Anti-reflective film, method for manufacturing same, and

By using transparent film substrate, hard coating and anti-reflective layer in the anti-reflective film, and using roll-to-roll sputtering film formation technology to heat the cracks of the anti-reflective film under high temperature or high temperature and high humidity, the cracks of the anti-reflective film are solved. Problem, it significantly improves its flexural resistance and visibility.

CN119096168APending Publication Date: 2024-12-06NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035774.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-27
Filing Date
2023-04-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing anti-reflective films are prone to cracks in bending states under high temperature or high temperature and high humidity environments, resulting in a decrease in visibility of the display.

Method used

The combined structure of transparent film substrate, hard coating and anti-reflective layer is adopted, and the heat treatment is carried out at high temperature through roll-to-roll sputtering film formation technology, so as to control the dimensional change rate of the laminated body within a specific range, and increase the anti-reflective film. Heat resistance and humidity resistance.

Benefits of technology

The anti-reflective film is not prone to cracks when bending under high temperature or high temperature and high humidity, which significantly improves its bending resistance and ensures the visibility and stability of the display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096168A_ABST
    Figure CN119096168A_ABST
Patent Text Reader

Abstract

An anti-reflection film (10) has a transparent film substrate (11), a hard coat layer (12), and an anti-reflection layer (13) in this order. It is preferable that the dimensional change rate of the antireflection film (10) in the first direction before and after the heat resistance test be-0.10% or more and 0.10% or less. It is also preferable that the dimensional change rate of the antireflection film (10) in the first direction before and after the wet heat resistance test is 0.01% or more and 0.20% or less. The transparent film substrate (11) is preferably a polyethylene terephthalate film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an anti-reflection film and a method for manufacturing the same, and an image display device. Background Art

[0002] An anti-reflection film is arranged on the visible side of image display devices such as liquid crystal displays and organic EL displays to prevent image quality degradation caused by reflection of outdoor light and to improve contrast. The anti-reflection film has an anti-reflection layer composed of a laminate of multiple thin films with different refractive indices on a transparent film substrate.

[0003] For example, Patent Document 1 discloses an antireflection film having a SiO primer layer on a hard coating film, and an antireflection layer on the SiO primer layer, wherein the antireflection layer includes niobium oxide (NbO) as a high refractive index layer. 2 O 5 ) layer and the silicon oxide (SiO 2 ) layers in an alternating stack.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-47876 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In recent years, a bendable image display device (foldable display) having an organic EL panel using a bendable substrate (flexible substrate) such as a resin film has been put into practical use. As a cover window of the foldable display, an anti-reflection film having an anti-reflection layer provided on a flexible substrate is used.

[0009] Foldable displays are usually stored in a folded state. In the folded state, compressive stress is applied to the inner side of the folded portion (bend portion), and tensile stress is applied to the outer side of the bend portion. If the display is folded with the display surface as the inner side, the anti-reflection film is in a folded state (bend state) with the surface formed by the anti-reflection layer as the inner side. If the display is stored in a bent state at high temperature or high temperature and high humidity, fine cracks may occur in the anti-reflection layer, which may cause the visibility of the display to decrease.

[0010] In view of the above, an object of the present invention is to provide an anti-reflection film and a method for manufacturing the same, as well as an image display device using the anti-reflection film, wherein the anti-reflection film is not prone to cracking in the anti-reflection layer even when stored in a bent state at high temperature or high temperature and high humidity, and has excellent bending resistance.

[0011] Solutions for solving problems

[0012] <Aspects of the present invention>

[0013] The present invention includes the following aspects.

[0014] [1] An antireflection film comprising, in order: a transparent film substrate, a hard coat layer, and an antireflection layer, wherein when subjected to a heat resistance test in an environment at a temperature of 85° C. for 48 hours, the dimensional change rate in the direction of any one side before and after the heat resistance test is not less than −0.10% and not more than 0.10%.

[0015] [2] The antireflection film according to [1], wherein the dimensional change rate in a direction perpendicular to the side direction before and after the heat resistance test is -0.10% to 0.10%.

[0016] [3] An antireflection film comprising, in order: a transparent film substrate, a hard coating layer, and an antireflection layer, wherein when subjected to a moisture and heat resistance test at a temperature of 60° C. and a relative humidity of 95% for 48 hours, the dimensional change rate in the direction of any one side before and after the moisture and heat resistance test is greater than or equal to 0.01% and less than or equal to 0.20%.

[0017] [4] The antireflection film according to [3], wherein the dimensional change rate in a direction perpendicular to the side direction before and after the moisture and heat resistance test is 0.01% or more and 0.20% or less.

[0018] [5] The antireflection film according to any one of [1] to [4], wherein the transparent film substrate is a polyethylene terephthalate film.

[0019] [6] The antireflection film according to any one of [1] to [5], wherein the thickness of the antireflection layer is 150 nm to 280 nm.

[0020] [7] The antireflection film according to any one of [1] to [6], further comprising: a primer layer disposed between the hard coat layer and the antireflection layer.

[0021] [8] The antireflection film according to any one of [1] to [7], further comprising an antifouling layer disposed on a side of the antireflection layer opposite to the hard coat layer.

[0022] [9] The antireflection film according to any one of [1] to [8], further comprising: a pressure-sensitive adhesive layer disposed on the side of the transparent film substrate opposite to the hard coat layer.

[0023]

[10] An image display device comprising: an image display panel; and the antireflection film according to any one of [1] to [9], arranged on a visible side of the image display panel.

[0024]

[11] A method for manufacturing an anti-reflection film, which is the method for manufacturing an anti-reflection film as described in any one of [1] to [9], comprising: a step Sa, forming the anti-reflection layer on the side of the hard coating layer opposite to the transparent film substrate side using a roll-to-roll sputtering film forming device; and a step Sb, after the step Sa, heating the stacked body formed with the anti-reflection layer.

[0025]

[12] The method for producing an antireflection film according to

[11] , wherein in the step Sb, the laminate is heated at a temperature of 110° C. or higher.

[0026] Effects of the Invention

[0027] According to the present invention, an antireflection film and a method for manufacturing the same, as well as an image display device using the antireflection film, can be provided, wherein the antireflection film is not prone to cracking in the antireflection layer even when stored in a bent state at high temperature or high temperature and high humidity, and has excellent bending resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a cross-sectional view showing an example of the antireflection film of the present invention.

[0029] Figure 2 It is a cross-sectional view showing another example of the antireflection film of the present invention.

[0030] Figure 3 It is a cross-sectional view showing an example of the image display device of the present invention.

[0031] Figure 4 It is a cross-sectional view showing a bent state of a test piece when evaluating the bending resistance of an antireflection film. DETAILED DESCRIPTION

[0032] Hereinafter, a preferred embodiment of the present invention will be described. First, the terms used in this specification will be described. "Refractive index" is the refractive index of light of a wavelength of 550nm in an atmosphere at a temperature of 23°C. The "main surface" of a layered object (more specifically, a transparent film substrate, a hard coating layer, an adhesive layer, etc.) refers to a surface orthogonal to the thickness direction of the layered object. The numerical value of the thickness (film thickness) of each layer constituting the anti-reflection film is the arithmetic mean of 10 measurement values ​​obtained by randomly selecting 10 measurement locations from the image of the cross section obtained by cutting the layer along the thickness direction, and measuring the thickness of the selected 10 measurement locations.

[0033] "The direction of any one side" means a direction parallel to any one of the four sides of the antireflection film of a rectangle or a square. Hereinafter, the direction of any one side of the antireflection film may sometimes be referred to as the "first direction". In addition, the direction orthogonal to the first direction (specifically, the direction parallel to the side orthogonal to the first direction among the above four sides) may sometimes be referred to as the "second direction". The first direction is, for example, the film conveyance direction when forming the antireflection layer by a sputtering method in a roll to roll manner (hereinafter sometimes referred to as the "MD direction"). The second direction is, for example, the direction orthogonal to the film conveyance direction when forming the antireflection layer by a sputtering method in a roll to roll manner (hereinafter sometimes referred to as the "TD direction").

[0034] Hereinafter, sometimes the suffix "series" is added after the compound name to collectively refer to the compound and its derivatives. In addition, when the suffix "series" is added after the compound name to indicate a polymer name, it means that the repeating unit of the polymer is derived from the compound or its derivatives. The components, functional groups, etc. exemplified in this specification can be used alone or in combination of two or more unless otherwise specified.

[0035] In order to facilitate understanding, the drawings referred to in the following description schematically show each constituent element in the main body, and the size, number, shape, etc. of each constituent element shown in the drawings may sometimes be different from the actual ones for the convenience of making the drawings. In addition, for the convenience of explanation, in the drawings described later, the same constituent parts as those in the drawings described before are given the same reference numerals and their descriptions are omitted.

[0036] <First Embodiment: Antireflection Film>

[0037] Hereinafter, as specific examples of the antireflection film according to the first embodiment of the present invention, the antireflection film ARF1 and the antireflection film ARF2 will be described. Both the antireflection film ARF1 and the antireflection film ARF2 are antireflection films (laminates) having a transparent film substrate, a hard coat layer, and an antireflection layer in this order. For the antireflection film ARF1, when a heat resistance test is carried out in an environment at a temperature of 85°C for 48 hours, the dimensional change rate in the first direction before and after the heat resistance test is -0.10% or more and 0.10% or less. For the antireflection film ARF2, when a damp heat resistance test is carried out in an environment at a temperature of 60°C and a relative humidity of 95% for 48 hours, the dimensional change rate in the first direction before and after the damp heat resistance test is 0.01% or more and 0.20% or less.

[0038] The shrinkage of the antireflection film ARF1 in the first direction is suppressed at high temperature, so even if it is stored in a bent state at high temperature, cracks are not easily generated in the antireflection layer, and the bending resistance is excellent. In addition, the shrinkage of the antireflection film ARF2 in the first direction is suppressed at high temperature and high humidity, so even if it is stored in a bent state at high temperature and high humidity, cracks are not easily generated in the antireflection layer, and the bending resistance is excellent. Hereinafter, the antireflection film ARF1 and the antireflection film ARF2 will each be described as "antireflection film ARF" when no distinction is required. In addition, the property that cracks are not easily generated in the antireflection layer even if it is stored in a bent state at high temperature is sometimes abbreviated as "bending resistance at high temperature". In addition, the property that cracks are not easily generated in the antireflection layer even if it is stored in a bent state at high temperature and high humidity is sometimes abbreviated as "bending resistance at high temperature and high humidity".

[0039] In the following, high temperature or high temperature and high humidity is sometimes described as "harsh environment". In addition, the property that cracks are not easily generated in the anti-reflection layer even when stored in a bent state under a harsh environment is sometimes referred to as "bending resistance under harsh environment". In addition, a heat resistance test of an anti-reflection film kept at a temperature of 85°C for 48 hours is sometimes referred to as "heat resistance test". In addition, a moisture and heat resistance test of an anti-reflection film kept at a temperature of 60°C and a relative humidity of 95% for 48 hours is sometimes referred to as "moisture and heat resistance test". In addition, a heat resistance test or a moisture and heat resistance test is sometimes described as a "harsh environment test". In the following, unless otherwise specified, a "harsh environment test" is a test on an anti-reflection film.

[0040] In addition, the relative humidity of the atmosphere in the heat resistance test is, for example, 1% or less, and may be 0.5% or less, or 0.1% or less.

[0041] When the length in the first direction or the second direction before the harsh environment test is set to L1 (unit: mm), and the length in the first direction or the second direction after the harsh environment test is set to L2 (unit: mm), the dimensional change rate (unit: %) in the first direction or the second direction before and after the harsh environment test is calculated according to the formula "dimensional change rate = 100×(L2-L1) / L1". When the dimensional change rate in the first direction or the second direction is less than 0%, it means that the length in the first direction or the second direction becomes smaller through the harsh environment test. On the other hand, when the dimensional change rate in the first direction or the second direction is greater than 0%, it means that the length in the first direction or the second direction becomes larger through the harsh environment test. The method for measuring the dimensional change rate is the same method as that in the embodiments described later or a method in accordance therewith.

[0042] In order to obtain the antireflection film ARF1 having more excellent bending resistance at high temperatures, the dimensional change rate in the second direction before and after the heat resistance test is preferably -0.10% or more and 0.10% or less.

[0043] In order to obtain an anti-reflection film ARF1 having better bending resistance at high temperatures, the dimensional change rates in the first direction and the second direction before and after the heat resistance test are preferably not less than -0.09%, more preferably not less than -0.08%, and may be not less than -0.07%, not less than -0.06%, or not less than -0.05%. In addition, in order to obtain an anti-reflection film ARF1 having better bending resistance at high temperatures, the dimensional change rates in the first direction and the second direction before and after the heat resistance test are preferably not more than 0.09%, more preferably not more than 0.05%, and may be not more than 0.04%, not more than 0.03%, not more than 0.02%, or not more than 0.01%. In order to obtain an anti-reflection film ARF1 with further excellent bending resistance at high temperatures, at least one of the dimensional change rates in the first direction and the second direction before and after the heat resistance test is preferably greater than 0.00% and less than 0.10%, more preferably greater than 0.00% and less than 0.04%, further preferably greater than 0.00% and less than 0.03%, further preferably greater than 0.00% and less than 0.02%, and particularly preferably greater than 0.00% and less than 0.01%.

[0044] In order to obtain an antireflection film ARF1 having particularly excellent bending resistance at high temperatures, it is preferred that the dimensional change rate in the first direction before and after the heat resistance test is 0.00% or more and 0.10% or less, and the dimensional change rate in the second direction before and after the heat resistance test is -0.07% or more and 0.00% or less, more preferably the dimensional change rate in the first direction before and after the heat resistance test is 0.00% or more and 0.04% or less, and the dimensional change rate in the second direction before and after the heat resistance test is -0.07% or more and 0.00% or less, and further preferably the dimensional change rate in the first direction before and after the heat resistance test is 0.00 % or more and 0.03% or less, and the dimensional change rate in the second direction before and after the heat resistance test is -0.06% or more and 0.00% or less, more preferably the dimensional change rate in the first direction before and after the heat resistance test is 0.00% or more and 0.02% or less, and the dimensional change rate in the second direction before and after the heat resistance test is -0.05% or more and 0.00% or less, and particularly preferably the dimensional change rate in the first direction before and after the heat resistance test is 0.00% or more and 0.01% or less, and the dimensional change rate in the second direction before and after the heat resistance test is -0.05% or more and 0.00% or less. When the dimensional change rates in the first direction and the second direction before and after the heat resistance test are within the above ranges, in order to further suppress the generation of cracks in the anti-reflection layer in a bent state at high temperature, it is preferred to store the anti-reflection film ARF1 in a state where it is bent in the first direction.

[0045] In order to obtain an antireflection film ARF2 having better bending resistance under high temperature and high humidity, the dimensional change rate in the second direction before and after the moisture and heat resistance test is preferably 0.01% or more and 0.20% or less.

[0046] In order to obtain an anti-reflection film ARF2 with better bending resistance under high temperature and high humidity, the dimensional change rates in the first direction and the second direction before and after the moisture and heat resistance test are preferably 0.02% or more, more preferably 0.03% or more, and may also be 0.04% or more, 0.05% or more, 0.06% or more, 0.07% or more, 0.08% or more, or 0.09% or more. In addition, in order to obtain an anti-reflection film ARF2 with better bending resistance under high temperature and high humidity, the dimensional change rates in the first direction and the second direction before and after the moisture and heat resistance test are preferably 0.15% or less, more preferably 0.14% or less, and further preferably 0.13% or less. In order to obtain an anti-reflection film ARF2 with further excellent bending resistance under high temperature and high humidity, the dimensional change rates in the first direction and the second direction before and after the moisture and heat resistance test are preferably from 0.05% to 0.13%, more preferably from 0.06% to 0.13%, further preferably from 0.07% to 0.13%, further preferably from 0.08% to 0.13%, and particularly preferably from 0.09% to 0.13%.

[0047] In order to obtain an antireflection film ARF2 having particularly excellent bending resistance under high temperature and high humidity, it is preferred that the dimensional change rate in the first direction before and after the moisture and heat resistance test is 0.05% or more and 0.11% or less, and the dimensional change rate in the second direction before and after the moisture and heat resistance test is 0.10% or more and 0.13% or less, more preferably the dimensional change rate in the first direction before and after the moisture and heat resistance test is 0.06% or more and 0.11% or less, and the dimensional change rate in the second direction before and after the moisture and heat resistance test is 0.11% or more and 0.13% or less, and further preferably the dimensional change rate in the first direction before and after the moisture and heat resistance test is 0.0 The dimensional change rate in the first direction before and after the moisture and heat resistance test is preferably 0.7% or more and 0.11% or less, and the dimensional change rate in the second direction before and after the moisture and heat resistance test is 0.11% or more and 0.13% or less, and the dimensional change rate in the first direction before and after the moisture and heat resistance test is more preferably 0.08% or more and 0.11% or less, and the dimensional change rate in the second direction before and after the moisture and heat resistance test is more preferably 0.11% or more and 0.13% or less, and the dimensional change rate in the first direction before and after the moisture and heat resistance test is particularly preferably 0.09% or more and 0.11% or less, and the dimensional change rate in the second direction before and after the moisture and heat resistance test is more preferably 0.12% or more and 0.13% or less. When the dimensional change rates in the first direction and the second direction before and after the moisture and heat resistance test are within the above ranges, in order to further suppress the generation of cracks in the anti-reflection layer in a bent state under high temperature and high humidity, it is preferred to store the anti-reflection film ARF2 in a state where it is bent in the first direction.

[0048] Hereinafter, the structure of the antireflection film ARF will be described with reference to the drawings. Figure 1 It is a cross-sectional view showing an example of the antireflection film ARF. Figure 1 The antireflection film 10 shown in this example includes a transparent film substrate 11, a hard coating layer 12, and an antireflection layer 13. When the antireflection film 10 is the antireflection film ARF1, the dimensional change rate in the first direction before and after the heat resistance test of the antireflection film 10 is not less than -0.10% and not more than 0.10%. In addition, when the antireflection film 10 is the antireflection film ARF2, the dimensional change rate in the first direction of the antireflection film 10 before and after the moisture and heat resistance test is not less than 0.01% and not more than 0.20%.

[0049] In addition, the antireflection film 10 further includes: a primer layer 18 disposed between the hard coating layer 12 and the antireflection layer 13; and an antifouling layer 19 disposed on the side of the antireflection layer 13 opposite to the hard coating layer 12. That is, the antireflection film 10 includes: a transparent film substrate 11, a hard coating layer 12, a primer layer 18, an antireflection layer 13, and an antifouling layer 19 in this order.

[0050] The anti-reflection layer 13 has four layers, starting from the hard coating layer 12 side (primer layer 18 side), in sequence: a high refractive index layer 14, a low refractive index layer 15, a high refractive index layer 16 and a low refractive index layer 17. The details of the high refractive index layer and the low refractive index layer will be described later. It should be noted that the anti-reflection layer of the anti-reflection film ARF is not limited to a four-layer structure such as the anti-reflection layer 13, but can also be a two-layer structure, a three-layer structure, a five-layer structure or a stacked structure of more than six layers. The anti-reflection layer of the anti-reflection film ARF is preferably an alternating stack of more than two high refractive index layers and more than two low refractive index layers. In order to reduce reflection at the air interface, it is preferred that the outermost layer (the layer farthest from the hard coating layer 12) of the anti-reflection layer of the anti-reflection film ARF is a low refractive index layer.

[0051] Anti-reflection film ARF can also be Figure 1 The anti-reflection film 10 shown in the figure has different layer structures. For example, the anti-reflection film ARF can also be as follows Figure 2 The antireflection film 20 shown further includes a pressure-sensitive adhesive layer 21 disposed on the side of the transparent film substrate 11 opposite to the hard coat layer 12 side.

[0052] The adhesive constituting the adhesive layer 21 is not particularly limited, and for example, a transparent adhesive based on the following polymers can be appropriately selected and used: acrylic polymers, silicone polymers, polyesters, polyurethanes, polyamides, polyvinyl ethers, vinyl acetate-vinyl chloride copolymers, modified polyolefins, epoxy resins, fluorine resins, natural rubber, synthetic rubber, etc. The thickness of the adhesive layer 21 is not particularly limited, but is preferably 5 μm or more and 100 μm or less from the viewpoint of both thinness and adhesiveness.

[0053] A release liner (not shown) may be temporarily bonded to the main surface of the adhesive layer 21 on the opposite side to the transparent film substrate 11. The release liner is used, for example, until the anti-reflection film 20 is attached to the image display panel 101 (see FIG. Figure 3 ) to the bonding, the surface of the adhesive layer 21 is protected. As the constituent material of the release liner, a plastic film formed of acrylic acid, polyolefin, cyclic polyolefin, polyester, etc. is preferably used. The thickness of the release liner is, for example, not less than 5 μm and not more than 200 μm. It is preferred that a release treatment is applied to the surface of the release liner. As the material of the release agent used for the release treatment, silicone-based materials, fluorine-based materials, long-chain alkyl-based materials, fatty acid amide-based materials, etc. can be listed.

[0054] As mentioned above, the structure of the antireflection film of the first embodiment is described with reference to the drawings, but the antireflection film of the present invention is not limited to the above structure.

[0055] For example, the dimensional change rate in the first direction before and after the heat resistance test may be -0.10% to 0.10%, and the dimensional change rate in the first direction before and after the moisture and heat resistance test may be 0.01% to 0.20%. In this case, an antireflection film having excellent bending resistance at high temperature and excellent bending resistance at high temperature and high humidity can be obtained.

[0056] In addition, the anti-reflection film of the present invention may also be an anti-reflection film without a primer layer and an anti-fouling layer. In addition, the anti-reflection film of the present invention may also be provided with an optical functional layer different from the layers (transparent film substrate, hard coating layer, primer layer, anti-reflection layer and anti-fouling layer) contained in the above-mentioned constitution.

[0057] Next, elements of the antireflection film (more specifically, the antireflection film ARF) according to the first embodiment will be described.

[0058] [Transparent film substrate]

[0059] The transparent film substrate is, for example, a flexible transparent resin film. As the material constituting the transparent film substrate, for example, polyester resin, polyolefin resin, polystyrene resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polysulfone resin, polyamide resin, polyimide resin, cellulose resin, norbornene resin, polyarylate resin and polyvinyl alcohol resin can be cited. As polyester resin, for example, polyethylene terephthalate (PET), polybutylene terephthalate and polyethylene naphthalate can be cited. As polyolefin resin, for example, polyethylene, polypropylene and cycloolefin polymer (COP) can be cited. As cellulose resin, for example, cellulose triacetate (TAC) can be cited. These materials can be used alone or in combination of two or more. As the material of the transparent film substrate, from the viewpoint of transparency and strength, it is preferably selected from one of the group consisting of polyester resin, polyolefin resin and cellulose resin, more preferably selected from one of the group consisting of PET, COP and TAC, and further preferably PET. That is, as the transparent film substrate, preferably, one film selected from the group consisting of polyester resin films, polyolefin resin films and cellulose resin films, more preferably, one film selected from the group consisting of PET films, COP films and TAC films, and further preferably, PET films.

[0060] From the viewpoint of strength, the thickness of the transparent film substrate is preferably 5 μm or more, more preferably 10 μm or more, and further preferably 20 μm or more. From the viewpoint of handleability, the thickness of the transparent film substrate is preferably 300 μm or less, and more preferably 200 μm or less.

[0061] One or both main surfaces of the transparent film substrate may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0062] From the viewpoint of improving the transparency of the antireflection film, the total light transmittance (JIS K7375-2008) of the transparent film substrate is preferably 80% or more, more preferably 90% or more, and further preferably 95% or more and 100% or less.

[0063] [Hard coating]

[0064] The hard coat layer is a layer that improves the mechanical properties of the anti-reflection film, such as the hardness and elastic modulus. The hard coat layer is, for example, composed of a cured product of a curable resin composition (composition for forming a hard coat layer). As the curable resin contained in the curable resin composition, for example, polyester resins, acrylic resins, carbamate resins, acrylic carbamate resins, amide resins, silicone resins, epoxy resins, and melamine resins can be listed. These curable resins can be used alone or in combination of two or more. From the viewpoint of improving the hardness of the hard coat layer, as the curable resin, it is preferably selected from one or more of the group consisting of acrylic resins and acrylic carbamate resins, and more preferably acrylic resins.

[0065] In addition, as a curable resin composition, for example, a UV-curable resin composition and a thermosetting resin composition can be listed. From the viewpoint of improving the productivity of the anti-reflection film, as a curable resin composition, a UV-curable resin composition is preferably used. The UV-curable resin composition includes one or more selected from the group consisting of a UV-curable monomer, a UV-curable oligomer, and a UV-curable polymer. As a specific example of a UV-curable resin composition, a hard coat forming composition described in Japanese Patent Publication No. 2016-179686 can be listed.

[0066] In addition, the curable resin composition may also contain microparticles. By adding microparticles to the curable resin composition, the hardness, surface roughness, refractive index and anti-glare properties in the hard coating layer can be adjusted. As microparticles, for example, metal oxide particles, glass particles and organic particles can be listed. As materials for metal oxide particles, for example, silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, calcium oxide, tin oxide, indium oxide, cadmium oxide and antimony oxide can be listed. As materials for organic particles, for example, polymethyl methacrylate, polystyrene, polyurethane, acrylic acid-styrene copolymer, benzoguanamine, melamine and polycarbonate can be listed.

[0067] From the viewpoint of improving the hardness of the hard coating layer, the thickness of the hard coating layer is preferably 1 μm or more, more preferably 2 μm or more. From the viewpoint of ensuring the flexibility of the antireflection film, the thickness of the hard coating layer is preferably 50 μm or less, more preferably 40 μm or less, further preferably 35 μm or less, and further preferably 30 μm or less.

[0068] The main surface of the hard coating layer on the side opposite to the transparent film substrate side may also be subjected to surface modification treatment. Examples of surface modification treatments include plasma treatment, corona treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment. In order to improve the adhesion between the layer (e.g., primer layer described later) provided on the side opposite to the transparent film substrate side of the hard coating layer and the hard coating layer, the main surface of the hard coating layer on the side opposite to the transparent film substrate side is preferably subjected to plasma treatment.

[0069] [Primer layer]

[0070] In order to improve the adhesion between the hard coating layer and the anti-reflection layer, it is preferred to provide a primer layer between the hard coating layer and the anti-reflection layer. Materials for the primer layer include metals (or semi-metals) such as silicon, nickel, chromium, tin, gold, silver, platinum, zinc, titanium, indium, tungsten, aluminum, zirconium, palladium, etc.; alloys of these metals (or semi-metals); oxides, fluorides, sulfides or nitrides of these metals (or semi-metals), etc. The oxide constituting the primer layer may also be a composite oxide such as indium tin oxide (ITO). Among them, inorganic oxides are preferred as materials for the primer layer, and silicon oxide, indium oxide or ITO are particularly preferred.

[0071] In order to improve the adhesion between the hard coat layer and the antireflection layer and ensure the light transmittance of the primer layer, the thickness of the primer layer is preferably 0.5 nm to 20 nm, more preferably 0.5 nm to 10 nm, and further preferably 1.0 nm to 10 nm.

[0072] [Anti-reflective layer]

[0073] The anti-reflection layer includes two or more thin films with different refractive indices. Generally, in the case of the anti-reflection layer, the optical film thickness (the product of the refractive index and the thickness) of the thin film is adjusted in such a way that the inverted phases of the incident light and the reflected light cancel each other out. By making the anti-reflection layer into a multilayer laminate of two or more thin films with different refractive indices, the reflectivity can be reduced within a wide wavelength range of visible light.

[0074] Examples of the material of the thin film constituting the antireflection layer include metal (or semimetal) oxides, nitrides, fluorides, etc. The antireflection layer is preferably an alternating stack of high refractive index layers and low refractive index layers.

[0075] The refractive index of the high refractive index layer is, for example, greater than 1.9, preferably greater than 2.0. Examples of materials for the high refractive index layer include: titanium oxide, niobium oxide, zirconium oxide, tantalum oxide, zinc oxide, indium oxide, ITO, antimony-doped tin oxide (ATO), etc. Among them, preferably one or more selected from the group consisting of titanium oxide and niobium oxide. The refractive index of the low refractive index layer is, for example, less than 1.6, preferably less than 1.5. Examples of materials for the low refractive index layer include: silicon oxide, titanium nitride, magnesium fluoride, barium fluoride, calcium fluoride, hafnium fluoride, lanthanum fluoride, etc. Among them, silicon oxide is preferred. It is particularly preferred to use niobium oxide (NbO2) as the high refractive index layer. 2 O 5 ) film and silicon oxide (SiO 2 ) thin films are alternately stacked. In addition to providing low refractive index layers and high refractive index layers, medium refractive index layers having a refractive index greater than 1.6 and less than 1.9 may also be provided.

[0076] The film thickness of high refractive index layer and low refractive index layer is preferably more than 5nm and below 200nm respectively, more preferably more than 10nm and below 150nm.As long as according to refractive index, stacking constitution etc., the film thickness of each layer is designed in a way that the reflectivity of visible light tapers down.For example, as the stacking constitution of high refractive index layer and low refractive index layer, following four layers of constitution can be listed: from the hard coat side, comprise the high refractive index layer of more than optical thickness 20nm and below 55nm, the low refractive index layer of more than optical thickness 35nm and below 55nm, the high refractive index layer of more than optical thickness 80nm and below 250nm and the low refractive index layer of more than optical thickness 100nm and below 150nm.

[0077] The anti-reflection layer is niobium oxide (Nb 2 O 5 ) film and silicon oxide (SiO 2 ) films are alternately stacked, the antireflection layer may include, in order from the hard coating side, a niobium oxide film having a thickness of 5 nm to 20 nm, a silicon oxide film having a thickness of 20 nm to 40 nm, a niobium oxide film having a thickness of 65 nm to 120 nm, and a silicon oxide film having a thickness of 60 nm to 100 nm.

[0078] In order to obtain an anti-reflection film with better bending resistance under harsh environments, the thickness of the anti-reflection layer is preferably 150 nm or more and 280 nm or less, more preferably 180 nm or more and 280 nm or less, further preferably 190 nm or more and 260 nm or less, and further preferably 200 nm or more and 250 nm or less. It should be noted that in this specification, the "thickness of the anti-reflection layer" is the sum of the thicknesses of the layers constituting the anti-reflection layer (total thickness).

[0079] [Antifouling layer]

[0080] The anti-reflection film preferably has an anti-fouling layer on the side of the anti-reflection layer opposite to the hard coating layer, and more preferably has an anti-fouling layer as the outermost layer of the anti-reflection film. By providing the anti-fouling layer, for example, the influence of pollution (fingerprints, hand dirt, dust, etc.) from the external environment can be reduced, and pollutants attached to the surface of the anti-reflection film can be easily removed.

[0081] In order to suppress the reduction of the antireflection performance of the antireflection layer, the antifouling layer preferably has a small refractive index difference with the outermost layer (eg, low refractive index layer) of the antireflection layer. The refractive index of the antifouling layer is preferably 1.6 or less, more preferably 1.55 or less.

[0082] As the material of the antifouling layer, a fluorine-containing compound is preferred. The fluorine-containing compound has excellent antifouling properties and can contribute to a low refractive index. Among them, alkoxysilane compounds containing a perfluoropolyether skeleton are preferred from the perspective of excellent hydrophobicity and high antifouling properties. Examples of alkoxysilane compounds containing a perfluoropolyether skeleton include: alkoxysilane compounds having a plurality of linear or branched perfluorooxyalkylene units having a carbon number of 1 to 4. Examples of linear or branched perfluorooxyalkylene units having a carbon number of 1 to 4 include: perfluorooxymethylene units (-CF 2 O-), perfluoroethylene units (-CF 2 CF 2 O-), perfluorooxypropylene unit (-CF 2 CF 2 CF 2 O-), perfluorooxyisopropylidene unit (-CF(CF 3 )CF 2 O-) etc.

[0083] The thickness of the antifouling layer is, for example, 2 nm or more and 50 nm or less. There is a tendency that the greater the thickness of the antifouling layer, the more improved the antifouling property. The thickness of the antifouling layer is preferably 5 nm or more, more preferably 7 nm or more, and further preferably 8 nm or more. On the other hand, from the viewpoint of improving the anti-glare property, the thickness of the antifouling layer is preferably 30 nm or less, more preferably 20 nm or less.

[0084] [Preferred embodiment of antireflection film]

[0085] In order to obtain an antireflection film having particularly excellent bending resistance at high temperatures, the antireflection film of the first embodiment preferably satisfies the following condition 1, more preferably satisfies the following condition 2, further preferably satisfies the following condition 3, and further preferably satisfies the following condition 4.

[0086] Condition 1: At least one of the dimensional change rates in the first direction and the second direction before and after the heat resistance test is 0.00% or more and 0.04% or less.

[0087] Condition 2: The above-mentioned condition 1 is satisfied, and the thickness of the antireflection layer is 150 nm or more and 280 nm or less.

[0088] Condition 3: The dimensional change rate in the first direction before and after the heat resistance test is 0.00% or more and 0.04% or less, and the dimensional change rate in the second direction before and after the heat resistance test is -0.07% or more and 0.00% or less.

[0089] Condition 4: The above-mentioned condition 3 is satisfied, and the thickness of the antireflection layer is 150 nm or more and 280 nm or less.

[0090] Furthermore, in order to obtain an antireflection film having particularly excellent bending resistance under high temperature and high humidity, the antireflection film of the first embodiment preferably satisfies the following condition i, more preferably satisfies the following condition ii, further preferably satisfies the following condition iii, and further preferably satisfies the following condition iv.

[0091] Condition i: The dimensional change rates in the first direction and the second direction before and after the moisture and heat resistance test are both 0.05% or more and 0.13% or less.

[0092] Condition ii: The above condition i is satisfied, and the thickness of the antireflection layer is 150 nm or more and 280 nm or less.

[0093] Condition iii: The dimensional change rate in the first direction before and after the moisture and heat resistance test is 0.05% or more and 0.11% or less, and the dimensional change rate in the second direction before and after the moisture and heat resistance test is 0.10% or more and 0.13% or less.

[0094] Condition iv: The above condition iii is satisfied, and the thickness of the antireflection layer is 150 nm or more and 280 nm or less.

[0095] In addition, in order to obtain an anti-reflection film having particularly excellent bending resistance at high temperatures and particularly excellent bending resistance at high temperatures and high humidity, the anti-reflection film of the first embodiment preferably satisfies the above-mentioned conditions 1 and i, more preferably satisfies the above-mentioned conditions 2 and ii, further preferably satisfies the above-mentioned conditions 3 and iii, and further preferably satisfies the above-mentioned conditions 4 and iv.

[0096] <Second Embodiment: Image Display Device>

[0097] Next, an image display device according to a second embodiment of the present invention is described. The image display device according to the second embodiment includes: an image display panel; and the antireflection film according to the first embodiment, which is arranged on the visible side of the image display panel. Hereinafter, the description of the contents repeated in the first embodiment is omitted.

[0098] Figure 3 It is a cross-sectional view showing an example of the image display device according to the second embodiment. Figure 3 The image display device 100 shown in the figure comprises: an image display panel 101; and an anti-reflection film 10 as an example of the anti-reflection film of the first embodiment, which is arranged on the visible side ( Figure 3 In the image display device 100 , the transparent film substrate 11 of the antireflection film 10 is bonded to the image display panel 101 via the adhesive layer 21 .

[0099] As the image display panel 101, an image display panel including an image display cell such as a liquid crystal cell or an organic EL cell can be exemplified.

[0100] As for the image display device of the second embodiment, an anti-reflection film is arranged on the visible side of the image display panel, so that the reflection of external light is reduced and the visibility is excellent. In addition, the image display device of the second embodiment has the anti-reflection film of the first embodiment (anti-reflection film with excellent bending resistance in harsh environments), so even if it is stored in a state of bending with the anti-reflection layer forming surface side as the inner side, it is not easy to generate cracks in the anti-reflection layer at the bent portion. Therefore, the image display device of the second embodiment can also be used as a foldable display, for example. In order to obtain a foldable display that can further suppress the generation of cracks in the anti-reflection layer in a harsh environment, the bending portion of the foldable display is preferably a bending portion that can bend the anti-reflection film in the first direction.

[0101] <Third Embodiment: Method for Producing Antireflection Film>

[0102] Next, a method for producing an antireflection film according to a third embodiment of the present invention will be described. The method for producing an antireflection film according to the third embodiment is a preferred method for producing an antireflection film according to the first embodiment. Hereinafter, descriptions of contents that overlap with those of the first embodiment will be omitted.

[0103] The method for manufacturing an anti-reflection film of the third embodiment includes: step Sa, forming an anti-reflection layer on the side of the hard coating layer opposite to the transparent film substrate side using a roll-to-roll sputtering film forming device; and step Sb, after step Sa, heating the laminated body formed with the anti-reflection layer. The method for manufacturing an anti-reflection film of the third embodiment includes step Sa and step Sb, so the anti-reflection film of the first embodiment can be easily manufactured. Hereinafter, step Sa is described as "anti-reflection layer forming step". In addition, step Sb is described as "anti-reflection layer heating step".

[0104] The method for manufacturing the antireflection film of the third embodiment may also include steps (other steps) other than the antireflection layer forming step and the antireflection layer heating step. As other steps, for example, there can be listed: a hard coating layer forming step described later, a hard coating layer surface treatment step, a hard coating layer heating step, a primer layer forming step, and an antifouling layer forming step.

[0105] Hereinafter, each step included in an example of the method for producing the antireflection film according to the third embodiment will be described.

[0106] [Hard Coat Formation Step]

[0107] The hard coat forming step is a step of forming a hard coat on a transparent film substrate. For example, a curable resin composition (composition for forming a hard coat) is applied to a transparent film substrate, and the solvent is removed and the resin is cured as required to form a hard coat. The composition for forming a hard coat, for example, includes the above-mentioned curable resin and a polymerization initiator (e.g., a photopolymerization initiator), and includes a solvent that can dissolve or disperse these components as required.

[0108] In addition to the above-mentioned components, the hard coat forming composition may also contain additives such as microparticles, leveling agents, viscosity modifiers (thixotropic agents, thickeners, etc.), antistatic agents, antiblocking agents, dispersants, dispersion stabilizers, antioxidants, ultraviolet absorbers, defoaming agents, surfactants, lubricants, etc.

[0109] As a coating method for the hard coat forming composition, any appropriate method such as rod coating, roller coating, gravure coating, rod coating, slot orifice coating, curtain coating, fountain coating, comma coating, etc. can be adopted. The drying temperature of the coating film after coating can be set to an appropriate temperature according to the composition of the hard coat forming composition, for example, above 50°C and below 150°C. In the case where the resin component in the hard coat forming composition is a thermosetting resin, the coating film is cured by heating. In the case where the resin component in the hard coat forming composition is a photocurable resin, the coating film is cured by irradiating active energy rays such as ultraviolet rays. The cumulative light amount of the irradiated light is preferably 100mJ / cm 2 Above and 500mJ / cm 2 the following.

[0110] [Surface treatment process of hard coating]

[0111] In the surface treatment process of the hard coating layer, the main surface of the hard coating layer on the opposite side to the transparent film substrate side is subjected to surface modification treatment. Examples of surface modification treatments include plasma treatment, corona treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment. When the surface modification treatment is plasma treatment, argon gas is used as an inert gas, for example. In addition, the discharge power in the plasma treatment is, for example, 10 W or more and 10,000 W or less.

[0112] [Hard coating heating process]

[0113] The hard coating heating process is a process of heating a laminate including a hard coating (e.g., a film-like laminate having a transparent film substrate and a hard coating) before arranging other layers (e.g., a primer layer, an anti-reflection layer, etc.) on the hard coating. By arranging the hard coating heating process, for example, the dimensional change of the anti-reflection film caused by the heat shrinkage of the transparent film substrate can be suppressed.

[0114] In the third embodiment, a roll-to-roll sputtering film forming device is used in the anti-reflection layer forming step, so from the viewpoint of improving productivity, in the hard coating heating step, it is preferred to heat the laminate while conveying it in a roll-to-roll manner. Examples of the heating device during heating include a hot air oven, an infrared heater, and the like.

[0115] The heating temperature of the above-mentioned laminate in the hard coating heating step is, for example, 100° C. to 200° C. The heating time of the above-mentioned laminate in the hard coating heating step is, for example, 30 seconds to 30 minutes. It should be noted that, when a surface treatment step of the hard coating and a hard coating heating step are provided, the hard coating heating step may be implemented before the surface treatment step of the hard coating or after the surface treatment step of the hard coating.

[0116] [Primer layer forming step]

[0117] The primer layer forming process is a process for forming a primer layer (film forming) on ​​the hard coat layer. The film forming method of the primer layer is not particularly limited, and can be any of a wet coating method and a dry coating method. From the perspective of being able to form a thin film with uniform film thickness, dry coating methods such as vacuum evaporation, CVD, and sputtering are preferred. In addition, in the third embodiment, a roll-to-roll sputtering film forming device is used in the anti-reflection layer forming process, so from the perspective of improving productivity, as a film forming method for the primer layer, a method (roll-to-roll sputtering method) of film formation using a roll-to-roll sputtering film forming device is preferred.

[0118] In a roll-to-roll sputtering method, a long film (e.g., a transparent film substrate having a hard coating layer formed thereon) can be continuously formed into a film, for example, a primer layer and an anti-reflection layer, while being transported in the long dimension direction (MD direction). In the sputtering method, film formation is performed while an inert gas such as argon and a reactive gas such as oxygen as required are introduced into a film forming chamber. In the case where an oxide layer is formed as a primer layer, the film formation of the oxide layer by sputtering can be performed by any of a method using an oxide target and reactive sputtering using a metal (or semi-metal) target.

[0119] As power sources for implementing the sputtering method, for example, there can be listed: DC power supply, AC power supply, RF power supply and MFAC power supply (AC power supply with a frequency band of several kHz to several MHz). The discharge power in the sputtering method is, for example, greater than 1 kW and less than 100 kW, preferably greater than 1 kW and less than 50 kW. The surface temperature of the film-forming roller when implementing the sputtering method is, for example, greater than -25°C and less than 25°C, preferably greater than -20°C and less than 0°C. The pressure in the film-forming chamber when implementing the sputtering method is preferably greater than 0.01 Pa and less than 10 Pa, more preferably greater than 0.05 Pa and less than 5 Pa, and further preferably greater than 0.1 Pa and less than 1 Pa.

[0120] [Anti-reflection layer forming step]

[0121] In the anti-reflection layer forming step, the anti-reflection layer is formed on the side of the hard coating layer opposite to the transparent film substrate side (e.g., the hard coating layer surface or the primer layer surface) using a roll-to-roll sputtering film forming device. That is, in the third embodiment, each layer of the anti-reflection layer is formed using a roll-to-roll sputtering method. When the sputtering method is implemented in the anti-reflection layer forming step, the film forming conditions can be appropriately set among the conditions described in the above-mentioned [primer layer forming step].

[0122] Through the research of the present inventors, it is clear that if the layers of the anti-reflection layer are formed by a roll-to-roll sputtering method, the anti-reflection film is easy to shrink in a harsh environment. In particular, when a stretched film such as a PET film is used as a transparent film substrate, the shrinkage of the anti-reflection film is significant. It is speculated that when a laminated body (e.g., a film-like laminated body having at least a transparent film substrate and a hard coating layer) to be formed with an anti-reflection layer is transported by a roll-to-roll method, tension is applied to the laminated body in the transport direction, so residual stress is generated in the laminated body, and the anti-reflection film is easy to shrink in a harsh environment.

[0123] [Antifouling layer forming step]

[0124] The antifouling layer forming step is a step of forming an antifouling layer on the side of the antireflection layer opposite to the hard coating layer. In the antifouling layer forming step, for example, a fluorine-containing compound is used as a material to form the antifouling layer by a dry coating method. Examples of the dry coating method include vacuum evaporation, sputtering, and CVD, and vacuum evaporation is preferred.

[0125] [Anti-reflection layer heating process]

[0126] The anti-reflection layer heating process is a process for heating a laminated body formed with an anti-reflection layer (hereinafter sometimes described as a "film with an anti-reflection layer"). By heating the film with an anti-reflection layer, for example, at least a portion of the residual stress of the film with an anti-reflection layer is removed, thereby suppressing the shrinkage of the anti-reflection film under harsh environments. As a result, an anti-reflection film with excellent bending resistance under harsh environments is obtained. It should be noted that, when an anti-fouling layer forming process is provided, the anti-reflection layer heating process can be implemented before the anti-fouling layer forming process or after the anti-fouling layer forming process. When an anti-fouling layer forming process is provided, in order to obtain an anti-reflection film with better bending resistance under harsh environments, the anti-reflection layer heating process is preferably implemented after the anti-fouling layer forming process.

[0127] In the third embodiment, a roll-to-roll sputtering film forming device is used in the anti-reflection layer forming step, so from the viewpoint of improving productivity, in the anti-reflection layer heating step, it is preferred to heat the film with the anti-reflection layer while conveying it in a roll-to-roll manner. Examples of the heating device during heating include a hot air oven, an infrared heater, and the like.

[0128] In order to obtain an antireflection film with better bending resistance under a harsh environment, the heating temperature of the film with an antireflection layer in the antireflection layer heating step is preferably 110° C. or more, more preferably 115° C. or more, further preferably 120° C. or more, and may be 130° C. or more, 140° C. or more, 150° C. or more, 160° C. or more, 170° C. or more, or 180° C. or more. In addition, in order to obtain an antireflection film with better bending resistance under a harsh environment, the heating time of the film with an antireflection layer in the antireflection layer heating step is preferably 30 seconds or more, more preferably 1 minute or more, further preferably 2 minutes or more, and may be 5 minutes or more, 10 minutes or more, or 15 minutes or more.

[0129] In order to suppress the decrease in transparency of the anti-reflection film, the heating temperature of the film with the anti-reflection layer in the anti-reflection layer heating step is preferably 200° C. or less, and more preferably 190° C. or less. In addition, in order to suppress the decrease in transparency of the anti-reflection film, the heating time of the film with the anti-reflection layer in the anti-reflection layer heating step is preferably 30 minutes or less, and more preferably 20 minutes or less.

[0130] The dimensional change rates in the first and second directions before and after the above-mentioned heat resistance test and the dimensional change rates in the first and second directions before and after the above-mentioned moisture and heat resistance test can be adjusted by changing the heating conditions in the anti-reflection layer heating process (specifically, heating temperature, heating time, etc.).

[0131] Example

[0132] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the following examples.

[0133] <Production of antireflection film of Example 1>

[0134] [Hard Coat Formation Step]

[0135] A UV-curable multifunctional acrylic resin composition ("Z-850-50H-D" manufactured by AICA Industries, solid content concentration: 44% by weight) converted to 100 parts by weight of solid content, 4 parts by weight of a photopolymerization initiator ("Omnirad2959" manufactured by IGM Resins) and 0.05 parts by weight of a leveling agent ("LE-303" manufactured by Kyoeisha Chemical Co., Ltd.) were mixed to obtain a mixed solution. Then, methyl isobutyl ketone was added to the obtained mixed solution to obtain a hard coat forming composition having a solid content concentration of 40% by weight. Next, the hard coat forming composition was applied to one main surface of a PET film ("50U48" manufactured by Toray, thickness: 50μm) serving as a transparent film substrate to form a coating film. Next, the coating film was dried by heating it at a temperature of 80°C for 60 seconds, and then cured by ultraviolet irradiation. During ultraviolet irradiation, a high-pressure mercury lamp was used as a light source, ultraviolet rays with a wavelength of 365nm were used, and the accumulated light amount was set to 300mJ / cm 2 Thus, a hard coating layer having a thickness of 3 μm was formed on the PET film.

[0136] [Surface treatment process of hard coating]

[0137] Next, a plasma treatment device in a roll-to-roll manner was used to plasma-treat the surface of the hard coating layer while conveying the PET film having the hard coating layer formed thereon in a vacuum atmosphere of 1.0 Pa. During the plasma treatment, argon gas was used as an inert gas, and the discharge power was set to 150 W. Thus, a laminate having a PET film and a hard coating layer treated with plasma (hereinafter sometimes referred to as "optical film F1") was obtained.

[0138] [Hard coating heating process]

[0139] Next, the optical film F1 was heated at a temperature of 140° C. for 2 minutes using a hot air oven while being conveyed by a roll-to-roll conveyor.

[0140] [Primer layer forming step]

[0141] Next, the heated optical film F1 was introduced into a roll-to-roll sputtering film forming apparatus, and the pressure in the film forming chamber was reduced to 1×10 -4 Pa. Then, while conveying the optical film F1, argon and oxygen were introduced at a volume ratio of 100:10, the surface temperature of the film-forming roller was set to -8°C, and an ITO layer (primer layer) with a thickness of 1.5 nm was formed on the hard coating layer by sputtering. The primer layer was formed using an ITO target containing indium oxide and tin oxide at a weight ratio of 90:10 as a target material. In addition, when forming a film by sputtering, the power supply was set to an MFAC power supply, the discharge power was set to 2.5 kW, and the pressure in the film-forming chamber was set to 0.2 Pa.

[0142] [Anti-reflection layer forming step]

[0143] After the primer layer was formed, the following layers were sequentially formed on the primer layer by sputtering while the optical film F1 after the primer layer was formed was transported using a roll-to-roll sputtering film forming apparatus. The first layer was Nb with a thickness of 12 nm. 2 O 5 layer (refractive index: 2.33); second layer: SiO with a thickness of 28 nm 2 layer (refractive index: 1.46); third layer: Nb with a thickness of 100 nm 2 O 5 layer; and a fourth layer: SiO with a thickness of 85 nm 2 layer. Thus, an antireflection layer having a four-layer structure (a four-layer structure consisting of a first layer, a second layer, a third layer, and a fourth layer) is formed on the primer layer. In the film formation of each of the first to fourth layers, the surface temperature of the film forming roller is set to -8°C, the power supply is set to an MFAC power supply, and the pressure in the film forming chamber is set to 0.7 Pa. In addition, in the film formation of the first layer, an Nb target is used, argon and oxygen are introduced at a volume ratio of 100:5, and the discharge power is set to 10.5 kW. In the film formation of the second layer, an Si target is used, argon and oxygen are introduced at a volume ratio of 100:30, and the discharge power is set to 14 kW. In the film formation of the third layer, an Nb target is used, argon and oxygen are introduced at a volume ratio of 100:13, and the discharge power is set to 22 kW. In the film formation of the fourth layer, an Si target is used, argon and oxygen are introduced at a volume ratio of 100:30, and the discharge power is set to 12 kW.

[0144] [Antifouling layer forming step]

[0145] The coating agent ("SHIN-ETSU SUBELYN KY1903-1" manufactured by Shin-Etsu Chemical Co., Ltd., active ingredient: alkoxysilane compound containing a perfluoropolyether skeleton) was dried and solidified as a vapor deposition source, and the heating temperature of the vapor deposition source was set to 260°C, and an antifouling layer with a thickness of 12 nm was formed on the antireflection layer by vacuum vapor deposition. Thus, a laminate having a PET film, a hard coat layer, a primer layer, an antireflection layer, and an antifouling layer was obtained (hereinafter sometimes described as "optical film F2").

[0146] [Anti-reflection layer heating process]

[0147] Next, the optical film F2 was heated at a temperature of 120° C. for 2 minutes using a hot air oven while being conveyed by a roll-to-roll conveyor. Thus, the antireflection film of Example 1 was obtained.

[0148] <Preparation of Antireflection Films of Examples 2 to 9 and Comparative Examples 1 to 5>

[0149] The heating conditions of the optical film F1 in the hard coating heating process and the heating conditions of the optical film F2 in the anti-reflection layer heating process were changed to the conditions shown in Table 1. The anti-reflection films of Examples 2 to 9 and Comparative Examples 1 to 5 were obtained by the same production method as Example 1. It should be noted that the hard coating heating process was not performed in the production of the anti-reflection films of Examples 6 to 9 and Comparative Example 4. In addition, the anti-reflection layer heating process was not performed in the production of the anti-reflection films of Comparative Examples 4 and 5.

[0150] [Table 1]

[0151] Heating conditions of hard coating heating process Heating conditions of the anti-reflection layer heating process Example 1 140℃×2min 120℃×2min Example 2 140℃×2min 140℃×2min Example 3 140℃×2min 160℃×2min Example 4 140℃×2min 180℃×2min Example 5 140℃×2min 180℃×15min Example 6 No heating treatment 120℃×2min Example 7 No heating treatment 140℃×2min Example 8 No heating treatment 160℃×2min Example 9 No heating treatment 180℃×2min Comparative Example 1 140℃×2min 60℃×2min Comparative Example 2 140℃×2min 80℃×2min Comparative Example 3 140℃×2min 100℃×2min Comparative Example 4 No heating treatment No heating treatment Comparative Example 5 140℃×2min No heating treatment

[0152] <Measurement method of dimensional change rate>

[0153] [Measurement method of dimensional change rate before and after heat resistance test]

[0154] As a test piece for measuring the dimensional change rate before and after the heat resistance test, a laser processing machine (GCC "LaserPro Spirit GLS") was used to cut out a test piece of 100mm×100mm (length in the MD direction: 100mm, length in the TD direction: 100mm) from each antireflection film. The atmospheric temperature and relative humidity when cutting the test piece were 20°C and 50%, respectively. Next, each test piece was subjected to a heat resistance test in a drying oven (ESPEC "PH-202") at a temperature of 85°C and a relative humidity of less than 1% for 48 hours, and then allowed to stand for 24 hours in an atmosphere at a temperature of 20°C and a relative humidity of 50%, and the dimensional change rate before and after the heat resistance test was obtained. That is, based on the length L1 (100 mm) in each direction at a temperature of 20°C and a relative humidity of 50% before the heat resistance test and the length L2 in each direction measured after standing for 24 hours in an atmosphere at a temperature of 20°C and a relative humidity of 50% after the heat resistance test, the dimensional change rate of each test piece in each direction (MD direction and TD direction) was calculated by the above formula.

[0155] [Measurement method of dimensional change rate before and after moisture and heat resistance test]

[0156] As a test piece for measuring the dimensional change rate before and after the moisture and heat resistance test, a laser processing machine ("LaserPro Spirit GLS" manufactured by GCC) was used to cut a test piece of 100mm×100mm in size (length in the MD direction: 100mm, length in the TD direction: 100mm) from each antireflection film. The atmospheric temperature and relative humidity when the test piece was cut were 20°C and 50%, respectively. Next, each test piece was subjected to a moisture and heat resistance test after being allowed to stand for 48 hours in a constant temperature and humidity tester ("PL-2J" manufactured by ESPEC) at a temperature of 60°C and a relative humidity of 95%, and then allowed to stand for 24 hours in an atmosphere at a temperature of 20°C and a relative humidity of 50%, and the dimensional change rate before and after the moisture and heat resistance test was determined. That is, based on the length L1 (100 mm) in each direction at a temperature of 20°C and a relative humidity of 50% before the moisture and heat resistance test and the length L2 in each direction measured after standing for 24 hours in an atmosphere at a temperature of 20°C and a relative humidity of 50% after the moisture and heat resistance test, the dimensional change rate of each test piece in each direction (MD direction and TD direction) was calculated by the above formula.

[0157] <Bending resistance evaluation>

[0158] [Evaluation of bending resistance at high temperature]

[0159] As test pieces for evaluating the bending resistance at high temperature, a laser processing machine ("LaserPro Spirit GLS" manufactured by GCC Corporation) was used to cut out test pieces 200 having a size of 10 mm in width and 100 mm in length (length direction: MD direction, width direction: TD direction) from each antireflection film. Figure 4 As shown, the surface of the test piece 200 on the antireflection layer (not shown) side is inward in the MD direction ( Figure 4 In a state of being bent in the X direction in the middle, both ends in the MD direction are attached to the spacer 300 having a thickness D (D: 4.0 mm or 3.8 mm). Figure 4 In the state, the bending radius of the bending portion of the test piece 200 is D / 2. Figure 4 The test piece 200 in the state was placed in a drying oven ("PH-202" manufactured by ESPEC) at a temperature of 85°C and a relative humidity of less than 1% for 48 hours, then taken out and the presence or absence of cracks in the bent part (white turbidity of the anti-reflection layer) was confirmed under an optical microscope. Then, if no cracks were confirmed, it was judged as A. On the other hand, if cracks were confirmed, it was judged as B. If the judgment result is A when a spacer with a thickness of 4.0 mm is used, it is evaluated as "excellent bending resistance at high temperature", and if the judgment result is B when a spacer with a thickness of 4.0 mm is used, it is evaluated as "not excellent bending resistance at high temperature".

[0160] [Evaluation of bending resistance under high temperature and high humidity]

[0161] As test pieces for evaluating the bending resistance under high temperature and high humidity, a laser processing machine ("LaserPro Spirit GLS" manufactured by GCC Corporation) was used to cut out test pieces 200 having a size of 10 mm in width and 100 mm in length (length direction: MD direction, width direction: TD direction) from each antireflection film. Figure 4 As shown, the surface of the test piece 200 on the antireflection layer (not shown) side is inward in the MD direction ( Figure 4 In a state of being bent in the X direction in the middle, both ends in the MD direction are attached to the spacer 300 having a thickness D (D: 4.0 mm or 3.8 mm). Figure 4 In the state, the bending radius of the bending portion of the test piece 200 is D / 2. Figure 4 The test piece 200 in the state was left to stand for 48 hours in a constant temperature and humidity tester ("PL-2J" manufactured by ESPEC) at a temperature of 60°C and a relative humidity of 95%, and then taken out, and the presence or absence of cracks in the bent part (white turbidity of the anti-reflection layer) was confirmed under an optical microscope. Then, if no cracks were confirmed, it was judged as A. On the other hand, if cracks were confirmed, it was judged as B. When the judgment result is A when a spacer with a thickness of 4.0 mm is used, it is evaluated as "excellent bending resistance under high temperature and high humidity", and when the judgment result is B when a spacer with a thickness of 4.0 mm is used, it is evaluated as "not excellent bending resistance under high temperature and high humidity".

[0162] <Evaluation Results>

[0163] Regarding Examples 1 to 9 and Comparative Examples 1 to 5, the dimensional change rates before and after the heat resistance test, the dimensional change rates before and after the moist heat resistance test, and the results of the determination of the bending resistance are shown in Table 2. In Table 2, "4.0 mm" and "3.8 mm" both refer to the thickness of the spacer used in the evaluation of the bending resistance.

[0164] [Table 2]

[0165]

[0166] As shown in Table 2, in Examples 1 to 9, the dimensional change rate in the MD direction before and after the heat resistance test was -0.10% to 0.10%. In Examples 1 to 9, the dimensional change rate in the MD direction before and after the moist heat resistance test was 0.01% to 0.20%.

[0167] As shown in Table 2, in Examples 1 to 9, the determination result of the bending resistance at high temperature when a spacer with a thickness of 4.0 mm was used was A. Therefore, the antireflection films of Examples 1 to 9 were excellent in bending resistance at high temperature. In Examples 1 to 9, the determination result of the bending resistance at high temperature and high humidity when a spacer with a thickness of 4.0 mm was used was A. Therefore, the antireflection films of Examples 1 to 9 were excellent in bending resistance at high temperature and high humidity.

[0168] As shown in Table 2, in Comparative Examples 1 to 5, the dimensional change rate before and after the heat resistance test was less than -0.10% in either the TD direction or the MD direction. In Comparative Examples 1 to 5, the dimensional change rate before and after the moist heat resistance test was less than 0.01% in either the TD direction or the MD direction.

[0169] As shown in Table 2, in Comparative Examples 1 to 5, the determination result of the bending resistance at high temperature when the spacer with a thickness of 4.0 mm was used was B. Therefore, the antireflection films of Comparative Examples 1 to 5 were not excellent in bending resistance at high temperature. In Comparative Examples 1 to 5, the determination result of the bending resistance at high temperature and high humidity when the spacer with a thickness of 4.0 mm was used was B. Therefore, the antireflection films of Comparative Examples 1 to 5 were not excellent in bending resistance at high temperature and high humidity.

[0170] The above results show that according to the present invention, an antireflection film having excellent bending resistance in a severe environment can be provided.

[0171] Description of Reference Numerals

[0172] 10, 20: anti-reflection film; 11: transparent film substrate; 12: hard coating layer; 13: anti-reflection layer; 18: primer layer; 19: antifouling layer; 21: adhesive layer; 100: image display device; 101: image display panel.

Claims

1. An anti-reflection film, in, The invention has: a transparent film substrate, a hard coating layer and an anti-reflection layer, When a heat resistance test was performed in an environment at a temperature of 85° C. for 48 hours, the dimensional change rate in any one side direction before and after the heat resistance test was −0.10% or more and 0.10% or less.

2. The antireflection film according to claim 1, in, The dimensional change rate in the direction perpendicular to the direction of the side before and after the heat resistance test is -0.10% or more and 0.10% or less.

3. An anti-reflective film, in, The invention has: a transparent film substrate, a hard coating layer and an anti-reflection layer, When a moisture and heat resistance test was performed under an environment of a temperature of 60° C. and a relative humidity of 95% for 48 hours, the dimensional change rate in any one side direction before and after the moisture and heat resistance test was 0.01% or more and 0.20% or less.

4. The antireflection film according to claim 3, in, The dimensional change rate in the direction perpendicular to the direction of the side before and after the moisture and heat resistance test is 0.01% or more and 0.20% or less.

5. The antireflection film according to claim 1 or 3, in, The transparent film substrate is a polyethylene terephthalate film.

6. The antireflection film according to claim 1 or 3, in, The anti-reflection layer has a thickness of 150 nm or more and 280 nm or less.

7. The antireflection film according to claim 1 or 3, in, The antireflection film further includes a primer layer disposed between the hard coat layer and the antireflection layer.

8. The antireflection film according to claim 1 or 3, in, The antireflection film further includes an antifouling layer disposed on a side of the antireflection layer opposite to the hard coating layer.

9. The antireflection film according to claim 1 or 3, in, The antireflection film further includes a pressure-sensitive adhesive layer disposed on the side of the transparent film substrate opposite to the hard coat layer.

10. An image display device, in, The invention comprises: an image display panel; and the antireflection film according to claim 1 or 3, which is arranged on the visible side of the image display panel.

11. A method for producing an antireflection film, which is the method for producing an antireflection film according to claim 1 or 3, include: Step Sa, forming the antireflection layer on the side of the hard coating layer opposite to the transparent film substrate side by using a roll-to-roll sputtering film forming device; as well as Step Sb: after the step Sa, heating the laminated body on which the antireflection layer is formed.

12. The method for producing an antireflection film according to claim 11, in, In the step Sb, the stacked body is heated at a temperature of 110° C. or higher.