Preparation method of self-supporting graphene-based electromagnetic shielding heat-conducting composite film

By using dispersant and pH regulation, Hummer's method of ultrasonic dispersion and vacuum suction filtration, hydroiodonic acid steam reduction and microwave sintering in graphene-based electromagnetic shielding materials, a self-supported graphene-based electromagnetic shielding thermal composite film is formed, and the solution is to solve the problem of The problems of complex process and low mechanical properties in the prior art are achieved, and the possibility of high performance and large-scale production is achieved.

CN119095362APending Publication Date: 2024-12-06QITAIHE BAOTAILONG GRAPHENE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411237507.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, when preparing graphene and silicon carbide composite electromagnetic shielding materials, the process is complex and the mechanical properties are low, making it difficult to achieve large-size and large-scale production. In addition, the simple graphene powder has poor dispersion and low structural strength, making it difficult to adapt to complex environments. Application requirements.

Method used

The uniform dispersion of carbon nanotubes and silicon carbide whiskers was prepared by dispersant and pH control method, and the ultrasonic dispersion of graphene oxide was prepared by Hummer's method. The self-support was formed by vacuum suction filtration, steam reduction of hydroiodic acid and microwave sintering. The graphene-based electromagnetic shielding thermally conductive composite film, carbon nanotubes and silicon carbide are uniformly laid between the graphene oxide sheet layers to form a three-dimensional foam structure.

Benefits of technology

It realizes the preparation of a high-performance graphene-based electromagnetic shielding thermally conductive composite film with simple operation and low cost, improves mechanical properties and comprehensive performance, and is suitable for applications in multiple fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095362A_ABST
    Figure CN119095362A_ABST
Patent Text Reader

Abstract

A preparation method of a self-supporting graphene-based electromagnetic shielding heat-conducting composite film relates to the technical field of new materials, and comprises the following steps: firstly, preparing graphene oxide with different oxidation degrees by adopting an improved Hummer's method; ultrasonically mixing the graphene oxide with uniformly dispersed carbon nanotubes and silicon carbide whiskers, regulating and controlling the pH value of a system and the addition amount of a dispersing agent, uniformly laying the carbon nanotubes and the silicon carbide whiskers between graphene oxide sheet layers through a vacuum filtration method, cleaning the obtained filter membrane, and performing vacuum pressing and drying; reducing the dried filter membrane in hydriodic acid steam, washing with water, washing with absolute ethyl alcohol, and drying at room temperature to obtain a reduced filter membrane; and finally, carrying out microwave sintering on the reduced film to obtain the self-supporting graphene-based electromagnetic shielding heat-conducting composite film. The method has the advantages that the preparation process is simple and easy to control, and raw materials are low in cost, easy to obtain and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention relates to the technical field of new materials, and in particular to a method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film. Background technology:

[0002] With the rapid development of electronic information technology, electromagnetic pollution has become the fifth largest source of pollution that threatens human survival after air pollution, water pollution, soil pollution and noise pollution. Therefore, it is urgent to develop light, wide-band, high-performance electromagnetic shielding materials to meet the development needs of intelligent electronic equipment. The carbon atoms in the graphene carbon layer are sp2 hybridized, and the delocalized large π bonds are vertically distributed on the carbon hexagonal ring. This special structure increases the absorption loss of graphene to electromagnetic waves (EMW); the functional groups and defects in graphene materials can aggravate the polarization loss of EMW; the lone pairs of electrons distributed at the edges and defects of graphene can introduce local magnetic moments, increase the magnetic loss to EMW, and increase the eddy current effect. At the same time, graphene has the advantages of light weight, high electrical conductivity, thermal conductivity, large dielectric constant and high specific surface area. Compared with traditional electromagnetic shielding materials, it is easier to meet the requirements of "light, thin, strong and wide" required by electromagnetic shielding materials, and has great potential in the design and development of high-performance electromagnetic shielding materials.

[0003] However, due to the poor dispersibility, low structural strength and low magnetic permeability of pure graphene powder, there is a serious impedance mismatch between graphene and the EMW of free space, which makes it difficult to adapt to the application requirements of complex environments. Graphene needs to be structured and composited to avoid the intrinsic defects of graphene materials, while maintaining the excellent physical and chemical properties of graphene and giving graphene three-dimensional structural properties. Silicon carbide, as a typical covalently bonded inorganic compound, has a series of advantages such as good stability, thermal shock resistance, friction and wear resistance, and integrates thermal protection, oxidation resistance, and structural load-bearing. In addition, silicon carbide is a wide bandgap semiconductor.

[0004] The saturated electron mobility is high and it has good wave absorption performance. The composite of graphene and SiC with different conductivity and dielectric constant can cause the interface charge aggregation and polarization between them on the one hand, and on the other hand, the formed heterogeneous interface can block or change the extension direction of the crack when loading, which is beneficial to enhance the anti-destruction ability of the composite material. In addition, the interface between graphene and SiC is easy to form Si-C covalent bonds, which helps to connect the graphene sheets tightly and prevent the sliding of the graphene sheets. The composite of graphene and SiC, giving play to the synergistic effect of the two, has been proven to be a promising electromagnetic shielding material, especially in applications under extreme conditions.

[0005] The current method for controlling the composite of graphene and SiC is to in situ grow SiC nanowires or nanofibers in three-dimensional graphene foam by impregnation pyrolysis, electrophoretic deposition, chemical vapor infiltration (CVI) or chemical vapor deposition (CVD) to prepare SiC / graphene composite electromagnetic shielding materials. The preparation process is quite complicated and time-consuming, and the composite materials prepared by these methods have low mechanical properties, making it difficult to achieve large-scale and large-scale actual production. Summary of the invention:

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and to provide a method for preparing a self-supporting graphene-based electromagnetic shielding thermal conductive composite film. It is a method for preparing a high-performance self-supporting graphene-based electromagnetic shielding thermal conductive composite film that is simple to operate and suitable for industrial production. The porous foam structure is formed by graphene self-assembly, and carbon nanotubes and silicon carbide whiskers are evenly distributed between graphene sheets. The distribution and loading amount of carbon nanotubes and silicon carbide are controllable.

[0007] In order to solve the problems existing in the background technology, the present invention adopts the following technical solution: The preparation method is as follows:

[0008] 1) Improving the dispersibility of silicon carbide whiskers by dispersant and pH control to obtain uniform silicon carbide whiskers

[0009] Evenly disperse the liquid;

[0010] 2) Improving the dispersibility of carbon nanotubes by dispersant and pH control to obtain a uniform dispersion of carbon nanotubes;

[0011] 3) ultrasonically dispersing the graphene oxide prepared by the improved Hummer's method in deionized water to obtain a uniformly dispersed solution of the graphene oxide;

[0012] 4) adding the dispersion of carbon nanotubes and silicon carbide whiskers to the uniform dispersion of graphene oxide, and dispersing and mixing them uniformly;

[0013] 5) uniformly layering carbon nanotubes and silicon carbide whiskers between graphene oxide sheets by vacuum filtration;

[0014] 6) washing the obtained filter membrane and vacuum pressing and drying;

[0015] 7) reducing the dried filter membrane in hydroiodic acid vapor;

[0016] 8) washing the reduced filter membrane with water and anhydrous ethanol, and drying to obtain the reduced filter membrane;

[0017] 9) Finally, the reduced filter membrane is microwave sintered to obtain a self-supporting graphene-based electromagnetic shielding and thermal conductive composite film.

[0018] The concentration of the uniform dispersion of silicon carbide whiskers in step 1) is 0.5-5 mg / L.

[0019] The concentration of the uniform dispersion of carbon nanotubes in step 2) is 5 to 80 mg / L.

[0020] In the step 3), the ultrasonic dispersion time of graphene oxide is 0.5 to 8 hours, and the concentration of the uniformly dispersed solution of graphene oxide is 1 to 10 mg / mL.

[0021] In the step 4), the mass ratio of the uniform dispersion solution of graphene oxide, the uniform dispersion solution of silicon carbide whiskers and the uniform dispersion solution of carbon nanotubes is 1:0.5-10:0.05-3.

[0022] The drying process in step 6) is vacuum pressing and drying, and the drying pressure is controlled at 0.2-2 MPa.

[0023] The drying temperature is between 30 and 100°C and the drying time is between 2 and 12 hours.

[0024] In the step 7), the filter membrane reduction process is carried out in hydroiodic acid vapor, the heating temperature is controlled at 40-100° C., and the reduction time is 0.5-4 hours.

[0025] In the step 8), the filter membrane is dried in a vacuum drying oven after cleaning, and the drying temperature is controlled between 30 and 100° C. for 2 to 24 hours.

[0026] In the step 9), the filter membrane is sintered in a microwave oven, the heating power is controlled at 500-1000W, and the sintering time is controlled at 2-12min.

[0027] The beneficial effects of the present invention are as follows: the present invention completes the preparation of a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film by a method combining vacuum filtration, steam reduction and microwave sintering. The advantages are that the raw materials are generally available, the cost is low, the preparation process is safe, and it is simple and easy; carbon nanotubes and silicon carbide whiskers use the shape adaptability of their own one-dimensional structure to evenly layer between graphene oxide sheets, and the strong reducing property of hydroiodic acid vapor self-assembles to form a three-dimensional foam graphene matrix. At the same time, the microwave sintering process is adopted, which not only simplifies the process, has a fast heating rate, a high sintering temperature, a short sintering time, energy saving and environmental protection, but also the obtained graphene-based composite film has good mechanical properties. The optimization of the microstructure and mechanical properties of the composite film makes it have good comprehensive performance and potential applications in more fields. Description of the drawings:

[0028] Figure 1 It is a physical diagram of the present invention;

[0029] Figure 2 It is a bending physical diagram of the present invention;

[0030] Figure 3 SEM electron microscope cross-sectional view of embodiment 1 of the present invention;

[0031] Figure 4 SEM electron microscope plan view of Example 1 of the present invention.

[0032] Figure 5 Infrared spectrum of the first embodiment of the present invention;

[0033] manual

[0034] Figure 6 The electromagnetic shielding effectiveness spectrum of the first embodiment of the present invention. Specific implementation method:

[0035] With reference to the figures, the present invention specifically adopts the following implementation mode: The preparation method is as follows:

[0036] 1) Improving the dispersibility of silicon carbide whiskers by dispersant and pH control to obtain a uniform dispersion of silicon carbide whiskers;

[0037] 2) Improving the dispersibility of carbon nanotubes by dispersant and pH control to obtain a uniform dispersion of carbon nanotubes;

[0038] 3) ultrasonically dispersing the graphene oxide prepared by the improved Hummer's method in deionized water to obtain a uniformly dispersed solution of the graphene oxide;

[0039] 4) adding the dispersion of carbon nanotubes and silicon carbide whiskers to the uniform dispersion of graphene oxide, and dispersing and mixing them uniformly;

[0040] 5) uniformly layering carbon nanotubes and silicon carbide whiskers between graphene oxide sheets by vacuum filtration;

[0041] 6) washing the obtained filter membrane and vacuum pressing and drying;

[0042] 7) reducing the dried filter membrane in hydroiodic acid vapor;

[0043] 8) washing the reduced filter membrane with water and anhydrous ethanol, and drying to obtain the reduced filter membrane;

[0044] 9) Finally, the reduced filter membrane is microwave sintered to obtain a self-supporting graphene-based electromagnetic shielding and thermal conductive composite film.

[0045] The concentration of the uniform dispersion of silicon carbide whiskers in step 1) is 0.5-5 mg / L. The concentration of the uniform dispersion of carbon nanotubes in step 2) is 5-80 mg / L. The ultrasonic dispersion time of graphene oxide in step 3) is 0.5-8 hours, and the concentration of the uniform dispersion of graphene oxide is 1-10 mg / mL.

[0046] In step 4) described in the specification, the mass ratio of the uniform dispersion solution of graphene oxide, the uniform dispersion solution of silicon carbide whiskers and the uniform dispersion solution of carbon nanotubes is 1:0.5-10:0.05-3. In step 6), the drying process is vacuum pressing drying, the drying pressure is controlled between 0.2 and 2 MPa, the drying temperature is 30-100°C, and the drying time is 2-12 hours. In step 7), the filter membrane reduction process is reduced in hydroiodic acid vapor, the heating temperature is controlled at 40-100°C, and the reduction time is 0.5-4 hours. In step 8), the filter membrane drying process after washing is dried in a vacuum drying oven, the drying temperature is controlled between 30-100°C, and the time is 2-24 hours. In step 9), the filter membrane sintering process is sintered in a microwave oven, the heating power is controlled at 500-1000W, and the sintering time is controlled at 2-12 minutes.

[0047] The specific preparation method according to the above steps is as follows:

[0048] 1) utilizing the electrostatic repulsion of carboxymethyl cellulose anions, a certain amount of silicon carbide whiskers are uniformly dispersed in deionized water to obtain a uniform dispersion of silicon carbide whiskers, and the concentration of the dispersion is controlled;

[0049] 2) utilizing the electrostatic repulsion of sodium dodecylbenzene sulfonate anions, uniformly dispersing a certain amount of carbon nanotubes (CNTs) in deionized water to obtain a uniform dispersion of carbon nanotubes (CNTs), and controlling the concentration of the dispersion;

[0050] 3) using ultrasonic waves to open the π bonds between graphene oxide sheets, uniformly dispersing a certain amount of graphene oxide in deionized water to obtain a graphene oxide dispersion solution, and controlling the ultrasonic time and the concentration of the dispersion solution;

[0051] 4) adding a certain amount of uniform dispersion of silicon carbide whiskers to the graphene oxide dispersion solution and mixing them uniformly to obtain a mixed solution 1, and controlling the concentration ratio of the mixed solution;

[0052] 5) Add a certain amount of uniform dispersion of carbon nanotubes (CNT) to the mixed solution 1, mix them evenly, obtain a mixed solution 2, and perform ultrasonic dispersion for a certain time to control the mass ratio of the mixed solution and the supersonic dispersion.

[0053] Sound dispersion time;

[0054] 6) using a vacuum filtration method to evenly layer the uniformly dispersed mixed solution 2 between graphene oxide sheets using the shape adaptability of their own one-dimensional structures, thereby obtaining a carbon nanotube (CNT) / silicon carbide whisker / graphene oxide composite filter membrane 1;

[0055] 7) vacuum drying the obtained carbon nanotube (CNT) / silicon carbide whisker / graphene oxide composite filter membrane, and controlling the pressure, temperature and time of the composite film drying process;

[0056] 8) reducing the vacuum-pressed dried carbon nanotube (CNT) / silicon carbide whisker / graphene oxide composite filter membrane 1 in hydroiodic acid vapor to obtain a carbon nanotube (CNT) / silicon carbide whisker / graphene oxide composite filter membrane 2, and controlling the heating temperature and time of the hydroiodic acid solution during the hydroiodic acid reduction process;

[0057] 9) washing the carbon nanotube (CNT) / silicon carbide whisker / graphene oxide composite filter membrane 2 and vacuum drying the filter membrane, and controlling the drying temperature and time during the drying process;

[0058] 10) Finally, the dried carbon nanotube (CNT) / silicon carbide whisker / graphene oxide composite filter membrane 2 is subjected to microwave sintering to obtain a self-supporting graphene-based electromagnetic shielding thermal conductive composite film, and the microwave heating power and time are controlled during the microwave sintering process.

[0059] Embodiment 1

[0060] First, 2 mg of SiC whiskers are uniformly dispersed in 1 L of deionized water solution of sodium carboxymethyl cellulose to obtain a uniform dispersion of SiC whiskers; 10 mg of carbon nanotubes (CNTs) are uniformly dispersed in 1 L of deionized water of sodium dodecylbenzene sulfonate to obtain a uniform dispersion of CNTs; 0.3 g of graphene oxide is ultrasonically dispersed in 100 mL of deionized water for 4 h to obtain a 3 mg / mL graphene oxide dispersion solution; 15 mL of the uniform dispersion of SiC whiskers is added to the graphene oxide dispersion solution and mixed uniformly to obtain a mixed solution 1; 5 mL of the uniform dispersion of CNT is added to the mixed solution 1 to mix uniformly to obtain a mixed solution 2, and ultrasonic dispersion is performed for 1 h; the uniformly dispersed mixed solution 2 is subjected to vacuum filtration to obtain a CNT / SiC / graphene oxide composite filter membrane 1; The obtained CNT / SiC / graphene oxide composite filter membrane 1 is vacuum-pressurized and dried, and the pressure of the composite film drying process is controlled at 0.5MPa, the drying temperature is controlled at 30°C, and the drying time is 15h; the CNT / SiC / graphene oxide composite filter membrane 1 after vacuum-pressurized drying is reduced in hydroiodic acid vapor to obtain CNT / SiC / graphene composite film 2, and the hydroiodic acid reduction process controls the heating temperature of the hydroiodic acid solution to 70°C, and the reduction time is 2h; the CNT / SiC / graphene composite film 2 is cleaned and vacuum-dried, and the drying process controls the drying temperature to 60°C, and the drying time is 12h; finally, the dried CNT / SiC / graphene composite film 2 is microwave-sintered to obtain a self-supporting graphene-based electromagnetic shielding thermal conductive composite film, and the microwave heating power is controlled at 800W and the heating time is 7min during the microwave sintering process.

[0061] Reference Figure 1-3 , it can be seen that graphene is in the form of a three-dimensional foam, and SiC whiskers and CNTs are arranged in a uniform array between the foam layers, forming a multi-level pore structure. Figure 4 , it can be seen that the multi-interface hybrid structure composed of alternating CNTs and SiC whiskers is beneficial to inducing interface loss and EMW absorption. Figure 5 The infrared spectra of graphene oxide, CNT / SiC / graphene composite film reduced by hydroiodic acid (S2) and CNT / SiC / graphene composite film after microwave sintering (S3) are shown. In the infrared spectrum of graphene oxide, the absorption vibration peak of COC bond at about 850cm-1, the absorption vibration peak of C=O bond at about 1800cm-1, and the absorption vibration peak of -COOH at about 1260cm-1. After hydroiodic acid reduction, the vibration peaks of -COOH and C=O functional groups in the sample have gradually disappeared, indicating that hydroiodic acid can effectively reduce the carboxyl functional groups in graphene oxide. After microwave sintering, the vibration peaks of oxygen-containing functional groups in graphene oxide are further weakened. Figure 6The results of the electromagnetic shielding effectiveness test of the self-supporting graphene-based composite film in the X-band. The test frequency is 8.2GHz~12.4GHz, and the test sample size is 22.86mm×10.16mm×2mm. As can be seen from the figure, the average value of electromagnetic shielding effectiveness (SET) reaches

[0062] The average thermal diffusion coefficient reaches 524.982.

[0063] Embodiment 2

[0064] First, 4 mg of SiC whiskers were uniformly dispersed in 1 L of deionized water solution of sodium carboxymethyl cellulose to obtain a uniform dispersion of SiC whiskers; 6 mg of carbon nanotubes (CNTs) were uniformly dispersed in 1 L of deionized water of sodium dodecylbenzene sulfonate to obtain a uniform dispersion of CNTs; 0.5 g of graphene oxide was ultrasonically dispersed in 100 mL of deionized water for 6 h to obtain a 5 mg / mL graphene oxide dispersion solution; 18 mL of the uniform dispersion of SiC whiskers was added to the graphene oxide dispersion solution and mixed evenly to obtain a mixed solution 1; 4 mL of the uniform dispersion of CNT was added to the mixed solution 1 to mix evenly to obtain a mixed solution 2, and ultrasonic dispersion was performed for 3 h; the uniformly dispersed mixed solution 2 was subjected to vacuum filtration to obtain a CNT / SiC / graphene oxide composite filter membrane 1; the obtained The first CNT / SiC / graphene oxide composite filter membrane is vacuum-pressed and dried, and the pressure of the composite film drying process is controlled at 0.8MPa, the drying temperature is controlled at 50°C, and the drying time is 10h; the first CNT / SiC / graphene oxide composite filter membrane after vacuum-pressurized drying is reduced in hydroiodic acid vapor to obtain a second CNT / SiC / graphene composite film, and the hydroiodic acid reduction process controls the heating temperature of the hydroiodic acid solution to 80°C, and the reduction time is 4h; the second CNT / SiC / graphene composite film is cleaned and vacuum-dried, and the drying process controls the drying temperature to 70°C, and the drying time is 5h; finally, the dried CNT / SiC / graphene composite film is microwave-sintered to obtain a self-supporting graphene-based electromagnetic shielding thermal conductive composite film, and the microwave heating power is controlled at 1000W and the heating time is 5min during the microwave sintering process.

[0065] Embodiment 3

[0066] First, 3 mg of SiC whiskers were uniformly dispersed in 1 L of deionized water solution of sodium carboxymethyl cellulose to obtain a uniform dispersion of SiC whiskers; 15 mg of carbon nanotubes (CNTs) were uniformly dispersed in 1 L of deionized water solution of sodium dodecylbenzene sulfonate to obtain a uniform dispersion of CNTs; 1.0 g of graphite oxide was uniformly dispersed in 1 L of deionized water solution of sodium dodecylbenzene sulfonate to obtain a uniform dispersion of CNTs;

[0067] The graphene oxide was ultrasonically dispersed in 100 mL of deionized water for 8 h to obtain a 10 mg / mL graphene oxide dispersion solution; 20 mL of SiC whisker dispersion was added to the graphene oxide dispersion solution and mixed evenly to obtain a mixed solution 1; 7 mL of CNT dispersion was added to the mixed solution 1 to mix evenly to obtain a mixed solution 2, which was ultrasonically dispersed for 4 h; the uniformly dispersed mixed solution 2 was vacuum filtered to obtain a CNT / SiC / graphene oxide composite filter membrane 1; the CNT / SiC / graphene oxide composite filter membrane 1 was vacuum-pressed and dried, and the pressure of the composite film drying process was controlled at 1.0 MPa and the drying temperature was controlled at 40 ℃, and the drying time is 10h; the CNT / SiC / graphene oxide composite filter membrane 1 after vacuum pressure drying is reduced in hydroiodic acid vapor to obtain CNT / SiC / graphene composite film 2, and the hydroiodic acid reduction process controls the heating temperature of the hydroiodic acid solution to 90℃, and the reduction time is 1h; the CNT / SiC / graphene composite film 2 is cleaned and vacuum dried, and the drying process controls the drying temperature to 40℃, and the drying time is 20h; finally, the dried CNT / SiC / graphene composite film 2 is subjected to microwave sintering to obtain a self-supporting graphene-based electromagnetic shielding thermal conductive composite film, and the microwave heating power is controlled at 700W and the heating time is 15min during the microwave sintering process.

[0068] In summary, the preparation method of the self-supporting graphene-based electromagnetic shielding thermal conductive composite film is completed by combining vacuum filtration, steam reduction and microwave sintering. Its advantages are that the raw materials are generally easy to obtain, the cost is low, the preparation process is safe, and it is simple and easy; carbon nanotubes and silicon carbide whiskers use the shape adaptability of their own one-dimensional structure to evenly layer between the graphene oxide sheets, and the strong reducing property of hydroiodic acid vapor self-assembles to form a three-dimensional foam graphene matrix. At the same time, the microwave sintering process is adopted, which not only simplifies the process, has a fast heating rate, a high sintering temperature, a short sintering time, energy saving and environmental protection, but also the obtained graphene-based composite film has good mechanical properties. The optimization of the microstructure and mechanical properties of the composite film makes it have good comprehensive performance and potential applications in more fields.

Claims

1. A method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film, characterized in that: The preparation method is as follows: 1) Improving the dispersibility of silicon carbide whiskers by dispersant and pH control to obtain a uniform dispersion of silicon carbide whiskers; 2) Improving the dispersibility of carbon nanotubes by dispersant and pH control to obtain a uniform dispersion of carbon nanotubes; 3) ultrasonically dispersing the graphene oxide prepared by the improved Hummer's method in deionized water to obtain a uniformly dispersed solution of the graphene oxide; 4) adding the dispersion of carbon nanotubes and silicon carbide whiskers to the uniform dispersion of graphene oxide, and dispersing and mixing them uniformly; 5) uniformly layering carbon nanotubes and silicon carbide whiskers between graphene oxide sheets by vacuum filtration; 6) washing the obtained filter membrane and vacuum pressing and drying; 7) reducing the dried filter membrane in hydroiodic acid vapor; 8) washing the reduced filter membrane with water and anhydrous ethanol, and drying to obtain the reduced filter membrane; 9) Finally, the reduced filter membrane is microwave sintered to obtain a self-supporting graphene-based electromagnetic shielding and thermal conductive composite film.

2. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: The concentration of the uniform dispersion of silicon carbide whiskers in step 1) is 0.5-5 mg / L.

3. Claims of a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1 The preparation method is characterized by: The concentration of the uniform dispersion of carbon nanotubes in step 2) is 5 to 80 mg / L.

4. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: In the step 3), the ultrasonic dispersion time of graphene oxide is 0.5 to 8 hours, and the concentration of the uniformly dispersed solution of graphene oxide is 1 to 10 mg / mL.

5. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: In the step 4), the mass ratio of the uniform dispersion solution of graphene oxide, the uniform dispersion solution of silicon carbide whiskers and the uniform dispersion solution of carbon nanotubes is 1:0.5-10:0.05-3.

6. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: The drying process in step 6) is vacuum pressing drying, the drying pressure is controlled between 0.2 and 2 MPa, the drying temperature is between 30 and 100° C., and the drying time is between 2 and 12 hours.

7. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: In the step 7), the filter membrane reduction process is carried out in hydroiodic acid vapor, the heating temperature is controlled at 40-100° C., and the reduction time is 0.5-4 hours.

8. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: In the step 8), the filter membrane is dried in a vacuum drying oven after cleaning, and the drying temperature is controlled between 30 and 100° C. for 2 to 24 hours.

9. The method for preparing a self-supporting graphene-based electromagnetic shielding and thermally conductive composite film according to claim 1, characterized in that: In the step 9), the filter membrane is sintered in a microwave oven, the heating power is controlled at 500-1000W, and the sintering time is controlled at 2-12min.