Adhesive for resin and laminate
By using resin adhesion agent made of Maillard reaction products and caramelization reaction products on the copper-based material substrate, the problem of insufficient adhesion between copper-based material and resin substrate in high-frequency printed wiring board is solved, and the problem of insufficient adhesion between copper-based material and resin substrate in high-frequency printed wiring board is achieved. The reduction of conductor loss and the efficient combination of resin materials with excellent dielectric properties is achieved.
Patent Information
- Application Number
- CN202380033172.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-28
- Filing Date
- 2023-06-23
- Publication Date
- 2024-12-06
AI Technical Summary
In printed wiring boards for high-frequency applications, the adhesion between the copper-based material substrate and the resin substrate is insufficient, resulting in increased conductor loss and the electrostatic interaction between the resin material with excellent dielectric characteristics and other materials becomes smaller. Lower follow-up.
The adhesion of the copper-based material substrate and the resin substrate is improved by forming a layer of the adhesion of the resin on the surface of the copper-based material substrate by using a resin adhesion agent.
It realizes excellent adhesion between the copper-based material substrate and the resin substrate with excellent dielectric properties, and is suitable for high-frequency printed wiring boards, reducing conductor losses and improving the electrostatic interaction of the material.
Smart Images

Figure BDA0005075695350000161 
Figure BDA0005075695350000171 
Figure BDA0005075695350000181
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive for resin and a laminate. Background Art
[0002] Copper-clad laminates are made by laminating a copper-based material substrate (copper foil and copper alloy foil, etc.) on one or both sides of a resin substrate (prepreg and resin film, etc., which are composite materials of organic compounds and inorganic compounds), and are widely used in the manufacture of printed wiring boards, etc.
[0003] The copper-based material substrate used in the copper-clad laminate is generally subjected to a surface roughening treatment to ensure adhesion with the desired resin substrate. For example, Patent Document 1 discloses a surface treatment agent for roughening the surface of a copper or copper alloy to obtain a copper surface or copper alloy surface having good adhesion with resins such as prepregs and solder resists and having deep concave-convex surfaces.
[0004] Prior Art Literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 7-292483 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, in recent years, with the high speed of communication, the high frequency of electrical signals is continuously developing, so a printed wiring board (high frequency printed wiring board) that can correspond thereto is needed. Specifically, a copper-based material substrate and a resin substrate that can suppress transmission loss are required. When the surface roughness of the copper-based material substrate is large, due to the skin effect, the conductor loss tends to become larger, so it is not desirable to roughen the surface of the copper-based material substrate like the previous copper-clad laminate to form deep concave-convex.
[0009] In addition, in the high-frequency region, the dielectric loss of materials with poor dielectric properties (high relative dielectric constant and dielectric loss tangent) is more significant, so it is desirable to use resin materials with excellent dielectric properties (low relative dielectric constant and dielectric loss tangent). However, materials with excellent dielectric properties have less electrostatic interaction with other materials and tend to have lower adhesion to other materials.
[0010] In summary, when copper-clad laminates are used in printed wiring boards for high-frequency applications, sufficient adhesion is required between the copper-based material substrate (especially a copper-based material substrate with low surface roughness) and the resin substrate (especially a resin substrate with excellent dielectric properties).
[0011] In view of the above, the present invention aims to provide, in one embodiment, a resin adhesive having excellent adhesion between a copper-based material substrate and a resin substrate. In another embodiment, the present invention aims to provide a laminate having the resin adhesive.
[0012] Means of solving the problem
[0013] The present invention relates to the following items. [1]
[0015] A resin adhesive comprises one or two selected from a Maillard reaction product (C) and a caramelization reaction product (D), wherein the Maillard reaction product (C) is obtained using a sugar (A) and / or a reductone (B), and an amine compound (G) as raw materials, and the caramelization reaction product (D) is obtained using a sugar (A) and / or a reductone (B) as raw materials. [2]
[0017] A laminated body comprising a copper-based material substrate, a layer of the resin adhesive as described in [1], and a resin substrate in this order. [3]
[0019] A resin adhesive, comprising one or two selected from a Maillard reaction product (C) and a caramelization reaction product (D), wherein the Maillard reaction product (C) is obtained using sugars (A) and / or reductones (B), and an amine compound (G) and / or an amine equivalent (H) as raw materials, and the caramelization reaction product (D) is obtained using sugars (A) and / or reductones (B) as raw materials. [4]
[0021] A laminated body comprising a copper-based material substrate, a layer of the resin adhesive as described in [3], and a resin substrate in this order.
[0022] Effects of the Invention
[0023] According to one embodiment of the present invention, a resin adhesive having excellent adhesion between a copper-based material substrate and a resin substrate can be provided. In particular, a resin adhesive having excellent adhesion between a copper-based material substrate with low surface roughness and a resin substrate with excellent dielectric properties can be provided. Therefore, for example, by using the resin adhesive, a copper-clad laminate having excellent adhesion between a copper-based material substrate with low surface roughness and a resin substrate with excellent dielectric properties can be provided. The copper-clad laminate can be applicable to printed wiring boards, particularly high-frequency printed wiring boards. DETAILED DESCRIPTION
[0025] <1. Adhesive for resin>
[0026] According to one embodiment of the present invention, the resin adhesive comprises one or two selected from the group consisting of a Maillard reaction product (C) and a caramelization reaction product (D), wherein the Maillard reaction product (C) is obtained from saccharides (A) and / or reductones (B), and amine compounds (G) and / or amine equivalents (H) as raw materials, and the caramelization reaction product (D) is obtained from saccharides (A) and / or reductones (B) as raw materials. The resin adhesive may include additives other than the Maillard reaction product (C) and the caramelization reaction product (D). As additives, for example, reaction accelerators (III), crosslinking agents (IV), pH regulators, etc. added when manufacturing the adhesive, and inorganic compounds, organic compounds, etc. added when manufacturing the adhesive liquid can be listed.
[0027] [1-1. Sugars (A)]
[0028] In the present invention, carbohydrates (A) refer to monosaccharides and polysaccharides (hereinafter referred to as compounds (E)) and derivatives of compounds (E) (hereinafter referred to as sugar derivatives (F)). Monosaccharides refer to compounds of polyols with more than 3 consecutive carbon atoms, more than 1 aldehyde group or ketone group, and more than 2 hydroxyl groups, and are carbohydrates that cannot be hydrolyzed. Polysaccharides refer to substances formed by the combination of two or more monosaccharides. The bonding mode of the sugars constituting the polysaccharide is not particularly limited, and examples thereof include ether bonds (particularly glycosidic bonds) or ester bonds. Carbohydrates (A) include carbohydrates having chain structures and ring structures, or can be provided in the form of a mixture of the two.
[0029] In the present invention, sugar derivatives (F) refer to compounds and salt compounds thereof in which the functional groups of compounds (E) are partially transformed. Partial transformation of functional groups refers to, for example, carboxylation, amination, etherification, esterification (for example, carboxylate, phosphate, sulfate, nitrate, carbonate, etc.), acylation, silylation, siloxane, hydroformylation, ketonization or halogenation of hydroxyl groups, and hydroxylation or carboxylation of aldehyde groups, as well as dehydration caused by the detachment of hydroxyl groups and their β-hydrogen atoms. In addition, salt compounds thereof refer to, for example, alkali metal salts such as lithium, sodium, potassium, rubidium, and cesium, alkaline earth metal salts such as beryllium, magnesium, calcium, strontium, and barium, and transition metal salts such as titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zirconium, niobium, and molybdenum. Typical sugar derivatives (F) include, but are not limited to, saccharic acid, sugar alcohol, amino sugar, dehydrated derivatives of sugars, and salt compounds thereof.
[0030] Specific examples of monosaccharides include, but are not limited to, dihydroxyacetone, glyceraldehyde, erythrose, threose, ribose, arabinose, xylose, lyxose, allose, altrose, glucose, mannose, gulose, idose, galactose, talose, erythrulose, xylulose, ribulose, psicose, fructose, sorbitol, tagatose, sedoheptulose, coriose, desaturase, dextrose ... Oxyribose, fucose, fuculose, rhamnose, allomethylose, quinovose, antiallose, talomethylose, digitarose, digitoxose, shimarose, tyvelose, abequose, paratose, colitose, ascarylose, etc.
[0031] Specific examples of polysaccharides and their derivatives include, but are not limited to, dihydroxyacetone dimer, glyceraldehyde dimer, sucrose, lactulose, lactose, maltose, trehalose, cellobiose, kojibiose, nigerose, isomaltose, isotrehalose, neotrehalose, sophorose, laminaribiose, gentiobiose, turanose, maltulose, palatinose, gentiobiulose, mannobiose, melibiose, melibiulose, neolactose, galactosucrose, scillabiose, neohesperidose, rutinose, rutinulose, vicianose, xylobiose, primeverose, trehalosamine, maltitol, cellobionic acid, lactosamine, lactosyldiamine, lactobionic acid, lactitol, hyalobiuronic acid acid), sucralose, nigerotriose, maltotriose, melezitose, maltotriulose, raffinose, ketose, ketotetraose, nigerotetraose, stachyose, acarbose, lactose oligosaccharides, maltose oligosaccharides, isomaltose oligosaccharides, gentio oligosaccharides, niger oligosaccharides, galactose oligosaccharides, wood oligosaccharides, Sugar oligosaccharides, soybean oligosaccharides, fructo-oligosaccharides, manno-oligosaccharides, glycogen, starch, cellulose, dextran, fructan, hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, carboxymethyl cellulose salts (e.g., sodium salt), alginic acid, propylene glycol alginate, agarose, cellulose derivatives, guargum, carrageenan, agar, chitosan, gellan gum, dextrin, dextran, starch, pullulan, etc.
[0032] In the present invention, sugar acid refers to a compound in which one or more aldehyde groups or terminal hydroxyl groups of compound (E) are converted into carboxyl groups. Specifically, the compounds include, but are not limited to, glyceric acid, erythric acid, threonic acid, ribonic acid, arabinic acid, xylic acid, lysonic acid, allonic acid, altronic acid, gluconic acid, mannonic acid, gulonic acid, idonic acid, galactonic acid, talonic acid, erythraric acid, tartaric acid, ribonic acid, arabinaric acid, xylaric acid, allaric acid, altraric acid, glucaric acid, mannuronic acid, iduronic acid, galactonic acid, glucuronic acid, mannuronic acid, gulonic acid, galacturonic acid, iduronic acid, and the like.
[0033] In the present invention, sugar alcohol refers to a compound in which one or more aldehyde groups or ketone groups of compound (E) are converted into hydroxyl groups. Specifically, it can be listed, but not limited to, sorbitol, mannitol, erythritol, pentaerythritol, threitol, arabitol, ribitol, xylitol, galactitol, rhamnitol, isomalt, maltitol, lactitol, palatinitol, etc.
[0034] In the present invention, amino sugar refers to a compound in which one or more hydroxyl groups of the compound (E) are substituted by an amino group, and a compound in which the amino group of the compound is further acylated. Specifically, it includes, but is not limited to, glucosamine, galactosamine, N-acetylglucosamine, N-aminoformylglucosamine, N-acetylgalactosamine, chitin, chitosan, chondroitin, hyaluronic acid, heparin, etc. In addition, some of the amino sugars are equivalent to the amine compound (G) or amine equivalent (H) described later.
[0035] In the present invention, the dehydrated derivative of sugar refers to a compound produced by an intramolecular dehydration reaction of compound (E). Specifically, furfural, hydroxymethylfurfural, etc. can be mentioned but are not limited thereto.
[0036] As the raw material sugar (A) for obtaining the Maillard reaction product (C) and / or the caramelization reaction product (D), monosaccharides, polysaccharides, sugar acids and salts thereof are preferred, among which reducing sugars (for example, reducing Cu in the Fehling reaction) are more preferred. 2+ Reduction to Cu +The sugar (A) may be used alone or in combination of two or more.
[0037] [1-2. Reductive ketones (B)]
[0038] In the present invention, reducing ketones (B) refer to compounds having a chemical structure represented by the following formula 1 in the molecule. Specifically, examples include, but are not limited to, ascorbic acid, erythorbic acid and salts thereof (e.g., alkali metal salts, alkaline earth metal salts or transition metal salts, and complex salts of the above metal salts). In addition, as long as the compound has the following chemical structure in the molecule, it can be a compound in which some functional groups have been transformed, and it can also be a salt compound thereof. Examples of "partial functional group transformation" are the same as those described in the description of sugars (A). Reducing ketones (B) can be used alone or in combination of two or more.
[0039]
Chemistry 1
[0040] -C(OH)=C(OH)-C(=O)-···(Formula 1)
[0041] [1-3. Maillard reaction products (C)]
[0042] In the present invention, the Maillard reaction product (C) refers to a brown substance generated by the reaction of sugars (A) and / or reductones (B) and amine compounds (G) as raw materials. In the Maillard reaction, sugars (A) and / or reductones (B) are combined with amine compounds (G), and further reactions such as decomposition, oxidation, condensation and polymerization are involved, but the reaction pathway is complicated and it is extremely difficult to perform component analysis of the Maillard reaction product (C). Therefore, in the present invention, a brown substance is generated by the reaction of sugars (A) and / or reductones (B) and amine compounds (G), that is, it is considered that the Maillard reaction product (C) is obtained.
[0043] In the present invention, whether a brown substance is generated is determined as follows. A liquid sample having a mass concentration of 10% by mass of the solute and / or dispersion medium of the resin adhesive to be measured is prepared. When the yellowness (YI) of the liquid sample is 2.5 or more, it is determined that "brown substance is generated". YI can be measured using a commercially available spectrocolorimeter. For example, using a spectrocolorimeter (SD7000) manufactured by Nippon Denshoku Industries Co., Ltd., the three stimulus values (X, Y, Z) in the XYZ colorimetric system are obtained by a spectrophotometric colorimetric method based on the transmittance measured under the conditions of auxiliary colored lights C and a 2-degree visual field. According to ASTM D1925, the three stimulus values are applied to the following formula to calculate YI.
[0044] YI=100(1.28X-1.06Z) / Y
[0045] When preparing a liquid sample, the solvent and / or dispersion medium for diluting the resin adhesive should be pure water. When concentrating the resin adhesive for preparing a liquid sample, the following method can be used: put the resin adhesive into a container, open it and leave it at 35°C or below to evaporate the solvent and / or dispersion medium, or use a rotary evaporator to remove the solvent and / or dispersion medium by reduced pressure distillation at 35°C or below.
[0046] In addition, the mass concentration of the liquid sample can be calculated from the weight of the resin adhesive before and after drying.
[0047] In addition, as a measurement method using a spectrocolorimeter, when the concentration of the resin adhesive is adjusted to 10% by mass, if the transmittance cannot be measured because the color of the liquid sample is too dark, the resin adhesive is diluted until the transmittance can be measured. When the measured YI is 2.5 or more, it is determined that "brown substance is generated."
[0048] In the present invention, the amine compound (G) refers to ammonia, primary amines, secondary amines and salts thereof. In addition, the amine compound (G) also includes amino acids, peptides, proteins and salts thereof. As the amine compound (G), preferably, amines (specifically primary amines, ammonia) and salts thereof that are less than secondary amines and primary amines are preferred, and ammonia and salts thereof are particularly preferred. In addition, the carbon adjacent to the amino group in the amine compound (G) is preferably primary carbon, secondary carbon or tertiary carbon. In addition, as the amine compound (G), for example, arylamines and salts thereof, alkylamines and salts thereof, heteroarylamines and salts thereof, and ammonia and salts thereof can be cited. Among them, preferably one or more selected from arylamines, alkylamines, heteroarylamines and ammonia, more preferably one or more selected from alkylamines, heteroarylamines and ammonia, and particularly preferred ammonia. The amine compound (G) can be used alone or in combination of two or more, or in combination with one or more of the amine equivalents (H) described later.
[0049] As the above-mentioned ammonia and its salt, ammonia and a salt compound composed of ammonia and an acid can be used. Examples of the acid that forms a salt with ammonia include hydrofluoric acid, hydrochloric acid, hydrobromic acid, hydroiodic acid, hypochlorous acid, chlorous acid, chloric acid, perchloric acid, nitric acid, nitrous acid, sulfuric acid, sulfurous acid, peroxymonosulfuric acid, peroxydisulfuric acid, phosphoric acid, phosphorous acid, hypophosphorous acid, hydrocyanic acid, cyanic acid, thiocyanic acid, carbonic acid, boric acid, silicic acid, chromic acid, dichromic acid, permanganic acid, molybdic acid, and tungstic acid, as well as inorganic acids such as formic acid, acetic acid, propionic acid, and butyric acid. , valeric acid, lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, lactic acid, malic acid, citric acid, benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, salicylic acid, gallic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid, malic acid, gluconic acid, methanesulfonic acid, benzenesulfonic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoroacetic acid and peracetic acid and other organic acids. The acid that forms a salt with ammonia may be used alone or in combination of two or more.
[0050] As the secondary amine, for example, 1 R 2 Compounds with the chemical structure of NH can be listed as R 1 , R 2 Compounds independently of each other having no substituent or arbitrarily having any substituent of alkyl, aryl and heteroaryl. In addition, it can be listed as a substituent having no substituent or arbitrarily having a saturated heterocyclic amine and a substituent having no substituent or arbitrarily having an unsaturated heterocyclic amine, the unsaturated heterocyclic amine being an unsaturated heterocyclic amine with or without aromaticity. As the above-mentioned substituent, it can be listed as an alkyl, alkenyl, alkynyl, aryl, hydroxyl, sulfhydryl, carbonyl (such as aldehyde, ketone, carboxyl, acyl, ester, amide, etc.), imino, thiocarbonyl, fluoro, chloro, bromo, iodo, nitro, sulfo, cyano, alkoxy, trifluoromethyl, azo, silanyl or siloxy. Examples of secondary amines include dimethylamine, diethylamine, dipropylamine, dibutylamine, diallylamine, diphenylamine, dibenzylamine, diethanolamine, ethylmethylamine, N-methylaniline, methylbenzylamine, aziridine, azetidine, pyrrolidine, piperidine, morpholine, pyrrole, pyrazole, imidazole, 1,2,3-triazole, 1,2,4-triazole, tetrazole, indoline, indole, and proline.
[0051] As the primary amine, for example, a compound having a chemical structure of RNH2, compounds in which R is not substituted or arbitrarily has any substituent of an alkyl group, an aryl group, and a heteroaryl group having a partial structure of -NH- in the ring structure can be cited. Examples of primary amines include methylamine, ethylamine, propylamine, butylamine, octylamine, cyclohexylamine, allylamine, ethanolamine, propanolamine, benzylamine, furfurylamine, phenylethylamine, aniline, methoxyaniline, trifluoromethylaniline, aminobenzoic acid, aminosalicylic acid, nitroaniline, cyanoaniline, fluoroaniline, chloroaniline, bromoaniline, iodoaniline, aminophenol, aminothiophenol, naphthylamine, aminopyridine, hydroxylamine, aminotriazine, aminothiazole, amino-1,3,4-thiadiazole , amino-1,2,3-thiadiazole, 2-amino-5-mercapto-1,3,4-thiadiazole, aminopyrazine, aminopyrimidine, amino-1,2,4-triazine, amino-1,3,5-triazine, L-dopamine, dopamine, norepinephrine, glycine, alanine, valine, leucine, isoleucine, cysteine, methionine, serine, threonine, aspartic acid, glutamic acid, glutamine, arginine, phenylalanine, tyrosine, etc.
[0052] The amine compound (G) may be a monoamine having one amino group in one molecule and a salt thereof, or a polyamine having two or more amino groups and a salt thereof. In addition, the amine compound (G) may be a monomer or a polymer. The amino group of the polyamine may include a primary amino group, a secondary amino group, or a combination of the two. Examples of the polyamine include ethylenediamine, diethylenetriamine, hexamethylenediamine, triethylenetetramine, piperazine, phenylenediamine, aminobenzylamine, diaminonaphthalene, diaminopyridine, triaminopyridine, diaminopyrimidine, triaminopyrimidine, diamino-1,3,5-triazine, triamino-1,3,5-triazine, aminopyrazole, aminoimidazole, aminobenzimidazole, amino-1H-tetrazole, amino-1,2,4-triazole, diamino-1,2,4-triazole, diaminodiphenylmethane, dimethylthiotoluenediamine, diaminodiphenyl sulfone, diaminodiphenyl ether, bis(3-aminophenoxy)benzene, bis[2-(4-aminophenyl)-2-propyl]benzene, adenine, lysine, histidine, tryptophan, gelatin, albumin, casein, silk protein, keratin, yolk protein, ovalbumin, yeast protein, collagen, chitosan, and hydrazine.
[0053] In the present invention, the amine equivalent (H) refers to a compound that can easily generate an amine compound (G) by hydrolysis. In the present invention, the amine equivalent (H) generates ammonia, a primary amine or a secondary amine, and then undergoes a Maillard reaction with a sugar (A) and / or a reductone (B). In order to promote hydrolysis, heating or warming conditions may be added, or a catalyst or an acid or a base may be added. Examples of the amine equivalent (H) include R 1 R 2 NC(=O)NR3 R 4 The urea derivative represented by R 1 R 2 NC(=S)NR 3 R 4 The thiourea derivative represented by R 1 OC(=O)NR 2 R 3 The carbamate compound represented by R 1 OC(=S)NR 2 R 3 O-thiocarbamate compounds represented by R 1 SC(=O)NR 2 R 3 The S-thiocarbamate compound represented by R 1 OC(=NR 2 )NR 3 R 4 The isourea derivative represented by R 1 SC(=NR 2 )NR 3 R 4 The isothiourea derivative represented by R 1 SC(=S)NR 2 R 3 The dithiocarbamate compound represented by R 1 C(=NR 2 )NR 3 R 4 The amidine compound represented by R 1 R 2 NC(=NR 3 )NR 4 R 5 Specific examples include urea, thiourea, carbamic acid, amidine, acetamidine, guanidine and its derivatives. In addition, the aromatic ring contains C(=N)-NR 1 R 2 Substances such as 3-amino-1H-1,2,4-triazole, melamine, etc. are not amine equivalents (H) but are equivalent to amine compounds (G). 1 To R 5 Each independently represents hydrogen, no substituent, or arbitrarily having any substituent of an alkyl group, an aryl group, or a heteroaryl group. The amine equivalent (H) may be used alone or in combination of two or more, or may be used in combination with the above-mentioned amine compound (G).
[0054] [1-4. Conditions of Maillard reaction]
[0055] The reaction conditions of the Maillard reaction are not particularly limited, as long as the raw materials of the sugar (A) and / or the reductone (B), and the amine compound (G) and / or the amine compound (G) generated from the amine equivalent (H) react to generate a brown substance, the concentrations of the sugar (A), the reductone (B) and the amine compound (G), the reaction time, the reaction pressure, the presence and type of the solvent and / or the dispersion medium (I), the reaction temperature (II), the addition of the reaction accelerator (III) and the addition of the crosslinking agent (IV), the adjustment of the pH (V), etc. during the reaction can be appropriately set. When the amine equivalent (H) is used, the amine equivalent (H) is decomposed in the reaction system to generate the amine compound (G), and the reaction conditions can be appropriately adjusted so that the Maillard reaction occurs. After the amine compound (G) is generated in the reaction system, the reaction conditions of the Maillard reaction can also be appropriately adjusted.
[0056] The solvent and / or dispersion medium (I) is not particularly limited, and polar aprotic or protic solvents and / or dispersion mediums are preferred, polar protic solvents are more preferred, and water is particularly preferred. In addition, the solvent and / or dispersion medium (I) may be used alone or in combination of two or more, but the content of water in the solvent and / or dispersion medium is preferably 10% by mass or more, more preferably 30% by mass or more, further preferably 50% by mass or more, further more preferably 70% by mass or more, particularly preferably 90% by mass or more, and most preferably only water.
[0057] The reaction temperature (II) is not particularly limited, but heating is preferred. The reaction temperature (II) is preferably, for example, 40 to 200°C, 60 to 200°C, 70 to 200°C, 80 to 200°C, 90 to 200°C, or 95 to 200°C.
[0058] Reaction promoter (III) (such as Lewis acid catalyst, free radical initiator and oxidant etc.) is not particularly limited, can be added or not added, generally can be used as long as it is an additive that promotes Maillard reaction. As Lewis acid catalyst, for example, metal salts that generate metal ions such as zinc ion, lead ion, iron ion and copper ion in aqueous solution can be listed. As free radical initiator, for example, peroxides and salts thereof such as hydrogen peroxide, tert-butyl hydroperoxide, peroxydisulfuric acid (peroxydisulfuric acid), peracetic acid (ethaneperoxoic acid) and oxo acids (oxo acid) and salts thereof such as perchloric acid and periodic acid can be listed. As oxidant, for example, nitric acid and its salt, permanganate, chromate, dichromate, hypochlorite, iron chloride (III), iron fluoride (III), iron nitrate (III), iron sulfate (III) etc. can be listed. Examples of other reaction accelerators (III) include sodium chloride, phosphoric acid and its salts, ammonium sulfite, ammonium metabisulfite, sodium sulfite, sodium pyrosulfite, potassium sulfite, potassium pyrosulfite, and sulfurous acid gas. The reaction accelerators (III) may be used alone or in combination of two or more.
[0059] During the Maillard reaction, a known crosslinking agent (IV) may or may not be used. The crosslinking agent is not particularly limited, as long as it is a compound that is combined with the structure of the Maillard reaction product to form a crosslinked structure. As a crosslinking agent, for example, zirconium carbonate, titanium alkoxide, silane coupling agent, colloidal silica, isocyanate, blocked isocyanate, glyoxal, polycarboxylic acid and its anhydride, phosphoric acid and phosphate, polycarboxylic acid (such as succinic acid, citric acid and maleic anhydride, etc.) and its salt, epoxy compound, aziridine compound, urethane compound, hydrazide compound, oxazoline compound, carbodiimide compound, methylol melamine compound (such as methylol melamine and alkylated methylol melamine, etc.), acetoacetyl compound, etc. can be listed. One kind of crosslinking agent (IV) can be used alone, or two or more kinds can be used in combination.
[0060] The pH (V) at the start of the reaction is not particularly limited, but the pH range in which the reaction is easy to proceed is variable depending on the amine compound (G) or amine equivalent (H) used, so it can be adjusted appropriately. The Maillard reaction is generally easy to proceed in a non-strongly acidic pH range (e.g., pH 2.0 to pH 14.0, pH 3.0 to pH 13.5, pH 4.0 to pH 13.5, or pH 5.0 to pH 13.5). However, in the case of using an amine compound (G) that causes a free radical reaction, such as ammonium peroxodisulfate, the reaction can proceed even in a strongly acidic state, so it can be selected in a wider pH range (e.g., pH 0.1 to pH 14.0, pH 0.2 to pH 14.0, pH 0.3 to pH 14.0, or pH 1.0 to pH 14.0). In addition, a pH adjuster can be appropriately added for pH adjustment, but it may not be added. As the pH adjuster, there is no particular limitation, and examples thereof include inorganic acids, organic acids, inorganic bases, organic bases, and the like. As inorganic acid, for example, hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, etc. can be cited. As organic acid, for example, acetic acid, propionic acid, oxalic acid, maleic acid, adipic acid, gallic acid, butyric acid, salicylic acid, benzoic acid, methanesulfonic acid, benzenesulfonic acid, chloroacetic acid, formic acid, phthalic acid, fumaric acid, citric acid, tartaric acid, acrylic acid, methacrylic acid, etc. can be cited. As inorganic base, for example, ammonia, ammonium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, barium hydroxide, etc. can be cited. As organic base, the above-mentioned amine compound (G) etc. can be cited. One kind of pH adjusting agent can be used alone, or two or more kinds can be used in combination.
[0061] [1-5. Caramelization reaction product (D)]
[0062] In the present invention, the caramelization reaction product (D) refers to a brown substance generated by the decomposition, oxidation, condensation and polymerization reactions of the sugar (A) and / or the reductone (B) as raw materials by heat or the like. The reaction path of the caramelization reaction is complicated, and it is extremely difficult to analyze the components of the caramelization reaction product (D). Therefore, in the present invention, when a brown substance is generated by the reaction of the sugar (A) and / or the reductone (B) itself, it is considered that the caramelization reaction product (D) is obtained. The determination of whether a brown substance is generated is performed by the method described above.
[0063] [1-6. Reaction conditions of caramelization reaction]
[0064] The reaction conditions of the caramelization reaction are not particularly limited, as long as a brown substance is generated by heating the sugar (A) and / or the reducing ketone (B) as the raw materials. The concentration of the sugar (A) and the reducing ketone (B), the reaction time, the reaction pressure, the presence and type of the solvent and / or the dispersion medium (i), the reaction temperature (ii), the addition of a reaction accelerator (iii) and the addition of a cross-linking agent (iv), the adjustment of pH (v), etc. during the reaction can be appropriately set.
[0065] Reaction conditions (i) to (iv) are the same as reaction conditions (I) to (IV) in [1-4. Reaction conditions for Maillard reaction], and their description is omitted.
[0066] The pH (v) at the start of the reaction is not particularly limited, and a pH adjusting agent may be appropriately added to adjust the pH, or may not be added. The pH adjusting agent is not particularly limited, and examples thereof include inorganic acids, organic acids, inorganic bases, organic bases, and the like. As inorganic acids, for example, hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, and the like may be cited. As organic acids, for example, acetic acid, propionic acid, oxalic acid, maleic acid, adipic acid, gallic acid, butyric acid, salicylic acid, benzoic acid, methanesulfonic acid, benzenesulfonic acid, chloroacetic acid, formic acid, phthalic acid, fumaric acid, citric acid, tartaric acid, acrylic acid, methacrylic acid, and the like may be cited. As inorganic bases, for example, ammonia, ammonium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, barium hydroxide, and the like may be cited. As organic bases, the above-mentioned amine compounds (G) and the like may be cited. One pH adjusting agent may be used alone, or two or more may be used in combination.
[0067] As the Maillard reaction product (C) and the caramelization reaction product (D), commercially available products can be used. As the above-mentioned commercially available products, for example, commercially available caramel coloring can be cited. Caramel coloring is generally divided into four types: caramel I, caramel II, caramel III, and caramel IV (Japan Ministry of Health, Labor and Welfare, Consumer Affairs Agency, "9th Edition of Food Additives Official Book 2018")
[0068] Commercially available caramel coloring can be used in either liquid or powder form.
[0069] Caramel I is a substance obtained by heat-treating edible carbohydrates such as starch hydrolysate, molasses or sugar, or a substance obtained by heat-treating by adding an acid or an alkali, wherein no sulfite compound and ammonium compound are used. Caramel II is a substance obtained by further adding a sulfite compound during the reaction of caramel I. Caramel I and caramel II correspond to the caramelization reaction product (D). Specific commercially available products include liquid caramel manufactured by Morita Food Systems Co., Ltd. (product names: S-70, S-65, S-60, S-60S, SS, SSS, SM, SB, MK and F), powdered caramel manufactured by the same company (product names: SAP and FP), liquid caramel manufactured by Senba Sugar Chemical Industry Co., Ltd. (product names: caramel KS-S, caramel KS-SB, caramel KS-SNT, caramel KS-NB and caramel KS-45), powdered caramel manufactured by the same company (product names: powdered caramel SW, powdered caramel S-180W, powdered caramel KS-W, powdered caramel KS-SS, powdered caramel C-85, powdered caramel KS-LW, powdered caramel KS-SSW, powdered caramel MW and powdered caramel BD-W), and caramel color I manufactured by Kanto Chemical Co., Ltd.
[0070] Caramel III is obtained by adding an amino compound to edible carbohydrates such as starch hydrolysate, molasses or sugars, or by adding an acid or alkali thereto and heat-treating them, wherein no sulfite compound is used. Caramel IV is obtained by further adding a sulfite compound during the reaction of caramel III. Caramel III and caramel IV correspond to the Maillard reaction product (C). Specific commercially available products include liquid caramel manufactured by Morita Food Systems Co., Ltd. (product names: SL, MC, MR, MU, CL, CL-150, MS, MH and DS), powdered caramel manufactured by the same company (product name: MRP), liquid caramel manufactured by Senba Sugar Chemical Industry Co., Ltd. (product names: caramel TO, caramel MG-18, caramel S, caramel TB, caramel KD, caramel BD-2, caramel Z-80, caramel Z-100, caramel Z-35 and caramel WH-N-92), powdered caramel manufactured by the same company (product names: powdered caramel MG-18W, powdered caramel KD-W and powdered caramel Z-35W), and caramel color III manufactured by Kanto Chemical Co., Ltd.
[0071] [1-7. Method for producing adhesive for resin]
[0072] According to one embodiment of the present invention, a method for producing an adhesive for a resin is provided. The method for producing an adhesive for a resin includes, for example, one or both of step 1 and step 2.
[0073] Step 1: A Maillard reaction occurs in a reaction system containing a sugar (A) and / or a reductone (B), and an amine compound (G) and / or an amine equivalent (H) as raw materials to produce a brown substance. The state of the raw materials in the reaction system may be gas, liquid or solid, or a combination thereof. The phase in the reaction system may contain any of a gas phase, a liquid phase, and a solid phase, but preferably contains a liquid phase. A solvent and / or a dispersion medium may be used, or may not be used.
[0074] Step 2: Caramelization reaction occurs in a reaction system containing carbohydrates (A) and / or reductones (B) as raw materials to produce a brown substance. The state of the raw materials in the reaction system may be gas, liquid or solid, or a combination thereof. The phase in the reaction system may contain any of a gas phase, a liquid phase and a solid phase, but preferably contains a liquid phase. A solvent and / or a dispersion medium may be used or not.
[0075] The sugars (A), the reducing ketones (B), the amine compounds (G), the amine equivalents (H), the Maillard reaction and the caramelization reaction are as described above.
[0076] <2. Laminated body>
[0077] The laminate of one embodiment of the present invention has a copper-based material substrate, a layer of the above-mentioned resin adhesive and a resin substrate in sequence. Typically, the laminate is provided as a copper-clad laminate having a copper-based material sheet, a layer of the above-mentioned resin adhesive and a resin sheet in sequence. In the copper-clad laminate, the copper-based material sheet can be laminated on a single surface of the resin sheet, or it can be laminated on both surfaces of the resin sheet. In addition, the copper-based material sheet can be laminated on the entire surface of one side or both sides of the resin sheet, or it can be laminated only on a portion of the surface. The layer of the resin adhesive is usually formed on the entire surface of the bonding surface of the copper-based material sheet with the resin sheet, but it can also be formed only on a portion of the bonding surface of the copper-based material sheet with the resin sheet. Similarly, the layer of the resin adhesive can be formed on the entire surface of the bonding surface of the resin sheet with the copper-based material sheet, or it can be formed only on a portion of the bonding surface of the resin sheet with the copper-based material sheet. In addition, when the copper-based material sheet is stacked on both sides of the resin sheet, as long as at least one side of the copper-based material sheet is stacked on the resin sheet by a layer of a resin adhesive of an embodiment of the present invention, it is preferred that the copper-based material sheets on both sides are stacked on the resin sheet by a layer of a resin adhesive of an embodiment of the present invention. The two copper-based material sheets stacked on both sides of the resin sheet may be the same or different, and the layers of the two resin adhesives may be the same or different. In the case where the copper-based material sheet is stacked on a single side of the resin sheet, other layers may also be stacked on the surface of the resin sheet on the opposite side of the surface of the stacked copper-based material sheet. As other layers, examples but not limited to, release film layers for protecting the resin sheet. In addition, the copper-clad laminate may further stack other layers on the surface of the copper-based material sheet on the opposite side of the surface stacked with the resin sheet. This other layer may be a layer of a resin adhesive, i.e., a layer containing one or both of a Maillard reaction product (C) and a caramelization reaction product (D).
[0078] [2-1. Copper-based material substrate]
[0079] The copper-based material substrate is a substrate with copper or a copper alloy as the main component (the concentration of copper or a copper alloy is 50% by mass or more, preferably 60% by mass or more, more preferably 75% by mass or more, and further preferably 85% by mass or more, for example 50 to 100% by mass), and is typically provided in the form of a sheet such as a plate or foil. The sheet can be composed of a single layer or can be composed of two or more layers stacked. As the content ratio of copper in the copper alloy, as long as it contains copper, it is not particularly limited, preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 75% by mass or more, and particularly preferably 85% by mass or more. As copper alloys, specific examples include, but are not limited to, copper-zinc alloys, copper-iron-phosphorus alloys, copper-tin alloys, copper-zirconium alloys, copper-nickel alloys, copper-silver alloys, etc. specified in JIS H3100:2012 or CDA (Copper Development Association) standards. The copper-based material substrate may also be a material for surface treatment of the copper foil or copper alloy foil of the copper-clad laminate used in the printed wiring board. As the surface treatment, for example, electroplating treatments such as single metal plating treatment or alloy plating treatment or chromate treatment may be cited. As the plating treatment, any of the known plating treatments may be cited, for example, single metal plating treatments or alloy plating treatments containing one or more elements selected from the group of nickel, zinc, tin, cobalt, molybdenum, copper, tungsten, phosphorus, arsenic, chromium, vanadium, titanium, aluminum, gold, silver, platinum group elements, iron, and tantalum may be cited. The plating treatment may be a single-layer plating or a multilayer plating of more than two layers. In addition, the copper-based material substrate may also be surface treated with a coupling agent such as a silane coupling agent, but according to the present invention, even if the copper-based material substrate is not subjected to a surface treatment based on a coupling agent, excellent adhesion between the copper-based material substrate and the resin substrate may be obtained. In addition, such a surface treatment may be carried out according to a known method.
[0080] As the copper-based material substrate, there is no particular limitation, and copper plates, copper alloy plates, copper foils, copper alloy foils, such as rolled copper plates, rolled copper alloy plates, rolled copper foils, rolled copper alloy foils, electrolytic copper foils, and electrolytic copper alloy foils, and materials subjected to the above-mentioned surface treatment on their surfaces can be appropriately used. In addition, copper foils with carriers and copper alloy foils with carriers, and copper foils and copper alloy foils subjected to the above-mentioned surface treatment on the surfaces of these copper foils and copper alloy foils can also be appropriately used. In this case, non-carrier copper foils with carrier copper foils and non-carrier copper alloy foils with carrier copper alloy foils can be used as copper-based material substrates of a laminate of one embodiment of the present invention. In addition, copper-plated materials, copper alloy-plated materials, copper-clad materials, laminates having copper-based material substrates such as copper alloy-clad materials on the surface, and materials obtained by subjecting the surfaces of these copper-based material substrates to the above-mentioned surface treatment can also be appropriately used. In this case, the copper-based material substrate contained in the laminate becomes the copper-based material substrate of a laminate of one embodiment of the present invention. The carrier of the copper foil with a carrier or the copper alloy foil with a carrier is not particularly limited, and any of the metal foils such as electrolytic copper foil or resin films generally used can be used. The thickness of the carrier is not particularly limited and can be appropriately selected. The copper foil with a carrier and the copper alloy foil with a carrier are generally, but not limited to, electrolytic copper foil with a carrier and electrolytic copper alloy foil with a carrier. In addition, the resin substrate can also be laminated on the copper-based material substrate contained in the copper-clad laminate produced by the existing method or in the present embodiment via the above-mentioned resin adhesive, and the laminate obtained in this way is also a laminate of an embodiment of the present invention.
[0081] The copper-based material substrate is usually preferably smooth on the surface. It is particularly preferred that the copper-based material substrate is smooth on both sides when it is provided in the form of sheets such as plates and foils. Specifically, the ten-point average roughness (Rzjis) of the surface is preferably 15 μm or less, more preferably 10 μm or less, further preferably 5 μm or less, particularly preferably 2.5 μm or less, and most preferably 1.5 μm or less. In addition, the copper-based material substrate is usually preferably not subjected to roughening treatment on its surface. The lower limit of the ten-point average roughness (Rzjis) of the surface of the copper-based material substrate is not particularly limited, and is usually preferably close to 0 μm. The ten-point average roughness of the surface of the copper-based material substrate is exemplified as a range of 0.0001 μm to 14 μm, preferably a range of 0.001 μm to 12 μm, and more preferably a range of 0.01 μm to 10 μm. In addition, the ten-point average roughness (Rzjis) can be measured according to JIS B0601:2001.
[0082] The thickness of the copper-based material substrate in the form of a sheet is not particularly limited and can be appropriately selected according to the purpose, etc., and is usually preferably 0.5 μm to 1000 μm, and more preferably 1 μm to 100 μm. In addition, the bonding area between the copper-based material substrate and the resin substrate is not particularly limited and can be appropriately selected according to the purpose, etc.
[0083] [2-2. Layer of resin adhesive]
[0084] The amount of the resin adhesive layer, i.e., the layer containing one or both of the Maillard reaction product (C) and the caramelization reaction product (D), per unit area is not particularly limited as long as the desired adhesion is obtained, but is preferably 0.1 mg / m 2 ~3000mg / m 2 , more preferably 0.5 mg / m 2 ~2000mg / m 2 , more preferably 0.5 mg / m 2 ~1500 mg / m 2 , and more preferably 0.5 mg / m 2 ~1000 mg / m 2 , and more preferably 0.5 mg / m 2 ~700 mg / m 2 , particularly preferably 0.5 mg / m 2 ~600 mg / m 2 , the most preferred is 0.5 mg / m 2 ~500 mg / m 2 .
[0085] In addition, the adhesion amount of the layer of the resin adhesive is the adhesion amount per single side (1 layer). The adhesion amount of the layer of the resin adhesive can be measured indirectly by adding an element not contained in the adhesive to the adhesive using fluorescent X-ray analysis (XRF). Specifically, a compound (hereinafter referred to as compound β) having a known amount of an element not contained in the adhesive (hereinafter referred to as element α) is added to the adhesive in a specific ratio, and a method of calculating the adhesion amount per unit area of the layer of the adhesive using fluorescent X-ray analysis according to the adhesion amount of the known amount of element α per unit area. As the ratio of compound β to the addition amount of the adhesive, for example, 5% to 40% by mass can be cited relative to the total solid content. As the content rate of element α in compound β, for example, 30% to 80% can be cited in terms of mass conversion. As compound β is not particularly limited, for example, ammonium zirconium carbonate can be cited, in which case element α can be set to Zr. In addition, compound β can also be used in the state of an aqueous solution.
[0086] The thickness of the resin adhesive layer is not particularly limited and can be appropriately selected so that the adhesion amount is within the above range. It is preferably 0.5 nm to 3000 nm, more preferably 0.5 nm to 2000 nm, further more preferably 0.5 nm to 1500 nm, particularly preferably 0.5 nm to 1000 nm, and most preferably 0.5 nm to 700 nm.
[0087] [2-3. Resin base material]
[0088] The resin substrate can be any substrate containing resin. Therefore, the resin substrate can be composed only of resin or contain components other than resin. In the case where the resin substrate contains components other than resin, the resin can be set as the main component (resin concentration is 50% by mass or more), or the resin can not be set as the main component. As components other than resin, inorganic fibers such as carbon fiber and glass fiber can be cited. As a resin substrate containing components other than resin, for example, a substrate impregnated with resin or resin composition in inorganic fibers (which can be set in the form of woven or non-woven fabrics) can be cited, typically prepreg. The resin substrate can typically be provided in the form of sheets such as films and prepregs. The sheet can be composed of a single layer or can be composed of two or more layers stacked. In addition, the sheet can be soft (prepreg) or hard (rigid). The resin contained in the resin substrate can be one or a mixture of two or more resins. In addition, the resin substrate can contain inorganic particles (fillers), various other additives, etc. as needed. In addition, the components other than the resin that the resin substrate can contain are not particularly limited, and components other than the above can also be used.
[0089] The resin contained in the resin base material is not particularly limited and can be appropriately selected depending on the intended use, but a thermoplastic resin can be preferably used.
[0090] In addition, a resin having a relative dielectric constant of 5.0 or less at a temperature of 25°C and 10 GHz is preferred, a resin having a relative dielectric constant of 4.0 or less is more preferred, and a resin having a relative dielectric constant of 3.5 or less is further preferred. Typically, a resin having a relative dielectric constant of more than 1.0 to 5.0, more typically 1.1 to 5.0, at a temperature of 25°C and 10 GHz can be used. The relative dielectric constant of the resin can be measured by the cavity resonator method according to JIS C2565:1992.
[0091] As the resin, specifically, fluororesins such as polytetrafluoroethylene (PTFE), perfluoroalkoxy fluororesin (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, liquid crystal polymer (LCP), aromatic polyetherketones such as polyetheretherketone (PEEK), polyphenylene ether (PPE), epoxy resin, bismaleimide triazine resin, cycloolefin polymer, polyimide, etc. are listed. Among them, PEEK and fluororesins (such as PTFE, PFA, FEP, ETFE, ECTFE, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, etc.) are preferred, fluororesins are more preferred, and PTFE is particularly preferred.
[0092] As the resin base material, a resin film or prepreg commercially available as a resin base material for a printed wiring board can be used.
[0093] When the resin substrate is in the form of a sheet, the thickness is not particularly limited and may be appropriately selected depending on the intended use, but is usually preferably 10 μm to 1000 μm, and more preferably 20 μm to 500 μm.
[0094] [2-4. Method for producing laminate]
[0095] The laminate of one embodiment of the present invention is typically a copper-clad laminate, which can be manufactured by sandwiching a copper-based material substrate and a resin substrate with the above-mentioned resin adhesive, preferably by forming a layer of resin adhesive on the surface of the copper-based material substrate, and then bonding the resin substrate on the layer of the resin adhesive. The resin adhesive can be provided in the form of a liquid or in the form of a sheet (e.g., a sheet-like hot melt adhesive). When the resin adhesive is in a liquid form, as described later, a method of bonding the resin substrate on the layer of the resin adhesive can be cited after forming a layer of resin adhesive on the surface of the copper-based material substrate. When the resin adhesive is in the form of a sheet, a method of bonding by sandwiching a sheet-like adhesive between the copper-based material substrate and the resin substrate can be cited. The preferred manufacturing method of the laminate of one embodiment of the present invention is exemplarily described below, but the manufacturing method of the laminate is not limited to the following method.
[0096] First, on a copper-based material substrate, typically a copper-based material sheet such as copper foil, copper plate, copper alloy foil or copper alloy plate (which may also be subjected to the surface treatment as described above), or in the case of using a laminate having a copper-based material substrate on the surface, a layer of a resin adhesive is formed on the copper-based material substrate (which may also be subjected to the surface treatment as described above).
[0097] The layer of the resin adhesive can be formed by, for example, dissolving or dispersing a resin adhesive containing one or both of the Maillard reaction product (C) and the caramelization reaction product (D) in a solvent (e.g., water) to prepare an adhesive for forming the layer of the resin adhesive, applying the adhesive to the surface of the copper-based material substrate, and then drying the adhesive.
[0098] The content of each compound in the adhesive liquid is not particularly limited and can be appropriately selected.
[0099] The solvent used in the adhesive liquid is not particularly limited, and can be appropriately selected from commonly used solvents. An organic solvent may be used, but water is generally preferred. Two or more solvents may be used in combination.
[0100] In the adhesive liquid, various commonly used additives may be added as needed, for example, inorganic compounds or organic compounds such as resins (for example, acrylic resins, epoxy resins, urethane resins, ether resins, amide resins, olefin-vinyl acetate copolymers, polyvinyl alcohol, polyalkylene glycol, styrene-maleic anhydride copolymers, oxidatively modified polyolefin resins, thickening polysaccharides, and cellulose nanofibers, etc., which are commonly used as adhesives), surfactants, defoamers, leveling agents, antibacterial and antifungal agents, dyes, pigments, fragrances, anti-adhesive agents, release agents, rust inhibitors, etc., or they may not be added.
[0101] The application of the adhesive liquid is not particularly limited and can be carried out by a known method, for example, bar coating, spray coating, spin coating, roll coating, curtain coating, electrostatic powder coating, flow dip coating, dipping, etc.
[0102] The drying conditions after the adhesive liquid is applied are not particularly limited and can be appropriately selected, but it is generally preferred to heat and dry the copper-based material substrate in a manner such that the maximum temperature (PMT) thereof is 60°C to 300°C. The drying temperature is not particularly limited as long as the adhesive liquid can be dried to form a layer of the resin adhesive, but the maximum temperature (PMT) thereof is more preferably in the range of 60°C to 250°C, and particularly preferably in the range of 60°C to 200°C. The drying time is not particularly limited as long as the adhesive liquid can be dried to form a layer of the resin adhesive, but for example, it can be 1 minute or more, 5 minutes or more, 10 minutes or more, 30 minutes or more, and can also be within 180 minutes, within 120 minutes, or within 60 minutes.
[0103] In addition, before forming the resin adhesive layer, the copper-based material substrate may be subjected to cleaning treatment such as acid degreasing, alkali degreasing, acid cleaning, alkali cleaning, water cleaning, etc., and drying after the cleaning treatment, etc. The cleaning treatment and drying can be performed according to known methods.
[0104] Then, on the layer of resin adhesive formed on the surface of the copper-based material substrate in this way, the laminate of the present embodiment can be manufactured by overlapping the resin substrate, typically a resin sheet such as a resin film or a prepreg, and heating, pressurizing, and bonding. In the case of manufacturing a laminate in which a copper-based material substrate is laminated on both sides of a resin substrate, the copper-based material substrate can also be bonded to both sides of a resin substrate such as a resin film or a prepreg at the same time through a layer of resin adhesive, or it can be bonded to each single side in sequence.
[0105] There is no particular limitation on the method of bonding the copper-based material substrate having a layer of resin adhesive on the surface to the resin film or prepreg, and the like, and the bonding can be performed using a known heating-pressing device. There is no particular limitation on the pressing conditions and heating conditions, and they can be appropriately selected according to the material used, the type of resin, etc. For example, the pressing pressure can be 1 kgf / cm 2 ~1000kgf / cm 2 The pressing time can be 0.1 minutes to 1440 minutes, the pressing temperature can be 80°C to 600°C, and the typical pressing pressure can be 5kgf / cm 2 ~100kgf / cm 2 The pressing time can be 0.5 minutes to 600 minutes or less, and the pressing temperature can be 120°C to 450°C.
[0106] During the heating and pressurization, the heating and pressurization may be performed by reducing the pressure from normal pressure. [Example]
[0107] Hereinafter, the present invention will be described in further detail by way of examples and comparative examples. In addition, the present invention is not limited to the following examples.
[0108] <1. Production of Maillard Reaction Product (C) and Caramelization Reaction Product (D)>
[0109] As the raw materials of the Maillard reaction product (C), the following sugars (A) or reducing ketones (B) and amine compounds (G) or amine equivalents (H) are used, and as the raw materials of the caramelization reaction product (D), the following sugars (A) or reducing ketones (B) are used. In addition, as an additive during the reaction, the following additive (I) is used. Unless otherwise specified, the sugars (A), reducing ketones (B), amine compounds (G), amine equivalents (H) and additives (I) are those manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0110] [Sugars (A)]
[0111] (A-1) Dihydroxyacetone (monosaccharide / ketose / triose)
[0112] (A-2) Xylose (monosaccharide / aldose / pentose)
[0113] (A-3) Arabinose (monosaccharide / aldose / pentose)
[0114] (A-4) Glucose (monosaccharide / aldose / hexose)
[0115] (A-5) Fructose (monosaccharide / ketose / hexose)
[0116] (A-6) Maltose (disaccharide)
[0117] (A-7) Gluconic acid (50 mass % aqueous solution) (saccharic acid)
[0118] (A-8) Pullulan (manufactured by Hayashihara Co., Ltd.) (polysaccharide)
[0119] (A-9) Selogen 5A (registered trademark) (sodium salt of carboxymethyl cellulose) (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) (polysaccharide)
[0120] (A-10) Gum arabic (manufactured by Sumitomo Pharma & Food Chemicals, Ltd.) (polysaccharide)
[0121] (A-11) Sorbitol (sugar alcohol)
[0122] [Reduced ketones (B)]
[0123] (B-1) Ascorbic acid (reduced ketone)
[0124] (B-2) Sodium ascorbate (salt of reduced ketone)
[0125] [Amine compound (G)]
[0126] (G-1) Ammonia water (28.0 to 30.0 mass%)
[0127] (G-2)Dibutylamine
[0128] (G-3)Aniline
[0129] (G-4) Trimethylenetetramine
[0130] (G-5) Epomin (registered trademark) P-1000 (manufactured by Nippon Catalyst Co., Ltd.)
[0131] (G-6) Ammonium chloride
[0132] (G-7) Ammonium Nitrate
[0133] (G-8) Glycine
[0134] (G-9) L-Asparagine Monohydrate
[0135] (G-10) 3-Amino-1H-1,2,4-triazole
[0136] (G-11) 3,5-Diamino-1H-1,2,4-triazole
[0137] (G-12) Ammonium peroxodisulfate
[0138] [Amine equivalent (H)]
[0139] (H-1) Urea
[0140] (H-2)Thiourea
[0141] [Additive (I)]
[0142] (I-1) 30% by mass hydrogen peroxide solution
[0143] (I-2) 35 mass% hydrochloric acid
[0144] (I-3) 50 mass% sodium hydroxide aqueous solution
[0145] [Maillard reaction product (C) production conditions]
[0146] [Manufacturing condition 1: C-1 to C-16, C-18 to C-36]
[0147] According to the formula shown in Table 1 and Table 2, ion exchange water is mixed with sugar (A) or reductone (B), and amine compound (G) or amine equivalent (H) to prepare an aqueous solution. For the Maillard reaction product (C-13, C-23 to C-25) using additives, the additive is added at this stage. The pH of the aqueous solution at room temperature at this time is shown in Table 1 and Table 2. Then, the aqueous solution before the above reaction is placed in a 100 mL polypropylene container and sealed, and the liquid temperature is set to 95°C in a circulating hot air drying furnace, and heated for the time shown in Table 1 and Table 2 to prepare a solution containing the Maillard reaction product (C). The manufactured Maillard reaction products are respectively designated as C-1 to C-16 and C-18 to C-36. Whether the Maillard reaction product is generated is determined by the above method using a spectrophotometer (SD7000) manufactured by Nippon Denshoku Industries Co., Ltd., by whether a brown substance is generated. In the case where a brown substance is generated, it is recorded as "yes" in Table 1 and Table 2. The same applies to the following manufacturing examples.
[0148] [Manufacturing condition 2: C-17]
[0149] According to the formula shown in Table 1, ion exchange water, reductone (B-1) and 30% by mass of ammonia water (G-1) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed to prepare an aqueous solution. The pH of the aqueous solution at room temperature is shown in Table 1. The aqueous solution and the stirrer chip were placed in a 100 mL glass beaker, and the liquid temperature was set to 90°C and heated and stirred for 8 hours to prepare a solution containing a Maillard reaction product (C). The manufactured Maillard reaction product was set to C-17.
[0150] [Caramelization reaction product (D) production conditions]
[0151] [Manufacturing Condition 3: D-1 to D-8]
[0152] According to the formula shown in Table 3, ion exchange water and sugar (A) are mixed to prepare an aqueous solution. For the caramelization reaction products (D-6 to D-8) using additives, the additives are added at this stage. The pH of the aqueous solution at room temperature at this time is shown in Table 3. Then, the aqueous solution before the above reaction is placed in a 100 mL polypropylene container and sealed, and the liquid temperature is set to 95°C in a circulating hot air drying furnace, and heated for the time shown in Table 3 to prepare a solution containing a caramelization reaction product (D). The manufactured caramelization reaction products are respectively set as D-1 to D-8. Whether a caramelization reaction product is generated is determined by the above method using a spectrophotometer (SD7000) manufactured by Nippon Denshoku Industries Co., Ltd., and whether a brown substance is generated. In the case of generating a brown substance, it is recorded as "yes" in Table 3. The following manufacturing examples are also the same.
[0153] [Manufacturing condition 4: D-9 to D-10]
[0154] According to the formula shown in Table 3, ion exchange water and reductone (B) were mixed to prepare an aqueous solution. The pH of the aqueous solution at room temperature is shown in Table 3. The aqueous solution and the stirrer chip were placed in a 100 mL glass beaker, and the liquid temperature was set to 90°C and heated and stirred for 8 hours to prepare a solution containing a caramelization reaction product (D). Thus, the Maillard reaction products D-9 to D-10 were prepared.
[0155] Table 1
[0156]
[0157] Table 2
[0158]
[0159] Table 3
[0160]
[0161] <2. Manufacturing of Copper Clad Laminates>
[0162] [Formation of Resin Adhesive Layer]
[0163] [Example 1]
[0164] As a copper-based material substrate, an electrolytic copper foil (thickness 18 μm, Rzjis 0.14 μm, Ra 0.05 μm) (K-1) having a heat-resistant plating layer and an electrolytic chromate layer in order from the outside to the inside was prepared. The solid content concentration of the Maillard reaction product (C-1) was adjusted by ion exchange water and applied (bar coating method) to one surface of the copper foil so that the adhesion amount of the adhesive layer formed on the copper foil surface was 12 mg / m 2 Then, the copper foil was dried at 100° C. for 1 minute in a circulating hot air drying oven to form an adhesive layer on the surface of the copper foil.
[0165] [Bonding of Copper Foil with Adhesive Layer and Resin Base Material]
[0166] The surface of the adhesive layer in the copper foil formed with the adhesive layer was bonded with a PTFE prepreg (manufactured by Rogers Company, trade name "RO3003 Bondply", thickness 0.1 mm) (L-1), and then covered with aluminum foil, and bonded in a state isolated from the atmosphere to produce a copper-clad laminate. The bonding condition was a pressing pressure of 30 kgf / cm 2 The pressing time is 45 minutes and the pressing temperature is 370°C.
[0167] [Examples 2 to 67]
[0168] In Examples 2 to 67, the adhesive (Maillard reaction products (C-2 to C-36)) shown in Table 4, caramelization reaction products (D-1 to D-10) and commercially available caramel pigments (J-1 to J-3 shown below) were used, and the concentration of the solid content was adjusted by ion exchange water so that the adhesive layer formed on the copper foil surface became the adhesion amount shown in Table 4, and was applied (bar coating method) to one surface of the copper-based material substrate (K-1 to K-3 shown below) shown in Table 4. The adhesive layer was formed by the same method as in Example 1. Then, the resin substrate (L-1 to L-3 shown below) shown in Table 4 was used, and the copper-clad laminate was manufactured by the same method as in Example 1 except that the adhesive was bonded under the conditions of the pressing time and pressing temperature shown in Table 4.
[0169] [Caramel Color]
[0170] (J-1) Commercially available caramel color, Caramel I
[0171] (J-2) Commercially available caramel color, Caramel III
[0172] (J-3) Commercially available caramel color, Caramel IV
[0173] [Copper-based material substrate]
[0174] (K-1) Electrolytic copper foil having a heat-resistant plating layer and an electrolytic chromate layer in order from the outside to the inside (thickness 18 μm, Rzjis 0.14 μm, Ra 0.05 μm)
[0175] (K-2) Electrolytic copper foil with heat-resistant plating layer (thickness 18 μm, Rzjis 1.05 μm, Ra 0.20 μm)
[0176] (K-3) Electrolytic copper foil (thickness 18 μm, Rzjis 0.89 μm, Ra 0.17 μm)
[0177] [Resin base material]
[0178] (L-1) PTFE prepreg (manufactured by Rogers Corporation, trade name "RO3003 Bondply", thickness 0.1 mm) (relative dielectric constant at 10 GHz: 3.0±0.04, dielectric loss tangent: 0.0010)
[0179] (L-2) ETFE sheet (manufactured by ASONE Co., Ltd., thickness 0.05 mm) (relative dielectric constant at 10 GHz: 2.6, dielectric loss tangent: 0.0150)
[0180] (L-3) PEEK is a prepreg (thickness 0.05 mm) (relative dielectric constant at 10 GHz is 3.1, dielectric loss tangent is 0.0033)
[0181] [Comparative Examples 1 to 4]
[0182] A copper-clad laminate was produced in the same manner as in Example 1 except that an aqueous solution of the sugars (A-4, A-5, A-8) or the reducing ketone (B-1) shown in Table 5 was used to form the adhesive layer.
[0183] [Comparative Example 5, Comparative Examples 7-8, Comparative Example 16, Comparative Example 21, Comparative Example 26]
[0184] No adhesive layer is formed, and a copper-clad laminate is manufactured by the same method as in Example 1, using a resin substrate (L-1 to L-3) shown in Table 5 or a material substrate other than a resin (O-1 to O-3 shown below), and bonding is performed under the conditions of pressing time and pressing temperature shown in Table 5.
[0185] [Comparative Example 6]
[0186] A copper-clad laminate was produced in the same manner as in Example 1 except that the copper-based material substrate (M-1) shown below was used and no adhesive layer was formed and bonding was performed under the conditions of the pressing time and pressing temperature shown in Table 5.
[0187] (M-1) Electrolytic copper foil having, from the outside to the inside, an adhesive layer of a silane coupling agent, a heat-resistant plating layer, and an electrolytic chromate layer (thickness 18 μm, Rzjis 1.77 μm, Ra 0.19 μm)
[0188] [Comparative Examples 9 to 15, Comparative Examples 17 to 20, Comparative Examples 22 to 25, Comparative Examples 27 to 30]
[0189] The adhesive shown in Table 5 (Maillard reaction product (C-4, C-17), caramelization reaction product (D-1), commercially available caramel pigment (J-2)) or commercially available water-based resin (N-1 to N-7 shown below) was used, and the solid content concentration was adjusted by ion exchange water so that the adhesive layer formed on the copper foil surface had an adhesion amount shown in Table 5. The adhesive layer was formed in the same manner as in Example 1. Then, a copper-clad laminate was manufactured in the same manner as in Example 1, except that the resin substrate (L-1 to L-3) shown in Table 5 or a material substrate other than resin (O-1 to O-3 shown below) was used and the pressing time and pressing temperature conditions shown in Table 5 were used for bonding.
[0190] [Water-based resin]
[0191] (N-1) Modepix (registered trademark) 302 (manufactured by Arakawa Chemical Industries, Ltd.) (epoxy resin)
[0192] (N-2) Gosenex (registered trademark) LW-100 (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) (sulfonated PVOH)
[0193] (N-3) ARROWBASE (registered trademark) YA-6010 (manufactured by UNITIKA Co., Ltd.) (modified polypropylene)
[0194] (N-4) PITZCOL (registered trademark) V-7154 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) (PVP / PVA)
[0195] (N-5) Aqualic (registered trademark) HL415 (manufactured by Nippon Catalyst Co., Ltd.) (polyacrylic acid)
[0196] (N-6) BONKOTE (registered trademark) CF-6140 (manufactured by DIC Corporation) (acrylic resin)
[0197] (N-7) ELITEL (registered trademark) KT-507 (manufactured by UNITIKA Co., Ltd.) (ester resin)
[0198] [Material base material other than resin]
[0199] (O-1) Fiberglass cloth
[0200] (O-2) SUS foil (manufactured by ASONE Co., Ltd., thickness 0.1 mm)
[0201] (O-3) Aluminum foil (manufactured by MA Aluminum Co., Ltd., thickness 12 μm)
[0202] The glass fiber cloth (O-1) was prepared by placing an epoxy resin prepreg (manufactured by Showa Denko Materials Co., Ltd., trade name "GEA-679N") in chloroform heated to 60°C to completely dissolve the epoxy resin, and then taking out only the glass fiber cloth. The prepreg was immersed in another chloroform heated to 60°C to remove the remaining epoxy resin, and then dried in a circulation drying oven at 80°C for 1 minute.
[0203] [Ten-point average roughness of copper foil surface (Rzjis)]
[0204] The ten-point average roughness (Rzjis) and the arithmetic mean roughness (Ra) of the surface of the copper foil bonded to the resin were measured using a laser microscope (VK-8701 manufactured by KEYENCE CORPORATION) in accordance with JIS B0601:2001.
[0205] [Amount of Adhesive Layer Adhered to Copper Foil Having Adhesive Layer Formed]
[0206] The adhesion amount of the adhesive layer is determined by the following method. A predetermined amount of ammonium zirconium carbonate aqueous solution is added to a Maillard reaction product (C-1) of known solid content concentration to prepare a coating treatment agent for measuring the adhesion amount. At this time, the solid content ratio of ammonium zirconium carbonate to the total solid content is set to 15% by mass. Next, the prepared coating treatment agent is used to form a coating film on an electrolytic copper foil (K-1) as a copper-based material substrate by a rod coating method, and then dried at 100°C for 1 minute in a circulating hot air drying furnace to form a dry coating film. The copper foil formed with the above-mentioned dry coating film is cut into 4 cm wide × 4 cm long as a measurement sample, and analyzed by a fluorescent X-ray analyzer (ZSX PrimusII manufactured by Rigaku Co., Ltd.) to determine the zirconium adhesion amount per unit area. Based on the result, the adhesion amount per unit area of the entire dry coating film in a known solid content concentration can be calculated. Therefore, without changing the type of rod coating, the above operation is performed at multiple solid content concentrations to prepare a biaxial diagram (calibration curve) with solid content concentration and adhesion amount as axes. Target adhesion amount In the above-mentioned biaxial graph, the interval of the value interpolated to the actually measured adhesion amount is confirmed, and the solid content concentration according to the target adhesion amount is calculated. A Maillard reaction product (C-1) with a known solid content concentration without adding an aqueous zirconium carbonate ammonium solution is used to prepare a copper-clad laminate for adhesion evaluation having an adhesive layer with a target adhesion amount. In the same way as the above method, for each adhesive (C-2 to C-36, D-1 to D-10, J-1 to J-3 and N-1 to N-7), the relationship between the solid content concentration and the adhesion amount is determined, and the solid content concentration is adjusted so that the adhesive layer formed on the surface of the copper foil has the adhesion amount shown in Tables 4 and 5. In addition, the relationship between the solid content concentration and the adhesion amount is determined according to the combination of each set of adhesives (C-2 to C-36, D-1 to D-10, J-1 to J-3 and N-1 to N-7) and electrolytic copper foil (K-1, K-2 or K-3) shown in Tables 4 and 5.
[0207] <3. Adhesion Evaluation>
[0208] The copper-clad laminates prepared in the above-mentioned embodiments and comparative examples were cut into 0.3 cm wide × 7 cm long, and the peeling strength (peel strength) of the copper foil in the 90° direction was measured according to JIS C5012:1993, and the adhesion was evaluated according to the following evaluation criteria. In addition, in this evaluation, the evaluation with a score of 2 points or less was regarded as poor adhesion. The results are shown in Tables 4 and 5.
[0209] [Evaluation criteria: peel strength]
[0210] 1 point: 0 N / cm or more but less than 1.0 N / cm
[0211] 2 points: 1.0 N / cm or more but less than 2.5 N / cm
[0212] 3 points: 2.5 N / cm or more but less than 5.0 N / cm
[0213] 4 points: 5.0 N / cm or more but less than 7.5 N / cm
[0214] 5 points: 7.5 N / cm or more but less than 10.0 N / cm
[0215] 6 points: 10.0 N / cm or more.
[0216] Table 4
[0217]
[0218]
[0219] Table 5
[0220]
Claims
1. A resin adhesive, comprising one or two selected from a Maillard reaction product (C) and a caramelization reaction product (D), wherein the Maillard reaction product (C) is obtained using a saccharide (A) and / or a reductone (B), and an amine compound (G) as raw materials, and the caramelization reaction product (D) is obtained using a saccharide (A) and / or a reductone (B) as raw materials.
2. A laminate comprising a copper-based material substrate, a layer of the adhesive for resin according to claim 1, and a resin substrate in this order.
3. A resin adhesive, comprising one or two selected from a Maillard reaction product (C) and a caramelization reaction product (D), wherein the Maillard reaction product (C) is obtained using sugars (A) and / or reductones (B), and an amine compound (G) and / or an amine equivalent (H) as raw materials, and the caramelization reaction product (D) is obtained using sugars (A) and / or reductones (B) as raw materials.
4. A laminate comprising a copper-based material substrate, a layer of the adhesive for resin according to claim 3, and a resin substrate in this order.
Citation Information