Total recovery method for negative electrode material of waste lithium battery

By disassembling the lithium battery in an inert atmosphere and using multi-step solvent treatment technology, efficient recycling of the negative electrode material of waste lithium battery is successfully achieved, resource waste and environmental pollution problems in traditional recycling methods are solved, and high-purity recycling and The goal of low energy consumption.

CN119092871APending Publication Date: 2024-12-06QINGDAO QINDACHENG TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411201870.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the recycling and treatment of waste lithium batteries, traditional methods have problems of resource waste and environmental pollution, especially the recycling efficiency and purity of the negative electrode materials are not high, and the energy consumption is high.

Method used

A method for recycling the negative electrode material of waste lithium battery, including disassembly of the lithium battery in an inert atmosphere, separating the lithium ions, copper sheets, graphite powder and binder in the negative electrode material through multi-step solvent treatment, and using distillation and Precipitation technology achieves high purity recovery and reduces energy consumption and pollution by recycling solvents and carbon dioxide precipitants.

Benefits of technology

It realizes efficient recycling of waste lithium battery negative electrode materials, reduces resource waste and environmental pollution, improves resource utilization, and has less time and low energy consumption, and a mild and pollution-free process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092871A_ABST
    Figure CN119092871A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of waste lithium battery recovery, and particularly relates to a total recovery method of a waste lithium battery negative electrode material. The method comprises the following steps: disassembling and crushing a waste lithium battery in an inert gas atmosphere in an electrified manner to obtain a negative electrode material, and treating the negative electrode material in a solvent A to obtain a negative electrode material solid and an electrolyte; and treating the obtained solid in a solvent B to obtain a negative electrode copper sheet, negative electrode powder containing elemental lithium and a binder. And adding the negative electrode powder containing elemental lithium into the solvent C for further treatment to obtain negative electrode graphite powder and lithium carbonate. The method provided by the invention has the advantages of mild conditions, easy realization of operation, simple process, no need of complex equipment, and easy realization of parameters of each process. The method has the advantages of high efficiency, no pollution, high recovery rate and the like, and the used solvent can be recycled, is green and environment-friendly and has high resource utilization rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recycling waste lithium batteries, and in particular relates to a method for fully recycling negative electrode materials of waste lithium batteries. Background Art

[0002] At present, lithium-ion batteries are widely used in large-scale energy storage, electric vehicles, electronic products and other fields. With the promotion and use of electric vehicles, the demand for lithium-ion batteries has increased year by year (patent CN 115571925). As the key to the power of new energy vehicles, lithium batteries are widely used due to their excellent chemical properties. As a result, more and more power batteries are scrapped; the problem is the recycling and treatment of waste power batteries (Energy Storage Science and Technology, 2023, 12(3), 822-834). Waste lithium batteries contain high-value resources such as metal materials, graphite powder, binders, and electrolytes. Therefore, waste lithium batteries have extremely high recycling value (patent CN 117488080 A).

[0003] If waste batteries cannot be effectively recycled, it will not only cause a waste of resources, but also cause certain pollution to the environment (patent CN 117566709 A). If a large number of scrapped lithium batteries are recycled, an important step is to recycle the negative electrode material and the electrolyte it contains. During the discharge process, some lithium ions can return to the positive electrode normally, but the discharge process is time-consuming and energy-consuming. The most direct way is to disassemble them with power. A large number of lithium ions remain on the negative electrode material when it is charged. If they are not recycled during battery recycling, it will not only cause a waste of resources, but also pollute the environment and cause combustion and other hazards. The traditional recycling process uses a high-temperature combustion method. The separation steps are complex and energy-consuming, and the purity of the obtained product is not high. The recycling process will also cause certain environmental pollution (Journal of the Chinese Society of Nonferrous Metals, 2019, 29(4), 878-886).

[0004] Therefore, how to efficiently recycle waste lithium battery negative electrode materials to avoid waste of resources and environmental pollution is a problem that needs to be solved urgently. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for fully recycling negative electrode materials of waste lithium batteries, recover the lithium ions remaining on the negative electrode materials, and recover and reuse the metal copper sheets, electrolytes, binders, and negative electrode graphite powder on the negative electrode materials, thereby reducing costs and improving resource utilization. The method is time-saving, energy-saving, and pollution-free.

[0006] The technical solutions adopted are:

[0007] A method for fully recycling negative electrode materials of waste lithium batteries comprises the following steps:

[0008] (1) dismantling the charged lithium battery in an inert atmosphere to separate and crush the negative electrode material with electrolyte;

[0009] (2) treating the negative electrode material containing the electrolyte obtained in step (1) in solvent A to obtain the negative electrode material and solvent A containing the electrolyte; distilling the solution A containing the electrolyte to obtain the electrolyte and solvent A;

[0010] (3) The negative electrode material obtained in step (2) is treated in solvent B to obtain a negative electrode copper sheet, a negative electrode powder containing elemental lithium, and solvent B containing a binder, and the solution B containing the binder is distilled to obtain a binder and solvent B;

[0011] (4) The negative electrode powder containing elemental lithium obtained in step (3) is treated in solvent C to obtain high-purity negative electrode graphite powder and solution C containing lithium hydroxide; and the solution C containing lithium hydroxide is further treated to obtain high-purity lithium carbonate precipitate and solvent C.

[0012] Preferably, in step (1), the inert atmosphere is one or more of nitrogen, argon or helium, preferably nitrogen.

[0013] Preferably, in step (1), the disassembly is performed by mechanical disassembly or manual disassembly, and the crushing is performed by mechanical crushing or manual crushing, and the size of the crushed objects is between 0.1-10 cm, preferably 1-5 cm.

[0014] Preferably, in the above step (2), solvent A is at least one of diethyl ether, ethylene glycol dimethyl ether, petroleum ether, ethyl acetate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, chloroform, dichloroethane, dichloroethylene, trichloroethylene, acetonitrile, acetone, tetrahydrofuran, methanol, ethanol, propanol, and isopropanol.

[0015] Preferably, in the above step (2), the treatment method refers to at least one of immersion, standing, stirring, ultrasound, vibration, hydrothermal, and solvent thermal; the distillation adopts atmospheric distillation or reduced pressure distillation, the distillation temperature is 30-200° C., the pressure is 0.1 Pa-100 kPa, and the time is 1-6 hours;

[0016] Preferably, in the above step (3), solvent B is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl ether, ethylene glycol dimethyl ether, petroleum ether, ethyl acetate, dichloromethane, chloroform, dichloroethane, dichloroethylene, trichloroethylene, acetonitrile, acetone, tetrahydrofuran, methanol, ethanol, propanol, and isopropanol.

[0017] Preferably, in the above step (3), the treatment method refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, and solvent thermal, and the time is 1 to 6 hours; the distillation adopts atmospheric distillation or reduced pressure distillation, the distillation temperature is 30 to 200°C, the pressure is 0.1Pa-100kPa, and the time is 1 to 48 hours, preferably 1 to 6 hours.

[0018] Preferably, in the above step (4), solvent C is at least one of diethyl ether, ethylene glycol dimethyl ether, ethyl acetate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, acetonitrile, acetone, tetrahydrofuran, water, sulfuric acid, nitric acid, benzenesulfonic acid, methanol, ethanol, propanol, and isopropanol.

[0019] Preferably, in the above step (4), the treatment method is at least one of sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, screening, and spray drying, and the time is 1 to 6 hours; the further treatment method refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, solvent thermal, sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, screening, and spray drying, and the time is 1 to 48 hours, preferably 1 to 6 hours;

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention is a method for fully recycling the negative electrode materials of waste lithium batteries. The lithium battery is compatible with at least one of ternary lithium batteries, lithium iron phosphate batteries, lithium cobalt oxide batteries, lithium manganese oxide batteries, nickel lithium manganese oxide batteries, nickel cobalt lithium manganese oxide batteries, nickel cobalt aluminum oxide batteries, and lithium titanate batteries. The present invention has mild temperature, easy conditions, simple operation process, no need for complex equipment, easy parameters of each process, and has the characteristics of high efficiency and pollution-free. The present invention can realize the effective recovery of negative electrode copper sheets, negative electrode graphite powder, electrolyte, and residual lithium elements on the negative electrode, avoiding waste of lithium resources and pollution of the environment. The solvent used for recovery can be recycled and reused, and carbon dioxide is used as a precipitant, which is more energy-saving and environmentally friendly, and can be recycled and processed in large quantities. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Flow chart of the method of the present invention. DETAILED DESCRIPTION

[0023] The embodiments are only for illustrative purposes; in order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0024] Example 1

[0025] like Figure 1 As shown, a method for fully recycling negative electrode materials of waste lithium batteries comprises the following steps:

[0026] (1) A used charged ternary lithium battery is disassembled in an inert atmosphere to remove the outer shell, separate the negative electrode material and crush it;

[0027] (2) Immerse the negative electrode material in solvent A with a volume ratio of 1:2, wherein the composition of solvent A is N-methylpyrrolidone, N,N-dimethylformamide and chloroform, and the volume ratio is 1:1:1. After stirring the solvent with a stirrer for 30 minutes, the stirrer speed is 400r / min, and the negative electrode material and solvent A containing the electrolyte are obtained by vacuum filtration at a pressure of 10Pa for 30 minutes; and the electrolyte and solvent A are obtained by distillation. The distillation adopts vacuum distillation at a pressure of 10Pa, a temperature of 60°C, and a time of 2h.

[0028] (3) All the negative electrode materials of the battery obtained in step 2 are completely immersed in a solvent B with a volume ratio of 1:2, wherein the composition of solvent B is tetrahydrofuran, dichloromethane and ethyl acetate, and the volume ratio is 1:1:1. The negative electrode material is stirred by a stirrer for 30 minutes, and the stirrer speed is 400r / min; after the negative electrode copper sheet, the lithium-containing negative electrode powder and the binder are separated, the copper sheet, the lithium-containing negative electrode powder and the solvent B containing the binder are obtained by processing; the processing method is to filter with filter screens of different apertures, and the filter diameter of the filter screen is 10μm-10cm. When the aperture is 100μm-10cm, the negative electrode copper sheet is obtained; when the aperture is 10-100μm, the negative electrode graphite powder and the solvent B containing the binder are obtained; the binder and the solvent B are obtained by distillation, and the distillation adopts reduced pressure distillation, the pressure is 10Pa, the temperature is 60℃, and the time is 2h.

[0029] (4) Add the graphite powder containing elemental lithium obtained in step 3 to solvent C with a volume ratio of 1:2, wherein the composition of solvent C is tetrahydrofuran, water and ethyl acetate, and the volume ratio is 1:1:1. After stirring the solvent with an agitator for 30 minutes, the agitator speed is 400r / min; vacuum filtration is performed to obtain high-purity negative electrode graphite powder and solvent C containing lithium hydroxide, the pressure is 10Pa, and the time is 30min; CO2 is introduced into solvent C containing lithium hydroxide, the introduction time is 60min, the pH is detected to be 7.0, and vacuum filtration is performed to obtain high-purity lithium carbonate precipitate and solvent C, the pressure is 10Pa, and the time is 30min.

[0030] Example 2

[0031] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0032] The volume ratio of N-methylpyrrolidone, N,N-dimethylformamide and chloroform in step (2) is 1:1:1, and N-methylpyrrolidone, N,N-dimethylformamide and toluene are replaced by the volume ratio of N-methylpyrrolidone, N,N-dimethylformamide and toluene in a volume ratio of 1:1:1.

[0033] The remaining unmentioned contents are the same as those in Example 1.

[0034] Example 3

[0035] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0036] The N-methylpyrrolidone, N,N-dimethylformamide and chloroform in a volume ratio of 1:1:1 in step (2) are replaced by N-methylpyrrolidone, dichloromethane and ethanol in a volume ratio of 1:1:1.

[0037] The remaining unmentioned contents are the same as those in Example 1.

[0038] Example 4

[0039] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0040] The volume ratio of N-methylpyrrolidone, N,N-dimethylformamide and chloroform in step (2) is 1:1:1, and N-methylpyrrolidone, chloroform and acetone in a volume ratio of 1:1:1 are replaced.

[0041] The remaining unmentioned contents are the same as those in Example 1.

[0042] Example 5

[0043] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0044] The volume ratio of N-methylpyrrolidone, N,N-dimethylformamide and chloroform in step (2) is 1:1:1, and then replaced by a volume ratio of N-methylpyrrolidone, N,N-dimethylformamide and chloroform in a volume ratio of 1:2:3.

[0045] The remaining unmentioned contents are the same as those in Example 1.

[0046] Example 6

[0047] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0048] The tetrahydrofuran, dichloromethane and ethyl acetate in a volume ratio of 1:1:1 in step (3) are replaced with tetrahydrofuran, dichloromethane and ethyl acetate in a volume ratio of 1:2:3.

[0049] The remaining unmentioned contents are the same as those in Example 1.

[0050] Example 7

[0051] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0052] The tetrahydrofuran, water and ethyl acetate in a volume ratio of 1:1:1 in step (4) are replaced with tetrahydrofuran, water and ethyl acetate in a volume ratio of 1:2:3.

[0053] The remaining unmentioned contents are the same as those in Example 1.

[0054] Example 8

[0055] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0056] The tetrahydrofuran, water and ethyl acetate in a volume ratio of 1:1:1 in step (4) are replaced with ethanol, water and acetonitrile in a volume ratio of 1:1:1.

[0057] The remaining unmentioned contents are the same as those in Example 1.

[0058] Example 9

[0059] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0060] The ternary lithium battery with a charge of 3.9V in step (1) is replaced with a lithium iron phosphate battery with a charge of 4.1V.

[0061] The remaining unmentioned contents are the same as those in Example 1.

[0062] Example 10

[0063] A method for fully recycling negative electrode materials of waste lithium batteries, which is different from Example 1 in that:

[0064] The ternary lithium battery with a charge of 3.9V in step (1) is replaced with a lithium cobalt oxide battery with a charge of 3.6V.

[0065] The remaining unmentioned contents are the same as those in Example 1.

[0066] Comparative Example 1

[0067] The traditional pyrolysis process is used to recycle the negative electrode materials of waste charged lithium batteries. The specific steps are as follows: dismantle the waste charged lithium batteries with electricity to obtain the negative electrode materials of waste charged lithium batteries; place the above-mentioned negative electrode materials of waste charged lithium batteries in a nitrogen-protected tubular furnace at 600℃ for 3h, ball mill for 1h, with a ball-to-material ratio of 30:1, and sieve through a sieve after grinding. The mesh number of the sieve used for sieving is 120 meshes, and the negative electrode powder and positive electrode current collector are recovered.

[0068] Comparative Example 2

[0069] The conventional friction de-powdering process is used to recycle the negative electrode materials of waste charged lithium batteries. The difference from comparative example 1 is that the operation of calcining at 600°C for 3h in a nitrogen-protected tubular furnace is removed and replaced by physical friction de-powdering.

[0070] Comparative Example 3

[0071] The conventional wet acid soaking process was used to recycle the negative electrode materials of waste charged lithium batteries. The difference from Comparative Example 1 was that the operation of calcining at 600°C for 3h in a nitrogen-protected tubular furnace was removed and replaced with soaking in concentrated sulfuric acid, followed by filtering, washing with water, and drying.

[0072] Table 1 Comparison of the recovery rate of negative electrode materials of waste charged lithium batteries in Examples 1-10 and Comparative Examples 1-3

[0073]

[0074]

[0075] By comparison, the method of the present invention has mild conditions, easy operation, simple process, no need for complex equipment, and easy implementation of parameters of each process. It has the advantages of high efficiency, no pollution, high recovery rate, etc., and at the same time, all resources are recovered, such as negative electrode graphite powder, electrolyte, binder, negative electrode current collector copper sheet, and residual lithium element on the negative electrode, avoiding waste of lithium resources and pollution of the environment. The solvent used for recycling can be recycled and reused, and carbon dioxide is used as a precipitant, which is more energy-saving and environmentally friendly. In terms of full resource recycling, it is superior to traditional processes and can be recycled and processed in large quantities.

[0076] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for fully recycling negative electrode materials of waste lithium batteries, characterized in that: The steps include: (1) dismantling the charged lithium battery in an inert atmosphere to separate and crush the negative electrode material with electrolyte; (2) treating the negative electrode material containing the electrolyte obtained in step (1) in solvent A to obtain the negative electrode material and solvent A containing the electrolyte; distilling the solution A containing the electrolyte to obtain the electrolyte and solvent A; (3) The negative electrode material obtained in step (2) is treated in solvent B to obtain a negative electrode copper sheet, a negative electrode powder containing elemental lithium, and solvent B containing a binder, and the solution B containing the binder is distilled to obtain a binder and solvent B; (4) The negative electrode powder containing elemental lithium obtained in step (3) is treated in solvent C to obtain high-purity negative electrode graphite powder and solution C containing lithium hydroxide; and the solution C containing lithium hydroxide is further treated to obtain high-purity lithium carbonate precipitate and solvent C.

2. The method for fully recycling negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (1), the inert atmosphere is at least one of nitrogen, argon or helium.

3. The method for fully recovering negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (1), the disassembly is performed by mechanical disassembly or manual disassembly, and the crushing is performed by mechanical crushing or manual crushing, and the size of the crushed objects is between 0.1 and 10 cm.

4. The method for fully recovering negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (2), solvent A is at least one of ether, ethylene glycol dimethyl ether, petroleum ether, ethyl acetate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, dichloromethane, chloroform, dichloroethane, dichloroethylene, trichloroethylene, acetonitrile, acetone, tetrahydrofuran, methanol, ethanol, propanol, and isopropanol.

5. The method for fully recycling negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (2), the treatment method refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, solvent thermal, sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, screening, and spray drying, and the time is 0.1 to 6 hours; the distillation adopts atmospheric distillation or reduced pressure distillation, the distillation temperature is 30 to 200° C., and the time is 1 to 6 hours.

6. The method for fully recovering negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (3), solvent B is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl ether, ethylene glycol dimethyl ether, petroleum ether, ethyl acetate, dichloromethane, chloroform, dichloroethane, dichloroethylene, trichloroethylene, acetonitrile, acetone, tetrahydrofuran, methanol, ethanol, propanol, and isopropanol.

7. The method for fully recovering negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (3), the treatment method refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, solvent thermal, sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, screening, and spray drying, and the time is 0.1 to 6 hours; the distillation adopts atmospheric distillation or reduced pressure distillation, the distillation temperature is 30 to 200° C., and the time is 1 to 6 hours.

8. The method for fully recovering negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (4), the solvent C is at least one of diethyl ether, ethylene glycol dimethyl ether, ethyl acetate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, acetonitrile, acetone, tetrahydrofuran, water, sulfuric acid, nitric acid, benzenesulfonic acid, methanol, ethanol, propanol, and isopropanol.

9. The method for fully recovering negative electrode materials of waste lithium batteries according to claim 1, characterized in that: In the step (4), the treatment method refers to at least one of sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, screening, and spray drying, and the time is 1 to 6 hours; the further treatment method refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, solvent thermal, sedimentation, filtration, membrane filtration, filter press, suction filtration, centrifugation, electrophoresis, crystallization, screening, and spray drying, and the time is 1 to 48 hours, preferably 1 to 6 hours.

Citation Information

Cited By

  • Method for recycling all resources of waste lithium batteries

    CN119092869A