Perovskite solar cell and preparation method thereof
By preparing an interface modification layer containing 1-ethyl-3-methylhexafluorophosphate on the surface of the nickel oxide layer in a perovskite solar cell, the problems of interface defects and non-radiative recombination in perovskite solar cells are solved. It improves the photoelectric conversion efficiency and stability, reduces costs, and is suitable for commercial applications.
Patent Information
- Application Number
- CN202411193629.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
In existing perovskite solar cells, there are defects in the interface between nickel oxide and perovskite layer and non-radiative recombination, resulting in low device stability and photoelectric conversion efficiency. The existing modification methods are costly or complex in processes, making it difficult to achieve uniformity. distributed.
The interface modification layer was prepared on the surface of the nickel oxide layer, using a self-assembled monolayer consisting of carbazole core and phosphonic acid, and 1-ethyl-3-methylhexafluorophosphate was added therein to form a uniformly distributed interface modification. The layer fills the vacancy defects of the perovskite layer, inhibits non-radiative recombination, and forms a carrier transport channel.
It realizes effective passivation of interface defects and accelerates carrier transmission, improves the photoelectric conversion efficiency and stability of perovskite solar cells, reduces material costs, simplifies the preparation process, and is suitable for commercial applications.
Smart Images

Figure CN119095401A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a perovskite solar cell and a perovskite solar cell. Background Art
[0002] Nickel Oxide (NiO X ) belongs to transition metal oxides and is an inorganic p-type semiconductor. Due to its cost-effectiveness, stability and scalability, it can be used as the hole transport layer (HTL) of inverted and tandem perovskite solar cells (PSCs). Oxygen vacancies and NiO X The presence of uncoordinated metal ion defects on the surface is the key to improving PCE. In addition, there are submicron-scale defects on the lower surface of the perovskite material. X The interaction with the perovskite film can also lead to interfacial reactions, resulting in non-radiative recombination at the interface. These phenomena can adversely affect the stability of the device and cause the loss of voltage open circuit (VOC), which poses a major obstacle to the realization of efficient and highly stable inverted PSCs. Therefore, solving these problems is crucial to improving the performance of inverted PSCs.
[0003] In order to solve the NiO X Interface problems with perovskite. In the prior art, the commonly used modified NiO X One way is to use NiO X The surface is prepared with an interface modification layer, such as a self-assembled monolayer (SAMs) composed of carbazole cores and phosphonic acid to achieve the effect of defect passivation. Another way is to add some organic molecules to the perovskite precursor. These additives will react with NiO X However, for the first method, the steric hindrance of carbazole in the SAM material will limit the formation of a dense monolayer on the substrate, thereby hindering the effective passivation of the bottom defects of the perovskite film. For the second method, the concentration of the additive added to the perovskite is difficult to control, so the interface effect is not ideal.
[0004] In order to solve the above-mentioned problems existing in the prior art, the art is in urgent need of an improved preparation technology for perovskite solar cells, which can reduce material costs, facilitate commercialization, and has a simple preparation process. It can not only achieve uniform distribution of the interface modification layer to modify and passivate the defects at the interface between the nickel oxide layer and the perovskite layer, but also fill the vacancy defects of organic cations and halogens at the bottom of the perovskite layer to synergistically solve the buried defect problem, inhibit non-radiative recombination at the interface, and enhance the passivation effect. At the same time, it can also form a carrier transport channel at the interface, accelerate carrier transport, and improve the photoelectric conversion efficiency of the device. Summary of the invention
[0005] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or decisive elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.
[0006] In order to overcome the above-mentioned defects of the prior art, the present invention provides a method for preparing a perovskite solar cell, and a perovskite solar cell, which can reduce material costs and be conducive to commercialization, and the preparation process is simple. Not only can the interface modification layer be evenly distributed to modify and passivate the defects at the interface between the nickel oxide layer and the perovskite layer, but the vacancy defects of the organic cations and halogens at the bottom of the perovskite layer can also be filled to synergistically solve the buried defect problem, inhibit non-radiative recombination at the interface, and enhance the passivation effect. At the same time, a carrier transmission channel can be formed at the interface, thereby accelerating carrier transmission and improving the photoelectric conversion efficiency of the device.
[0007] Specifically, the method for preparing a perovskite solar cell provided in accordance with the first aspect of the present invention comprises: preparing a hole transport layer on a substrate, wherein the hole transport layer comprises nickel oxide; preparing an interface modification layer on the surface of the hole transport layer, wherein 1-ethyl-3-methyl hexafluorophosphate is added to the interface modification layer; preparing a perovskite light absorption layer on the interface modification layer; preparing an electron transport layer on the perovskite light absorption layer; and preparing a metal electrode on the electron transport layer.
[0008] Furthermore, in some embodiments of the present invention, the step of preparing an interface modification layer on the hole transport layer includes: obtaining a material of a self-assembled monolayer composed of a carbazole core and a phosphonic acid, and dissolving it in a solvent of the interface modification layer to obtain a solution of the self-assembled monolayer, wherein the concentration range of the self-assembled monolayer is 0.5 to 1 mg / ml; adding the 1-ethyl-3-methyl hexafluorophosphate to the solution of the self-assembled monolayer to form a precursor of the interface modification layer, wherein the concentration range of the 1-ethyl-3-methyl hexafluorophosphate is 1 to 2 mg / ml; and spin coating the precursor of the interface modification layer on the surface of the hole transport layer to form the interface modification layer.
[0009] Furthermore, in some embodiments of the present invention, the solvent of the interface modification layer includes any one of ethanol and isopropanol, or a mixed solvent of the two.
[0010] Furthermore, in some embodiments of the present invention, the step of obtaining a self-assembled monolayer material composed of a carbazole core and a phosphonic acid and dissolving it to form a self-assembled monolayer solution includes: obtaining [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid and dissolving it in an ethanol solution to obtain the self-assembled monolayer solution.
[0011] Furthermore, in some embodiments of the present invention, the step of spin coating the precursor of the interface modification layer on the surface of the substrate to form the interface modification layer includes: depositing a thin film of the precursor of the interface modification layer on the surface of the hole transport layer by a one-step spin coating method.
[0012] Furthermore, in some embodiments of the present invention, the substrate comprises any one of glass made of fluorine-doped tin oxide, glass made of indium tin oxide, and a conductive substrate of flexible indium tin oxide. Before the step of preparing the hole transport layer on the substrate, the step further comprises: cleaning the substrate; and ozone treating the cleaned substrate.
[0013] Furthermore, in some embodiments of the present invention, the step of preparing a perovskite light-absorbing layer on the interface modification layer includes: obtaining a perovskite solution, dissolving it in an organic solvent of perovskite, and obtaining a perovskite precursor; spin-coating the perovskite precursor on the surface of the interface modification layer to deposit a perovskite film; and heating and annealing to obtain the perovskite light-absorbing layer.
[0014] Furthermore, in some embodiments of the present invention, the components of the perovskite include any one of FAMAPbI, FACsPbI, and FAMACsPbI, and the organic solvent of the perovskite includes a mixture of dimethylformamide and dimethyl sulfoxide, or a mixture of γ-butyrolactone and N-methylpyrrolidone, wherein the volume ratio of dimethylformamide to dimethyl sulfoxide, and γ-butyrolactone to N-methylpyrrolidone is in the range of 3-5:1.
[0015] Furthermore, in some embodiments of the present invention, after the step of preparing an electron transport layer on the perovskite light absorbing layer, it also includes: preparing a hole blocking layer on the surface of the electron transport layer, wherein the material of the hole blocking layer includes 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline.
[0016] In addition, the above-mentioned perovskite solar cell provided according to the second aspect of the present invention includes: a substrate, a hole transport layer, an interface modification layer, a perovskite light absorption layer, an electron transport layer, and a metal electrode stacked in sequence, wherein the interface modification layer located between the hole transport layer and the perovskite light absorption layer includes 1-ethyl-3-methyl hexafluorophosphate. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The above features and advantages of the present invention can be better understood after reading the detailed description of the embodiments of the present disclosure in conjunction with the following drawings. In the drawings, the components are not necessarily drawn to scale, and components with similar related properties or features may have the same or similar reference numerals.
[0018] Figure 1 A schematic structural diagram of a perovskite solar cell provided according to some embodiments of the present invention is shown;
[0019] Figure 2 A flow chart showing a method for preparing a perovskite solar cell according to some embodiments of the present invention; and
[0020] Figure 3 A flow chart of preparing an interface modification layer on a hole transport layer according to some embodiments of the present invention is shown.
[0021] Reference numerals:
[0022] 100 Perovskite Solar Cells;
[0023] 110 substrate;
[0024] 120 hole transport layer;
[0025] 130 interface modification layer;
[0026] 140 Perovskite light absorbing layer;
[0027] 150 Electron transport layer;
[0028] 151 hole blocking layer;
[0029] 160 Metal electrodes;
[0030] Steps S210 to S250; and
[0031] Steps S221~S223. DETAILED DESCRIPTION
[0032] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description.
[0033] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0034] In addition, the terms "upper", "lower", "left", "right", "top", "bottom", "horizontal" and "vertical" used in the following description should be understood as the directions shown in the paragraph and the related drawings. Such relative terms are only used for the convenience of description and do not mean that the device described therein must be manufactured or operated in a specific direction, and therefore should not be understood as limiting the present invention.
[0035] It is understood that although the terms "first", "second", "third", etc. may be used herein to describe various components, regions, layers and / or parts, these components, regions, layers and / or parts should not be limited by these terms, and these terms are only used to distinguish different components, regions, layers and / or parts. Therefore, the first component, region, layer and / or part discussed below may be referred to as a second component, region, layer and / or part without departing from some embodiments of the present invention.
[0036] As mentioned above, in the prior art, the commonly used modified NiO X One way is to use NiO X The surface is prepared with an interface modification layer, such as a self-assembled monolayer (SAMs) composed of carbazole cores and phosphonic acid to achieve the effect of defect passivation. Another way is to add some organic molecules to the perovskite precursor. These additives will react with NiO X However, for the first method, the steric hindrance of carbazole in the SAM material will limit the formation of a dense monolayer on the substrate, thereby hindering the effective passivation of the bottom defects of the perovskite film. For the second method, the concentration of the additive added to the perovskite is difficult to control, so the interface effect is not ideal.
[0037] In order to solve the above problems existing in the prior art, the present invention provides a method for preparing a perovskite solar cell, and a perovskite solar cell, which can reduce material costs, facilitate commercialization, and have a simple preparation process. Not only can the interface modification layer be evenly distributed to modify and passivate the defects at the interface between the nickel oxide layer and the perovskite layer, but the vacancy defects of the organic cations and halogens at the bottom of the perovskite layer can also be filled to synergistically solve the buried defect problem, inhibit non-radiative recombination at the interface, and enhance the passivation effect. At the same time, a carrier transmission channel can be formed at the interface to accelerate carrier transmission and improve the photoelectric conversion efficiency of the device.
[0038] In some non-limiting embodiments, the method for preparing the above-mentioned perovskite solar cell provided in the first aspect of the present invention can be used to prepare the above-mentioned perovskite solar cell provided in the second aspect of the present invention.
[0039] The following will describe the preparation principle of the above-mentioned method for preparing perovskite solar cells in combination with some examples of perovskite solar cells. Those skilled in the art will understand that these examples of the method for preparing perovskite solar cells are only some non-limiting implementation methods provided by the present invention, which are intended to clearly demonstrate the main concept of the present invention and provide some specific solutions that are convenient for the public to implement, rather than to limit the entire structure of the perovskite solar cell. Similarly, the perovskite solar cell is also only a non-limiting embodiment provided by the present invention, and does not constitute a limitation on the implementation subject of each step in the method for preparing these perovskite solar cells.
[0040] Please see Figure 1 , Figure 1 A schematic structural diagram of a perovskite solar cell provided according to some embodiments of the present invention is shown.
[0041] like Figure 1 As shown, in some embodiments of the present invention, the perovskite solar cell 100 may include a substrate 110, a hole transport layer 120, an interface modification layer 130, a perovskite light absorbing layer 140, an electron transport layer 150, and a metal electrode 160 stacked in sequence, wherein the interface modification layer 130 located between the hole transport layer 120 and the perovskite light absorbing layer 140 includes 1-ethyl-3-methyl hexafluorophosphate (EMImPF6).
[0042] Specifically, in order to better understand the structure of each layer in the above-mentioned perovskite solar cell 100, please refer to Figure 2 , Figure 2 A flow chart of a method for preparing a perovskite solar cell provided according to some embodiments of the present invention is shown.
[0043] like Figure 2 As shown, in some embodiments of the present invention, the method for preparing a perovskite solar cell may include the following steps S210: preparing a hole transport layer on a substrate, wherein the hole transport layer includes nickel oxide.
[0044] like Figure 2As shown, in some embodiments of the present invention, any one of glass made of doped tin oxide (FTO), glass made of indium tin oxide (ITO), and a conductive substrate of flexible indium tin oxide (ITO) can be obtained as the substrate 110 of the perovskite solar cell 100. Preferably, before performing the above step S210, the substrate 110 can be cleaned and pre-treated. Specifically, the substrate 110 can be placed in an ultrasonic cleaning device, and the substrate 110 can be cleaned in steps with detergent-free water, deionized water, and ethanol. The time for each step can be 20 minutes, and after the cleaning is completed, it is blown dry for use. Afterwards, the ultrasonically cleaned substrate 110 can be subjected to ozone treatment for 20 minutes to improve the wettability of the glass of the substrate 110.
[0045] Step S210 is performed to prepare a hole transport layer 120 on the surface of the clean substrate 110, wherein the hole transport layer 120 is nickel oxide (NiO X ) materials. Specifically, Figure 1 As shown, optionally, NiO X The substrate 110 is deposited by magnetron sputtering, and the sputtering method may be radio frequency sputtering.
[0046] Continue as Figure 2 As shown, after step S210 is performed, step S220 may be performed: preparing an interface modification layer on the surface of the hole transport layer, wherein 1-ethyl-3-methyl hexafluorophosphate is added to the interface modification layer.
[0047] Specifically, see Figure 3 , step S220 can be further concretized into steps S221 to S223.
[0048] In some embodiments of the present invention, step S221 can be performed first: obtain a self-assembled monolayer material composed of carbazole cores and phosphonic acid, and dissolve it in the solvent of the interface modification layer 130 to obtain a self-assembled monolayer solution, wherein the preferred range of the concentration of the self-assembled monolayer can be 0.5 to 1 mg / ml.
[0049] The material of the self-assembled monolayer (SAM) can be composed of a carbazole core and a phosphonic acid, such as 2PACz ([2-(9h-carbazole-9-yl)ethyl]phosphonic acid) and Me-4PACz ([4-(3,6-dimethyl-9h-carbazole-9yl)butyl]phosphonic acid). The solvent of the interface modification layer 130 can include any one of ethanol and isopropanol, or a mixed solvent of the two. For example, 0.5 mg of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid can be first obtained and dissolved in 1 ml of ethanol solution to obtain a solution of SAM.
[0050] Afterwards, step S222 may be performed: 1-ethyl-3-methyl hexafluorophosphate (EMImPF6) is added to the self-assembled monolayer solution to form a precursor of the interface modification layer 130, wherein the preferred range of the concentration of 1-ethyl-3-methyl hexafluorophosphate is 1 to 2 mg / ml. When the concentration of EMImPF6 is too low (e.g., less than or equal to 1 mg / ml), the precursor of the generated interface modification layer 130 is not suitable for NiO. X The passivation modification effect at the interface between the hole transport layer 120 and the perovskite light absorbing layer 140 is not obvious, and if the concentration of EMImPF6 is too high (for example, greater than or equal to 2 mg / ml), it may affect the transport of carriers at the interface. Continuing with the SAM solution obtained in the above example, 1.4 mg of EMImPF6 can be added to the obtained SAM solution to form a precursor of the interface modification layer 130.
[0051] In an embodiment of the present invention, by adding EMImPF6 to the SAM material, the defect of hindering the effective passivation of the bottom defects of the perovskite film caused by the steric hindrance of carbazole in the SAM material limiting the formation of a dense monolayer on the substrate can be solved, and the uniform distribution of SAM can be achieved to improve the passivation effect.
[0052] Further, preferably, the volume ratio of SAM to EMImPF6 in the above steps S221 and S222 can preferably be in the range of 1:1-1:2, so as to achieve uniform distribution of SAM on the hole transport layer 120 and achieve a good passivation effect.
[0053] Afterwards, step S223 may be performed: spin coating the precursor of the interface modification layer on the surface of the hole transport layer to form the interface modification layer.
[0054] Specifically, in some embodiments of the present invention, the precursor of the interface modification layer 130 can be deposited as a thin film on the surface of the hole transport layer 120 by a one-step spin coating method, wherein the spin coating speed of the precursor of the interface modification layer 130 is preferably in the range of 2000 to 3000 rpm, and the spin coating time can be 20s. Too small a spin coating speed (e.g., less than 2000 rpm) will result in an uneven distribution of the precursor of the interface modification layer 130, while too large a spin coating speed (e.g., greater than 3000 rpm) may result in a thin film of the generated interface modification layer 130 that is too thin, which is not conducive to carrier extraction. Then, heating annealing is performed to generate the interface modification layer 130. Optionally, the annealing temperature can be 80 to 100° C., and the annealing time can be controlled within the range of 10 to 15 min.
[0055] Please continue to return Figure 2After performing the above step S220 and preparing the interface modification layer 130 on the surface of the hole transport layer 120 , step S230 may be performed: preparing a perovskite light absorbing layer on the interface modification layer.
[0056] Specifically, in some embodiments of the present invention, a perovskite solution can be obtained and then dissolved in an organic solvent of perovskite to obtain a perovskite precursor. Then, in an ambient air with a humidity of 10 to 15%, the perovskite precursor is spin-coated on the surface of the interface modification layer 130 to deposit a perovskite film. If the ambient humidity during the spin coating process is too high, the perovskite will degrade. Afterwards, the perovskite light absorbing layer 140 can be obtained by heating and annealing. Optionally, the annealing temperature can be 100 to 150°C, and the annealing time can be controlled within the range of 10 to 35 minutes.
[0057] Further, the components of the perovskite may include but are not limited to any one of FAMAPbI, FACsPbI, and FAMACsPbI. The organic solvent used to dissolve the above perovskite solution may include a mixture of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), or a mixture of γ-butyrolactone (GBL) and N-methylpyrrolidone (NMP), wherein the volume ratio of dimethylformamide to dimethyl sulfoxide (DMF / DMSO) and γ-butyrolactone to N-methylpyrrolidone (GBL / NMP) can be in the range of 3-5:1.
[0058] In the present invention, in the above steps S210 to S230, during the preparation of the interface modification layer 130 located between the hole transport layer 120 and the perovskite light absorbing layer 140, a uniform distribution of the SAM material can be achieved by adding EMImPF6 to the SAM material, and the cations in EMImPF6 can fill the defects of organic cations and halogen vacancies at the bottom of the film of the perovskite light absorbing layer 140, thereby synergistically solving the buried defect problem, inhibiting non-radiative recombination, accelerating carrier transport, and improving device performance.
[0059] like Figure 2 As shown, after performing the above step S230, step S240 may be performed: preparing an electron transport layer on the perovskite light absorbing layer.
[0060] like Figure 1 As shown, in some optional embodiments, the electron transport layer 150 can be prepared on the upper layer of the perovskite light absorption layer 140 by evaporation. The materials that can be used for the electron transport layer 150 include fullerene (C 60 ) or fullerene derivatives (e.g., PCBM).
[0061] Furthermore, if Figure 1As shown, preferably, after performing the above step S230 and preparing the electron transport layer 150, a hole blocking layer 151 can be prepared on the surface of the electron transport layer 150 to adjust the distribution of electrons and holes in the device to improve the luminous efficiency and device life. Optionally, the material of the hole blocking layer 151 can be 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP). BCP, as a commonly used hole blocking material / electron transport material, is usually used in blue light and white light organic electroluminescent devices. Inserting the BCP film between the perovskite light absorbing layer 140 and the metal electrode 160 can significantly improve the electron collection rate at the interface, and its hole blocking ability will also increase with the increase of its thickness.
[0062] like Figure 2 As shown, after performing the above step S240, step S250 may be performed: preparing a metal electrode on the electron transport layer.
[0063] Combination Figure 1 As shown, in some preferred embodiments, a metal electrode 160 may be formed on the hole blocking layer 151. Preferably, the thickness of the metal electrode 160 may be in the range of 60 to 80 nm.
[0064] Although the above methods are illustrated and described as a series of actions for simplicity of explanation, it should be understood and appreciated that these methods are not limited by the order of the actions, because according to one or more embodiments, some actions may occur in a different order and / or concurrently with other actions from those illustrated and described herein or not illustrated and described herein but understandable to those skilled in the art.
[0065] Next, in order to better introduce the above-mentioned perovskite solar cell protected by the present invention and its preparation method, a specific embodiment of the present invention will be shown below, and compared with some comparative examples in the prior art.
[0066] Combination Figure 1 and Figure 2 As shown, in one embodiment of the present invention, the preparation method of the perovskite solar cell includes the following steps. FTO (fluorine-doped SnO2 conductive glass) is selected as the substrate 110, and the substrate 110 can be cleaned and pretreated first. Specifically, the FTO substrate 110 can be placed in an ultrasonic cleaning device, and the FTO substrate 110 can be cleaned in steps with detergent-free water, deionized water, and ethanol. Each step can take 20 minutes, and then it is blown dry for use. Then, the ultrasonically treated FTO substrate 110 can be treated with ultraviolet ozone for 20 minutes.
[0067] Then, step S210 is performed: preparing the hole transport layer 120 on the substrate 110. Specifically, NiOx can be deposited on the clean substrate 110 by magnetron sputtering, and the sputtering method can be radio frequency sputtering.
[0068] Then, step S220 is performed: an interface modification layer 130 is prepared on the surface of the hole transport layer 120. Specifically, 0.5 mg of Me-4PACZ can be dissolved in 1 ml of ethanol solution, and then 1.4 mg of EMImPF6 is added to the SAM solution to obtain a mixed SAM precursor, that is, a precursor of the interface modification layer. Then, the reserved mixed SAM precursor can be spin-coated on the hole transport layer 120 of NiOx, and a one-step spin coating method is used to deposit a thin film, and the spin coating speed can be 3000 rpm and the spin coating time can be 20 s.
[0069] Then, step S230 is performed: preparing a perovskite light absorbing layer 140 on the interface modification layer 130. Specifically, 1.5 mol of FA 0.85 Cs 0.15 Pb I3 The perovskite solution is dissolved in 1 ml of an organic solvent with a volume ratio of DMF:NMP=4:1, stirred for 2 hours for standby use, and a perovskite precursor can be obtained at this time. Afterwards, the standby perovskite precursor can be spin-coated on the interface modification layer 130, and a thin film can be deposited using a one-step spin coating method, the spin coating speed can be 5000 rpm, and the rotation time can be 30 seconds. Afterwards, 5 seconds before the end of the spin coating deposition, 300 microliters of anisole can be quickly added to obtain a perovskite wet film, and then the perovskite wet film is annealed in an environment of 150°C for 10 minutes to obtain a perovskite dry film, that is, a perovskite light absorbing layer 140.
[0070] Then, step S240 is performed: an electron transport layer 150 is prepared on the perovskite light absorption layer 140. Specifically, the electron transport layer 150 can be formed on the prepared perovskite light absorption layer 140. Fullerene (C) with a thickness of 30 nm was deposited at a rate of 60 ). Further, on the prepared electron transport layer 150, BCP with a thickness of 6 nm was evaporated at a speed of .
[0071] Then, step S250 is performed: a metal electrode 160 is prepared on the hole blocking layer 151 on the electron transport layer 150. Specifically, a gold film can be deposited by thermal evaporation to form a 110 nm thick silver electrode as the metal electrode 160.
[0072] In the following comparative example used as a comparison, step S210 and steps S230 to S250 are the same as those in the above specific embodiment and will not be described in detail here, but there is a difference in step S220.
[0073] Specifically, in the first comparative example, step S220 is not included, that is, the perovskite solar cell prepared in the first comparative example does not have the interface modification layer 130 , and the perovskite light absorbing layer 140 is directly prepared on the upper layer of the hole transport layer 120 .
[0074] In the second comparative example, the step of generating the interface modification layer 130 is included, but EMImPF6 is not added to the interface modification layer 130. Specifically, in the second comparative example, step S2201 may include: taking 0.5 mg of Me-4PACZ in 1 ml of ethanol solution until it is dissolved, and obtaining a pure SAM precursor that does not include EMImPF6. Then, the spare pure SAM precursor is spin-coated on the hole transport layer 120 of NiOx, and a one-step spin coating method is used to deposit a thin film, and its spin coating speed and time may be 3000 rpm and 20 s, respectively.
[0075] In the third comparative example, a step of generating an interface modification layer 130 is included, but the content of the added EMImPF6 is less, for example, only 1 mg. Specifically, in the third comparative example, step S2202 may include: taking 0.5 mg of Me-4PACZ in 1 ml of ethanol solution until dissolved, and then adding 1 mg of EMIMPF6 dissolved in the SAM solution to obtain a mixed SAM precursor. Then, the standby mixed SAM precursor is spin-coated on the hole transport layer 120 of NiOx, and a one-step spin coating method is used to deposit a thin film, and the spin coating speed can be 3000 rpm, and the spin coating time can be 20 s.
[0076] In the fourth comparative example, a step of generating an interface modification layer 130 is included, but the content of the added EMImPF6 is relatively large, for example, 2 mg. Specifically, in the fourth comparative example, step S2203 may include: taking 0.5 mg of Me-4PACZ in 1 ml of ethanol solution until dissolved, and then adding 2 mg of EMIMPF6 dissolved in the SAM solution to obtain a mixed SAM precursor. Then, the standby mixed SAM precursor is spin-coated on the hole transport layer 120 of NiOx, and a one-step spin coating method is used to deposit a thin film, and the spin coating speed can be 3000 rpm, and the spin coating time can be 20 s.
[0077] Through the above-mentioned specific embodiment and four comparative examples, and combined with the four parameters of the solar cells in the comparative test in Table 1 below, it can be seen that whether it is short-circuit current density (Jsc), open circuit voltage (Voc), fill factor (FF), or energy conversion efficiency (PCE), it is significantly better than the comparative example that does not include the interface modification layer 130, or the comparative example in which the content of EMImPF6 added in the interface modification layer 130 exceeds the preferred range.
[0078] <![CDATA[Jsc(mA / cm 2 )]]> Voc(V) FF(%) PCE(%) Example 1 26.43 1.17 82.4 25.48 Comparative Example 1 23.77 1.01 76.2 18.24 Comparative Example 2 25.79 1.12 79.6 22.99 Comparative Example 3 26.11 1.15 80.6 24.2 Comparative Example 4 26.04 1.15 80.2 24.01
[0079] Table 1
[0080] In summary, the present invention provides a method for preparing a perovskite solar cell, and a perovskite solar cell, which can reduce material costs, facilitate commercialization, and have a simple preparation process. It can not only achieve uniform distribution of the interface modification layer to modify and passivate the defects at the interface between the nickel oxide layer and the perovskite layer, but also fill the vacancy defects of organic cations and halogens at the bottom of the perovskite layer to synergistically solve the buried defect problem, inhibit non-radiative recombination at the interface, and enhance the passivation effect. At the same time, it can also form a carrier transmission channel at the interface, accelerate carrier transmission, and improve the photoelectric conversion efficiency of the device.
[0081] The previous description of the disclosure is provided to enable any person skilled in the art to make or use the disclosure. Various modifications to the disclosure will be apparent to those skilled in the art, and the general principles defined herein may be applied to other variations without departing from the spirit or scope of the disclosure. Thus, the disclosure is not intended to be limited to the examples and designs described herein, but should be granted the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a perovskite solar cell, characterized in that: include: Preparing a hole transport layer on a substrate, wherein the hole transport layer includes nickel oxide; An interface modification layer is prepared on the surface of the hole transport layer, wherein 1-ethyl-3-methyl hexafluorophosphate is added to the interface modification layer; Preparing a perovskite light absorbing layer on the interface modification layer; preparing an electron transport layer on the perovskite light absorbing layer; and A metal electrode is prepared on the electron transport layer.
2. The preparation method according to claim 1, characterized in that The step of preparing an interface modification layer on the hole transport layer comprises: Obtaining a self-assembled monolayer material composed of carbazole cores and phosphonic acid, and dissolving it in the solvent of the interface modification layer to obtain a self-assembled monolayer solution, wherein the concentration of the self-assembled monolayer is in the range of 0.5 to 1 mg / ml; Adding the 1-ethyl-3-methyl hexafluorophosphate to the solution of the self-assembled monolayer to form a precursor of the interface modification layer, wherein the concentration of the 1-ethyl-3-methyl hexafluorophosphate is in the range of 1 to 2 mg / ml; and The precursor of the interface modification layer is spin-coated on the surface of the hole transport layer to form the interface modification layer.
3. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The solvent of the interface modification layer includes any one of ethanol and isopropanol, or a mixed solvent of the two.
4. The method for preparing a perovskite solar cell according to claim 3, characterized in that: The step of obtaining a self-assembled monolayer material composed of carbazole cores and phosphonic acid and dissolving it to form a self-assembled monolayer solution comprises: [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid is obtained and dissolved in an ethanol solution to obtain the self-assembled monolayer solution.
5. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The step of spin coating the precursor of the interface modification layer on the surface of the substrate to form the interface modification layer comprises: The precursor of the interface modification layer is deposited as a thin film on the surface of the hole transport layer by a one-step spin coating method.
6. The preparation method according to claim 1, characterized in that: The substrate includes any one of glass made of fluorine-doped tin oxide, glass made of indium tin oxide, and a conductive substrate of flexible indium tin oxide, Before the step of preparing a hole transport layer on the substrate, the method further comprises: cleaning the substrate; and The cleaned substrate is subjected to ozone treatment.
7. The preparation method according to claim 1, characterized in that: The step of preparing a perovskite light absorbing layer on the interface modification layer comprises: obtaining a perovskite solution and dissolving it in an organic solvent of perovskite to obtain a perovskite precursor; Spin coating the perovskite precursor on the surface of the interface modification layer to deposit a perovskite film; and The perovskite light absorbing layer is obtained by heating and annealing.
8. The preparation method according to claim 1, characterized in that: The components of the perovskite include any one of FAMAPbI, FACsPbI, FAMACsPbI, and The organic solvent of the perovskite includes a mixture of dimethylformamide and dimethyl sulfoxide, or a mixture of γ-butyrolactone and N-methylpyrrolidone, wherein the volume ratio of dimethylformamide to dimethyl sulfoxide, and γ-butyrolactone to N-methylpyrrolidone is in the range of 3-5:
1.
9. The preparation method according to claim 1, characterized in that: After the step of preparing an electron transport layer on the perovskite light absorbing layer, the method further comprises: A hole blocking layer is prepared on the surface of the electron transport layer, wherein the material of the hole blocking layer includes 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline.
10. A perovskite solar cell, characterized in that: include: A substrate, a hole transport layer, an interface modification layer, a perovskite light absorption layer, an electron transport layer, and a metal electrode are stacked in sequence, wherein the interface modification layer located between the hole transport layer and the perovskite light absorption layer includes 1-ethyl-3-methyl hexafluorophosphate.