] Although embodiments of the present invention have been shown and described, it will be apparent to those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and concepts of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A fuel cell barrier layer slurry, comprising an organic phase, an inorganic phase and an additive phase, characterized in that: The weight percentages of the organic phase, inorganic phase and additive phase are as follows: Organic phase 15~50%, inorganic phase 50~75%, additive phase 0.5~10%; The organic phase includes a high molecular polymer, an organic solvent and an organic additive, and the weight percentage of the high molecular polymer, the organic solvent and the organic additive is as follows: High molecular polymer 5~30%, organic solvent 20~95%, organic additive 15% and below; The additive phase is an organic compound of gadolinium and / or an organic compound of cerium.
2. The fuel cell barrier layer slurry according to claim 1, characterized in that: The weight percentages of the organic phase, the inorganic phase and the additive phase are as follows: 30-40% of the organic phase, 55-65% of the inorganic phase and 5-10% of the additive phase.
3. The fuel cell barrier layer slurry according to claim 1, characterized in that: The weight percentage composition of the high molecular polymer, organic solvent and organic auxiliary agent is: 5-15% of the high molecular polymer, 80-95% of the organic solvent and 5-10% of the organic auxiliary agent.
4. The fuel cell barrier layer slurry according to claim 1, characterized in that: The high molecular polymer includes polymethacrylate, polyvinyl alcohol, polyvinyl butyral, ethyl cellulose, nitrocellulose, polyvinyl pyrrolidone, alkyd resin and rosin resin; the organic solvent includes tributyl citrate, trioctyl acetyl citrate, pentanediol, terpineol, diethylene glycol monomethyl ether, diethylene glycol monomethyl ether acetate and butyl acetate; the organic auxiliary agent includes lecithin, silane coupling agent, titanate coupling agent, polyamide wax, polyacrylic acid, octadecylamine, stearate, 1,4-butyrolactone, sodium lauryl sulfate, methyl amyl alcohol and oleyl amino oleate.
5. The fuel cell barrier layer slurry according to claim 1, characterized in that: The inorganic phase includes gadolinium oxide, cerium oxide or a mixture of the two in different proportions.
6. The fuel cell barrier layer slurry according to claim 1, characterized in that: The additive phase includes one or more of gadolinium oxalate, gadopentane acid, cerium oleate, cerium citrate, cerium oxalate, gadolinium stearate, cerium stearate, and gadolinium laurate.
7. A method for preparing a fuel cell barrier layer slurry according to any one of claims 1 to 6, characterized in that the steps as follows: 1) Preparing an organic phase: heating and dissolving a polymer in an organic solvent according to the weight percentage composition, then adding an organic additive, stirring with a stirrer until the polymer is completely dissolved, and cooling to obtain an organic phase; 2) Preparation of slurry: The organic phase, the inorganic phase and the additive phase are mixed evenly using a stirrer according to the weight percentage composition, and then fully ground using a three-roll mill to a fineness of 3 μm or less to obtain a slurry.
8. The method for preparing a fuel cell barrier layer slurry according to claim 7, characterized in that: In step 1), the organic solvent is first added into the container in proportion, and then the high molecular polymer is added under stirring conditions, dissolved in the organic solvent at 80-85° C., and finally the organic auxiliary agent is added; the mixture is stirred until transparent and then cooled to obtain an organic phase.
9. The method for preparing a fuel cell barrier layer slurry according to claim 7, characterized in that: In step 2), the mass ratio of gadolinium oxide to cerium oxide in the inorganic phase is (1-3): (7-9).
10. The method for preparing a fuel cell barrier layer slurry according to claim 7 or 9, characterized in that: In step 2), the additive phase accounts for 5-8% of the total weight.