Method for completely recycling positive electrode material of waste battery

Through solvent treatment and separation steps, the problems of high energy consumption and pollution in lithium battery recycling are solved, and the efficient and low energy consumption recovery of lithium battery positive electrode materials are achieved, which reduces costs and improves resource utilization, and provides an environmentally friendly and safe process flow .

CN119092872APending Publication Date: 2024-12-06QINGDAO QINDACHENG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201871.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing lithium battery recycling methods have problems of high energy consumption, pollution and high cost, especially the high-temperature combustion treatment produces toxic gases, while the acid-immersion method is complex and the equipment requirements are high, resulting in waste of lithium element resources and environmental pollution.

Method used

The positive electrode material of lithium battery is separated by solvent treatment. Through charged crushing, solvent dissolving binder, filtration and drying and distillation, the efficient recovery of positive electrode powder, binder and current collector is achieved, so as to avoid the generation of pollutants during the pyrolysis process. Reduce equipment maintenance costs.

Benefits of technology

It realizes efficient and low-energy recycling of the cathode material of waste lithium battery, reduces exhaust gas treatment costs, improves resource utilization, reduces recycling costs, and provides an environmentally friendly and safe process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092872A_ABST
    Figure CN119092872A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of waste lithium battery recovery, and particularly relates to a method for fully recovering a positive electrode material of a waste battery. According to the method, all-resource recovery of the waste lithium battery positive electrode material subjected to charged crushing and disassembling can be realized. The method comprises the following steps: treating and dissolving a binder by using a solvent aiming at the positive electrode part of the waste lithium battery which is crushed and disassembled in an electrified manner, separating a positive electrode material from a positive electrode current collector sheet, filtering through filter screens with two pore diameters, separating and drying to obtain the positive electrode current collector sheet and positive electrode powder, distilling filtrate to recover the solvent, and refining residues to obtain the positive electrode binder. The method provided by the invention has the characteristics of simple flow, easy operation realization, efficient recovery and no pollution, can realize all-resource recovery of all components including the positive electrode powder, the positive electrode current collector and the positive electrode binder in the positive electrode material of the waste charged lithium battery, avoids resource waste and environmental pollution, reduces the content of metal impurities such as aluminum in the positive electrode powder, and reduces the production cost. And the quality and value of the recycled positive electrode powder are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium battery recycling, and in particular relates to a method for fully recycling positive electrode materials of waste batteries. Background Art

[0002] As the current new energy vehicle industry enters a stage of rapid development and application technology continues to mature, lithium batteries, as the key to the power of new energy vehicles, have occupied a large share of the market due to their excellent chemical properties, and their production and application in new energy vehicles are also increasing day by day. Therefore, the number of corresponding scrapped lithium batteries is also increasing year by year. After a long period of use, lithium batteries cannot meet the performance standards of normal application scenarios, and simple stacking and discarding will not only cause environmental pollution and potential health hazards caused by the leakage of heavy metal elements, but also easily lead to resource waste of precious metal elements represented by lithium (patent CN 115141933 B). Therefore, utilizing the differences between the physical and chemical properties of the constituent materials, completing the recycling of materials through a process of cascade separation and enrichment, and improving the economic benefits of realizing high-value materials for lithium batteries is a good solution that conforms to the green economy (Journal of Power Sources, 2022, 20, 86-91).

[0003] Nowadays, the main structure of lithium batteries can be roughly divided into positive electrode, negative electrode, current collector, diaphragm and electrolyte (patent number: CN 117563557A). In addition, lithium elements are unevenly distributed in various parts of the battery. In order to achieve the overall efficient recovery of lithium elements, different treatment methods are often used for different actual environments during the recovery process (patent CN117650302 A). At present, the methods used by most battery recycling companies for recycling lithium battery materials are mainly divided into high-temperature combustion treatment and wet treatment of acid leaching (patent CN 117660761 A). The former is easy to operate, but it consumes a lot of energy during the treatment process, produces a large amount of toxic gases, and pollutes the environment (Chemical Management, 2023, 28, 91-94). The latter has a high recovery rate for lithium element materials, but it is often complicated to operate and requires the use of a large amount of organic acid and inorganic acid, which in turn produces a large amount of difficult-to-treat acidic wastewater (Nonferrous Metals, 2019, 3, 68-72). In addition, the wet treatment process using acid leaching has high requirements on equipment due to the corrosive effect of acidic substances, which increases the cost of subsequent equipment maintenance. In addition, some treatment processes also require the use of a certain amount of oxidant, which further increases the recycling cost of the battery (Contemporary Chemical Research, 2023, 2, 28-30, patent CN 117446769A).

[0004] Therefore, it is extremely urgent to develop a simple, efficient, practical, low-cost and pollution-free method for recycling lithium battery materials. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for fully recycling the positive electrode materials of waste batteries. The method has the characteristics of high efficiency and low energy consumption, is easy to implement, has a short process flow, consumes less time, and does not require a high-temperature roasting process. The technical solution adopted is:

[0006] A method for fully recycling positive electrode materials of waste batteries, the method comprising the following steps:

[0007] (1) Dismantling the waste charged lithium battery by charged crushing to obtain the waste charged lithium battery positive electrode material;

[0008] (2) treating the waste charged lithium battery positive electrode material obtained in step (1) with a solvent to dissolve the binder, so that the positive electrode powder is separated from the positive electrode current collector sheet to obtain a mixture I; the mixture I comprises a solvent, a positive electrode binder, a positive electrode powder and a positive electrode current collector sheet;

[0009] (3) filtering the mixture I obtained in step (2) through a large-pore filter to obtain a mixture II, and drying the material on the filter to obtain a positive electrode current collector sheet; the mixture II includes a solvent, a positive electrode binder and a positive electrode powder;

[0010] (4) filtering the mixture II obtained in step (3) through a small-pore filter to obtain a mixture III, and drying and grinding the material on the filter to obtain a positive electrode powder; the mixture III includes a solvent and a positive electrode binder;

[0011] (5) The mixture III obtained in step (4) is distilled to recover the solvent, and the residue is purified to obtain a positive electrode binder.

[0012] Preferably, in step (2), the solvent is at least one of dichloroethylene, trichloroethylene, dichloromethane, chloroform, dichloroethane, N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, methanol, ethanol, propanol, isopropanol, acetonitrile, ether, anisole, diethylene glycol dimethyl ether, acetone, tetrahydrofuran, and water;

[0013] Preferably, in step (2), the mass ratio of the solvent to the positive electrode material of the waste charged lithium battery is 1:1 to 10:1; the mass ratio of the solvent to the positive electrode material of the waste charged lithium battery is 2 to 8:1.

[0014] Preferably, in step (2), the treatment refers to at least one of immersion, standing, stirring, ultrasound, vibration, hydrothermal, and solvent thermal, with a treatment temperature of 10 to 150° C. and a treatment time of 0.1 to 48 h;

[0015] More preferably, in step (2), the treatment temperature is 30 to 130° C. and the treatment time is 1 to 5 hours.

[0016] Preferably, in step (3), the pore size of the large-pore filter screen is 40 to 250 meshes;

[0017] More preferably, in step (3), the pore size of the large-pore filter screen is 40 to 80 meshes.

[0018] Preferably, in step (4), the pore size of the small-pore filter is 0.1 to 100 microns; more preferably, in step (4), the pore size of the small-pore filter is 0.2 to 10 microns.

[0019] Preferably, in step (4), the drying temperature is 50 to 150° C. and the drying time is 1 to 48 hours;

[0020] More preferably, in step (4), the drying temperature is 120-150° C. and the drying time is 2-5 hours.

[0021] Preferably, in step (4), grinding is performed by ball milling or rod milling, and the rod / ball material ratio is 15 to 30:1.

[0022] Preferably, in step (5), the distillation is one of atmospheric distillation and reduced pressure distillation, the distillation temperature is 50-210° C., the pressure is 0.15-100 kPa, and the time is 1-6 h;

[0023] More preferably, in step (5), the distillation temperature is 90-210°C.

[0024] Preferably, in step (5), the refining is at least one of recrystallization, flocculation sedimentation, dissolution, filtration, distillation, decolorization, membrane filtration, centrifugation, drying, etc.;

[0025] More preferably, in step (5), the purification is first filtering, then decolorizing, recrystallizing, and finally drying.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The method of the present invention is suitable for the full recovery of positive electrode materials of waste charged lithium batteries such as waste charged lithium iron phosphate batteries, waste charged lithium cobalt oxide batteries, waste charged lithium manganese oxide batteries, waste charged nickel cobalt manganese oxide batteries, waste charged nickel cobalt aluminum oxide batteries, and waste charged lithium titanate oxide batteries, thereby realizing the full recovery of positive electrode material resources of waste charged lithium batteries, including the recovery of positive electrode powder, the recovery of binder, the recovery of positive electrode current collector, and the recycling of solvent.

[0028] The present invention adopts a solvent to dissolve the binder to separate the positive electrode material from the positive electrode current collector sheet. Compared with the traditional pyrolysis method, it avoids pollutants such as hydrogen fluoride generated by the pyrolysis of the binder during the pyrolysis process, greatly reduces the cost of subsequent tail gas treatment, and is more environmentally friendly and safe; and can maintain the molecular structure of the binder, providing a prerequisite for the subsequent recovery of the binder.

[0029] Compared with the traditional friction powder removal process, the present invention greatly reduces the content of binder and positive electrode current collector in the recovered positive electrode powder, making the recovered positive electrode powder easier to repair.

[0030] The positive electrode powder recovered by the present invention can be used as a positive electrode material for lithium batteries after lithium supplementation and repair. Compared with the traditional positive electrode active material regeneration technology of leaching and extracting lithium, the whole process reduces the use of leaching additives such as acids, alkalis, active substances and oxidants, greatly reduces costs and shortens the time required for the entire process.

[0031] The positive electrode current collector sheets recovered by the present invention can be used as building materials, packaging materials, transportation parts, etc., and can also be used as positive electrode current collectors again after a refining process; the positive electrode binder recovered by the present invention can be used as wires and cables, filter materials, building materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a flow chart of a method for fully recycling positive electrode materials of waste batteries disclosed in the present invention;

[0033] Figure 2 This is a physical picture of the recycled positive electrode current collector obtained by the present invention. DETAILED DESCRIPTION

[0034] The accompanying drawings are only for illustrative purposes; in order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0035] Example 1

[0036] like Figure 1 As shown, a method for fully recycling positive electrode materials of waste batteries comprises the following steps:

[0037] (1) dismantling the waste charged lithium iron phosphate square soft-pack battery to obtain the waste charged lithium battery positive electrode material;

[0038] (2) The waste charged lithium battery positive electrode material obtained in step (1) is immersed in a 1:1:1 mixture of N-methylpyrrolidone, trichloroethylene and dimethyl sulfoxide, and subjected to ultrasonic treatment for 3 hours at a temperature of 30° C. to obtain a mixture I; the components of the mixture I are a positive electrode current collector, a positive electrode powder, a positive electrode binder and a mixed solvent.

[0039] (3) The mixture I obtained in step (2) was filtered through a filter screen with a pore size of 40 to obtain a mixture II (mixture II is a positive electrode powder, a positive electrode binder and a mixed solvent). The material on the filter screen was dried at 150° C. for 5 h to obtain a positive electrode current collector sheet. Figure 2 As shown;

[0040] (4) The above mixture II is filtered through a filter with a pore size of 0.25 μm to obtain mixture III (mixture III is a positive electrode binder and a mixed solvent). The material on the filter is dried at 150°C for 5 hours, with a ball-to-material ratio of 30:1, and ball-milled for 1 hour to obtain positive electrode powder (actual image omitted).

[0041] (5) The mixture III was distilled at 210°C under normal pressure, and the residue was filtered hot (170°C, 0.2 μm filter), cooled to room temperature for recrystallization, filtered, dried at 160°C for 24 hours, and cooled to room temperature to obtain a positive electrode binder (actual image omitted).

[0042] Example 2

[0043] A method for fully recycling positive electrode materials of waste batteries, which is different from Example 1 in that:

[0044] The 1:1:1 ratio of N-methylpyrrolidone, trichloroethylene and dimethyl sulfoxide in step (2) is replaced with 1:1:1 ratio of N-methylpyrrolidone, dimethyl sulfoxide and methanol.

[0045] The remaining parts not mentioned are the same as those in Example 1.

[0046] Example 3

[0047] A method for fully recycling positive electrode materials of waste batteries, which is different from Example 1 in that:

[0048] The 1:1:1 ratio of N-methylpyrrolidone, trichloroethylene and dimethyl sulfoxide in step (2) is replaced with 1:1:1 ratio of N-methylpyrrolidone, trichloroethylene and methanol.

[0049] The remaining parts not mentioned are the same as those in Example 1.

[0050] Example 4

[0051] A method for fully recycling positive electrode materials of waste batteries, which is different from Example 1 in that:

[0052] The ultrasonic treatment for 3 h at a temperature of 30° C. in step (2) was replaced by heating to 100° C. with stirring at a speed of 800 rpm for 24 h.

[0053] The remaining parts not mentioned are the same as those in Example 1.

[0054] Example 5

[0055] A method for fully recycling positive electrode materials of waste batteries, which is different from Example 1 in that:

[0056] The lithium iron phosphate square soft-pack battery with a charge of 3.6V in step (1) is replaced with a ternary lithium blade battery with a charge of 3.9V.

[0057] The remaining parts not mentioned are the same as those in Example 1.

[0058] Comparative Example 1

[0059] The traditional pyrolysis process is used to recycle the positive electrode materials of waste charged lithium batteries. The specific steps are as follows: dismantle the waste charged lithium batteries with electricity to obtain the positive electrode materials of waste charged lithium batteries; place the above-mentioned positive electrode materials of waste charged lithium batteries in a nitrogen-protected tubular furnace at 550°C for 5 hours, ball mill for 1 hour, with a ball-to-material ratio of 30:1, and sieve the sieve after grinding. The mesh number of the sieve used for screening is 120 meshes, and the recovered positive electrode powder and the recovered positive electrode current collector are obtained.

[0060] Comparative Example 2

[0061] The conventional friction powder removal process is used to recycle the positive electrode material of the waste charged lithium battery. The difference from Comparative Example 1 is that the operation of calcining at 550° C. for 5 h in a nitrogen-protected tubular furnace is removed.

[0062] Table 1 Comparison of the recovery effect of waste charged lithium battery positive electrode materials between Examples 1-5 and Comparative Examples 1-2

[0063] Positive electrode powder recovery rate Aluminum content in positive electrode powder Binder recovery rate Positive current collector recovery rate Implementation Case 1 99.1% 0.02% 93.0% 98.1% Implementation Case 2 98.9% 0.05% 92.3% 97.8% Implementation Case 3 98.0% 0.04% 91.9% 98.6% Implementation Case 4 98.4% 0.03% 88.3% 98.3% Implementation Case 5 98.7% 0.03% 91.6% 98.2% Comparative Example 1 97.2% 1.8% 0 98.9% Comparative Example 2 95.6% 2.5% 0 98.6%

[0064] From the comparison of the recovery effects of waste charged lithium battery positive electrode materials of Examples 1-5 and Comparative Examples 1-2 in Table 1, it can be seen that the method for fully recovering waste battery positive electrode materials of the present invention can achieve high-efficiency recovery of positive electrode powder, binder and positive electrode current collector, while the conventional pyrolysis process and the conventional friction de-powdering process cannot recover the binder; and the content of metal impurities such as aluminum in the positive electrode powder recovered by the present invention is much lower than the positive electrode powder recovered by the conventional pyrolysis process and the conventional friction de-powdering process, thereby improving the quality and value of the recovered positive electrode powder.

[0065] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for fully recycling positive electrode materials of waste batteries, characterized in that: The method comprises the following steps: (1) Dismantling the waste charged lithium battery by charged crushing to obtain the waste charged lithium battery positive electrode material; (2) treating the waste charged lithium battery positive electrode material obtained in step (1) with a solvent to dissolve the binder and separate the positive electrode powder from the positive electrode current collector sheet to obtain a mixture I; (3) filtering the mixture I obtained in step (2) through a large-pore filter to obtain a mixture II, and drying the material on the filter to obtain a positive electrode current collector sheet; (4) filtering the mixture II obtained in step (3) through a small-pore filter to obtain a mixture III, and drying and grinding the material on the filter to obtain a positive electrode powder; (5) The mixture III obtained in step (4) is distilled to recover the mixed solvent, and the residue is purified to obtain a positive electrode binder.

2. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (2), the solvent is at least one of dichloroethylene, trichloroethylene, dichloromethane, chloroform, dichloroethane, N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, methanol, ethanol, propanol, isopropanol, acetonitrile, ether, anisole, diethylene glycol dimethyl ether, acetone, tetrahydrofuran, and water.

3. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (2), the mass ratio of the solvent to the positive electrode material of the waste charged lithium battery is 2 to 8:

1.

4. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (2), the treatment refers to at least one of immersion, standing, stirring, ultrasound, oscillation, hydrothermal, and solvent thermal, with a treatment temperature of 30 to 130° C. and a treatment time of 1 to 5 hours.

5. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (3), the pore size of the large-pore filter screen is 40 to 250 meshes.

6. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (4), the pore size of the small-pore filter is 0.2 to 10 microns.

7. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (4), the drying temperature is 120 to 150° C. and the drying time is 2 to 5 hours.

8. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (4), grinding is performed by ball milling or rod milling, and the rod / ball material ratio is 15 to 30:

1.

9. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (5), the distillation is one of atmospheric distillation and reduced pressure distillation, the distillation temperature is 90 to 210° C., and the pressure is 0.15 to 100 kPa.

10. The method for fully recycling positive electrode materials of waste batteries according to claim 1, characterized in that: In the step (5), the refining is at least one of recrystallization, flocculation sedimentation, dissolution, filtration, distillation, decolorization, membrane filtration, centrifugation, and drying.