Polycarbonate-based solid electrolyte with high ion transference number and preparation method thereof

By dispersing inorganic nanofillers in dialdehyde solution and introducing crown ether diamine and triamine to form COF structure, combining lithium salt and polycarbonate, the low ion migration number and low ion migration number in high energy density batteries is solved. The problem of insufficient interface compatibility achieves high ion migration number and excellent conductivity, and improves the mechanical and chemical stability of the battery.

CN119092809APending Publication Date: 2024-12-06ZHEJIANG ZHIBANG LITHIUM BATTERY NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196591.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional solid electrolytes have low ion migration numbers, low conductivity in high energy density batteries, and insufficient interface compatibility with electrode materials, which affects the overall performance and cycle stability of the battery.

Method used

Using a polycarbonate-based solid electrolyte preparation method with high ion migration number, the covalent organic framework (COF) is formed by dispersing inorganic nanofillers in a dialdehyde solution and introducing crown ether diamine and triamine. Mixed with lithium salts in supercritical carbon dioxide environment, combined with polycarbonate and plasticizer to form modified inorganic nanofillers, improving the ion transport channel and mechanical strength of the electrolyte.

Benefits of technology

It significantly improves the number of ion mobility, conductivity and mechanical strength of the electrolyte, enhances the physical and chemical stability of the battery, extends the service life of the electrolyte, and maintains good battery performance over a wide temperature range.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a polycarbonate-based solid electrolyte with high ion transference number, which comprises the following steps: S1, dispersing an inorganic nanofiller in a dialdehyde solution in a warm water bath, sequentially adding crown ether diamine and triamine, then adding a catalyst, uniformly stirring and mixing, and heating for reaction to form a COF coated and modified inorganic nanofiller; s2, adding the mixture into a reaction kettle, introducing carbon dioxide gas, and uniformly mixing the mixture with lithium salt in a supercritical state; and S3, carrying out high-energy ball milling on the mixture, polycarbonate, a plasticizer and an auxiliary agent, uniformly mixing, then coating a substrate with the mixture, and curing to obtain the polycarbonate-based solid electrolyte. According to the preparation method of the polycarbonate-based solid electrolyte, the polycarbonate-based solid electrolyte has the excellent performance of high ion transference number, the transmission efficiency of lithium ions is enhanced through COF coating modification, meanwhile, the high conductivity and good mechanical performance of the electrolyte are guaranteed, and the requirements of batteries with high energy density and high safety can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid electrolytes, and in particular to a polycarbonate-based solid electrolyte with a high ion migration number and a preparation method thereof. Background Art

[0002] In today's rapidly developing energy storage field, solid electrolytes, as one of the core components of lithium-ion batteries, have received widespread attention. Traditional solid electrolytes, despite their advantages in safety and thermal stability, still have some limitations, such as low ion migration number and conductivity, which limit their application in high energy density batteries. In addition, the poor interface compatibility between solid electrolytes and electrode materials also affects the overall performance and cycle stability of the battery. In the prior art, although the introduction of inorganic nanofillers can improve mechanical properties, it is often accompanied by problems of processing complexity and dispersion uniformity, which in turn affects the ion transport efficiency of the electrolyte. Therefore, the development of solid electrolytes with high ion migration number, excellent conductivity and good interface compatibility is the key to promoting the development of high energy density and high safety battery technology. At present, researchers are committed to exploring new materials and innovative preparation technologies to overcome the shortcomings of existing solid electrolytes and meet the growing demand for energy storage. Summary of the invention

[0003] In view of the above shortcomings of the prior art, the present invention provides a method for preparing a polycarbonate-based solid electrolyte with a high ion migration number to solve the technical problems encountered by traditional solid electrolytes in high energy density battery applications, such as low ion migration number, low electrical conductivity, and insufficient interface compatibility with electrode materials.

[0004] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0005] A method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number, the preparation method comprising the following steps:

[0006] S1: In a warm water bath, the inorganic nanofiller is dispersed in a dialdehyde solution, crown ether diamine and triamine are added in sequence, and then a catalyst is added, stirred and mixed evenly, and the temperature is raised to react to form a COF-coated modified inorganic nanofiller;

[0007] S2: adding the COF-coated and modified inorganic nanofiller obtained in step S1 into a reactor, introducing carbon dioxide gas, and mixing it evenly with the lithium salt under a supercritical state;

[0008] S3: The modified inorganic nanofiller obtained in step S2 is mixed evenly with polycarbonate, plasticizer, and additive by high-energy ball milling, and then coated on a substrate, and cured to obtain the polycarbonate-based solid electrolyte.

[0009] In the preparation process of step S1 of the present invention, firstly, the inorganic nanofiller is dispersed in the dialdehyde solution to achieve its uniform distribution in the subsequent materials, which helps to improve the overall performance of the electrolyte. Subsequently, crown ether diamines and triamines and catalysts are added to promote the formation of a covalent organic framework (COF), which not only provides additional ion transport channels and enhances the ion migration number of the electrolyte, but also improves the interfacial compatibility of the filler and the polycarbonate matrix through synergy with the inorganic nanofiller, reduces the interfacial impedance, and thus improves the ion transmission efficiency. The addition of inorganic nanofillers also significantly improves the mechanical strength of the final solid electrolyte and enhances the physical stability and durability of the battery. At the same time, the introduction of COF structure and inorganic nanofillers improves the thermal stability of the electrolyte, allowing it to work in a wider temperature range without losing structural integrity, and provides additional chemical stability, resists hydrolysis and oxidation, and effectively prolongs the service life of the electrolyte.

[0010] In the preparation process of step S2, by mixing the COF-coated modified inorganic nanofiller and the lithium salt under a supercritical carbon dioxide environment, the agglomeration of the inorganic nanofiller particles can be effectively avoided, and the uniformly dispersed modified inorganic nanofiller helps to form a continuous ion transport network, thereby enhancing the ionic conductivity of the electrolyte. At the same time, the permeability of the supercritical fluid can optimize the electrolyte structure at the nanoscale, improve its density and uniformity, reduce the interface energy between the inorganic nanofiller, the lithium salt and the polymer matrix, promote the combination between them, reduce the phase separation phenomenon, and thus obtain a more stable solid electrolyte.

[0011] As a preferred technical solution, the dialdehyde is at least one of glyoxal, succinaldehyde, terephthalaldehyde, furan dicarboxaldehyde, and glutaraldehyde.

[0012] As a preferred technical solution, the inorganic nanofiller is at least one of aluminum oxide, titanium dioxide, boron nitride, zinc oxide, zirconium oxide, and graphene.

[0013] As a preferred technical solution, the crown ether diamine is 4',4"-diaminodibenzo-18-crown-6 and / or 4',4" (5")-diaminodibenzo-15-crown-5.

[0014] As a preferred technical solution, the ternary amine is at least one of 1,5,9-benzotriamine, tris(4-aminophenyl)amine, tris(4'-amino-1,1'-biphenyl)amine, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 4,4',4"-triaminotriphenylmethane, and 1,3,5-tris(4-aminophenyl)benzene.

[0015] As a preferred technical solution, the lithium salt is at least one of LiClO4, LiPF6, LiBF4, LiTaF6, LiCF3SO3, LiN(SO2CF3)2, LiTFSI, and LiTf.

[0016] As a preferred technical solution, the plasticizer is composed of at least one carbonate selected from propylene carbonate, ethylene carbonate, propylene carbonate, and dimethyl carbonate and at least one ester compound selected from methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate (EA), propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, and butyl butyrate.

[0017] As a preferred technical solution, the auxiliary agent is at least one of an antioxidant, an ultraviolet absorber, a lubricant, and an antistatic agent.

[0018] Another aspect of the present invention is to provide a polycarbonate-based solid electrolyte with a high ion transfer number, wherein the polycarbonate-based solid electrolyte is prepared by the above-mentioned method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number.

[0019] Beneficial effects of the present invention:

[0020] The method for preparing a polycarbonate-based solid electrolyte with a high ion migration number of the present invention disperses inorganic nanofillers in a dialdehyde solution and introduces crown ether diamine and triamine to form a COF structure, which not only realizes the effective combination of inorganic nanofillers and polycarbonate matrix, but also significantly improves the ion migration number of the electrolyte. This design not only enhances the mechanical strength and thermal stability of the electrolyte, but also improves its chemical stability and conductivity, which helps to maintain battery performance in a wide range of application environments.

[0021] In general, the polycarbonate-based solid electrolyte of the present invention not only has excellent electrochemical and mechanical properties, but also ensures its long-term durability and operational stability in a wide temperature range. It has strong overall comprehensive performance and can meet the long-term durability and stability requirements of high energy density and high safety batteries. DETAILED DESCRIPTION

[0022] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0023] Example 1

[0024] The method for preparing a polycarbonate-based solid electrolyte with a high ion migration number in this embodiment comprises the following steps:

[0025] S1: In a 45°C warm water bath, 20g of inorganic nanofiller zirconium oxide was dispersed in 200mL of glutaraldehyde solution, and 0.45mol of 4',4"-diaminodibenzo-18-crown-6 and 0.15mol of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine were added in sequence, and then an appropriate amount of catalyst acetic acid solution was added, stirred and mixed evenly, and the temperature was raised to 110°C for reaction for 1h to form COF-coated modified inorganic nanofiller;

[0026] S2: 35 g of the COF-coated modified inorganic nanofiller obtained in step S1 and 10 g of lithium hexafluoroborate LiPF6 are added to a reactor, and carbon dioxide gas is introduced. Under a supercritical state, the COF-coated modified inorganic nanofiller and lithium hexafluoroborate are uniformly mixed for 5 minutes;

[0027] S3: The modified inorganic nanofiller obtained in step S2 is mixed evenly with polycarbonate, propylene carbonate, ethyl acetate, and an additive by high-energy ball milling, and then coated on a substrate, and cured to obtain the polycarbonate-based solid electrolyte. The mass ratio of the modified inorganic nanofiller to polycarbonate, propylene carbonate, ethyl acetate, and the additive is 5:100:8:7:2.

[0028] The auxiliary agent is composed of an antioxidant (bis(1,2-diphenylethyl) disulfide), an ultraviolet absorber (2-hydroxy-4-methoxybenzophenone), a lubricant (polyethylene wax), and an antistatic agent (ammonium dodecylbenzenesulfonate) in a mass ratio of 2:3:3:2.

[0029] Example 2

[0030] The method for preparing a polycarbonate-based solid electrolyte with a high ion migration number in this embodiment comprises the following steps:

[0031] S1: In a 45°C warm water bath, disperse 20g of inorganic nanofiller boron nitride in 200mL of furan dicarboxaldehyde solution, add 0.45mol of 4',4" (5")-diaminodibenzo-15-crown ether-5 and 0.15mol of 1,5,9-benzotriamine in sequence, and then add an appropriate amount of catalyst acetic acid solution, stir and mix evenly, heat to 110°C and react for 1.5h to form COF-coated modified inorganic nanofiller;

[0032] S2: 35 g of the COF-coated modified inorganic nanofiller obtained in step S1 and 10 g of lithium perchlorate LiClO4 are added to a reactor, and carbon dioxide gas is introduced. Under a supercritical state, the COF-coated modified inorganic nanofiller and lithium perchlorate are uniformly mixed for 5 minutes;

[0033] S3: The modified inorganic nanofiller obtained in step S2 is mixed evenly with polycarbonate, ethylene carbonate, propyl formate, and an additive by high-energy ball milling, and then coated on a substrate, and cured to obtain the polycarbonate-based solid electrolyte. The mass ratio of the modified inorganic nanofiller to polycarbonate, ethylene carbonate, propyl formate, and additive is 5:100:8:7:2.

[0034] The auxiliary agent is composed of an antioxidant (bis(1,2-diphenylethyl) disulfide), an ultraviolet absorber (2-hydroxy-4-methoxybenzophenone), a lubricant (polyethylene wax), and an antistatic agent (ammonium dodecylbenzenesulfonate) in a mass ratio of 2:3:3:2.

[0035] Example 3

[0036] The method for preparing a polycarbonate-based solid electrolyte with a high ion migration number in this embodiment comprises the following steps:

[0037] S1: In a 45°C warm water bath, 20g of inorganic nanofiller zinc oxide was dispersed in 200mL of glyoxal solution, 0.45mol of 4',4"-diaminodibenzo-18-crown-6 and 0.15mol of tris(4'-amino-1,1'-diphenylamine)amine were added in sequence, and then an appropriate amount of catalyst acetic acid solution was added, stirred and mixed evenly, and the temperature was raised to 110°C for reaction for 1h to form COF-coated modified inorganic nanofiller;

[0038] S2: 35 g of the COF-coated modified inorganic nanofiller obtained in step S1 and 10 g of lithium bis(trifluoromethanesulfonyl)imide LiTFSI are added to a reactor, and carbon dioxide gas is introduced. Under a supercritical state, the COF-coated modified inorganic nanofiller and lithium bis(trifluoromethanesulfonyl)imide are uniformly mixed for 5 minutes;

[0039] S3: The modified inorganic nanofiller obtained in step S2 is mixed evenly with polycarbonate, dimethyl carbonate, ethyl propionate, and an additive by high-energy ball milling, and then coated on a substrate, and cured to obtain the polycarbonate-based solid electrolyte. The mass ratio of the modified inorganic nanofiller to polycarbonate, dimethyl carbonate, ethyl propionate, and an additive is 5:100:8:7:2.

[0040] The auxiliary agent is composed of an antioxidant (bis(1,2-diphenylethyl) disulfide), an ultraviolet absorber (2-hydroxy-4-methoxybenzophenone), a lubricant (polyethylene wax), and an antistatic agent (ammonium dodecylbenzenesulfonate) in a mass ratio of 2:3:3:2.

[0041] Comparative Example 1

[0042] The raw material composition and preparation steps of the method for preparing a polycarbonate-based solid electrolyte with a high ion migration number in this comparative example are substantially the same as those in Example 1, except that the preparation method in this comparative example does not include step S1.

[0043] Comparative Example 2

[0044] The raw material composition and preparation steps of the method for preparing a polycarbonate-based solid electrolyte with a high ion migration number in this comparative example are basically the same as those in Example 1, except that the preparation method in this comparative example does not include step S2.

[0045] The polycarbonate-based solid electrolytes with high ion migration numbers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to performance tests, and the performance results are shown in Table 1:

[0046] Among them, the mechanical strength performance test method is: cut the sample into long strips with a length of 120mm and a width of 15mm. On a universal material testing machine, the mechanical strength of the solid electrolyte is evaluated through a tensile test, with tensile strength and elongation at break as evaluation indicators.

[0047] The ionic conductivity performance test is to connect the prepared solid electrolyte sample to an AC impedance spectroscopy measuring instrument to test the ionic conductivity of the solid electrolyte through AC impedance spectroscopy.

[0048] The ion migration number is tested by DC polarization method; the experiment is carried out at an ambient temperature of 25°C, maintaining constant humidity and air pressure. The battery configuration is a symmetrical cell, using stainless steel as the electrode material, with an area of ​​1 square centimeter. A constant DC voltage of 0.5 volts is applied between the two electrodes of the battery. A high-precision digital multimeter is used to record the current value every 30 seconds for the first 10 minutes. The electrolyte is a 10 mm thick solid electrolyte membrane. The change in current through the electrolyte over time is measured to calculate the ion migration number.

[0049] Thermal stability test method: The thermal stability of the sample material is evaluated by thermogravimetric analysis (TGA), specifically by heating from room temperature to 250°C at a heating rate of 5°C / min, and the thermal stability is evaluated based on the mass loss rate of the sample.

[0050] Electrochemical stability window test method: The electrochemical stability window of the electrolyte is determined by cyclic voltammetry (CV), which measures the maximum voltage range that the electrolyte can withstand without decomposition. Table 1 project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Tensile strength, MPa 81.4 78.5 82.3 67.2 81.2 Elongation at break, % 35.4 32.3 35.8 47.6 35.5 Ionic conductivity, S / cm 0.0036 0.0033 0.0034 0.0015 0.0024 Ion migration number 0.96 0.96 0.95 0.85 0.91 Thermal stability, % 0.8 0.7 0.8 1.2 0.9 Electrochemical stability window, V 5.2 5.1 5.3 4.5 4.7

[0051] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention claimed.

Claims

1. A method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number, characterized in that: The preparation method comprises the following steps: S1: In a warm water bath, the inorganic nanofiller is dispersed in a dialdehyde solution, crown ether diamine and triamine are added in sequence, and then a catalyst is added, stirred and mixed evenly, and the temperature is raised to react to form a COF-coated modified inorganic nanofiller; S2: adding the COF-coated and modified inorganic nanofiller obtained in step S1 into a reactor, introducing carbon dioxide gas, and mixing it evenly with the lithium salt under a supercritical state; S3: The modified inorganic nanofiller obtained in step S2 is mixed evenly with polycarbonate, plasticizer, and additive by high-energy ball milling, and then coated on a substrate, and cured to obtain the polycarbonate-based solid electrolyte.

2. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The dialdehyde is at least one of glyoxal, succinaldehyde, terephthalaldehyde, furan dicarboxaldehyde and glutaraldehyde.

3. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The inorganic nanofiller is at least one of aluminum oxide, titanium dioxide, boron nitride, zinc oxide, zirconium oxide and graphene.

4. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The crown ether diamine is 4',4"-diaminodibenzo-18-crown-6 and / or 4',4" (5")-diaminodibenzo-15-crown-5.

5. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The ternary amine is at least one of 1,5,9-benzotriamine, tris(4-aminophenyl)amine, tris(4'-amino-1,1'-biphenyl)amine, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, 4,4',4"-triaminotriphenylmethane and 1,3,5-tris(4-aminophenyl)benzene.

6. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The lithium salt is at least one of LiClO4, LiPF6, LiBF4, LiTaF6, LiCF3SO3, LiN(SO2CF3)2, LiTFSI, and LiTf.

7. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The plasticizer is composed of at least one carbonate selected from propylene carbonate, ethylene carbonate, propylene carbonate and dimethyl carbonate and at least one ester compound selected from methyl formate, ethyl formate, propyl formate, butyl formate, methyl acetate, ethyl acetate (EA), propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate and butyl butyrate.

8. The method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in claim 1, characterized in that: The auxiliary agent is at least one of an antioxidant, an ultraviolet absorber, a lubricant, and an antistatic agent.

9. A polycarbonate-based solid electrolyte with a high ion transfer number, characterized in that: The polycarbonate-based solid electrolyte is prepared by the method for preparing a polycarbonate-based solid electrolyte with a high ion transfer number as claimed in any one of claims 1 to 8.