Gallium nitride power device and preparation method thereof

The gallium nitride power device addresses high electric field-induced breakdown by employing compressive and tensile stress dielectric layers to manage electric field distribution, enhancing breakdown voltage without increasing on-resistance.

CN119096369APending Publication Date: 2024-12-06XIAMEN SANAN INTEGRATED CIRCUIT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480001559.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Gallium nitride (GaN) HEMT devices face breakdown due to excessively high electric field strength near the drain end, which limits their application in high-voltage fields without increasing on-resistance.

Method used

A gallium nitride power device design featuring a substrate with an epitaxial layer, gate structure, source, and drain, where a first dielectric layer comprising compressive and tensile stress dielectric layers is arranged to gradually change widths along specific directions, reducing peak electric fields and maintaining or reducing on-resistance.

Benefits of technology

Effectively reduces peak electric fields at the gate edge near the drain, preventing device breakdown while maintaining or reducing overall on-resistance through optimized stress dielectric layer configurations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096369A_ABST
    Figure CN119096369A_ABST
Patent Text Reader

Abstract

The invention discloses a gallium nitride power device and a preparation method thereof. The gallium nitride power device comprises a substrate (10), an epitaxial layer (20), a gate structure (30), a source electrode (40), a drain electrode (50) and a first dielectric layer (60), the epitaxial layer (20) between the gate structure (30) and the drain electrode (50) is defined as a first region (A1) of the epitaxial layer (20), and the epitaxial layer (20) between the gate structure (30) and the source electrode (40) is defined as a second region (A2) of the epitaxial layer (20); the first dielectric layer (60) is arranged on the side, away from the substrate (10), of the epitaxial layer (20) and located in the first area (A1), the first dielectric layer (60) comprises a pressure stress dielectric layer (61) and a tensile stress dielectric layer (62) which are arranged on the same layer and extend in the first direction, pointing to the drain electrode (50), of the gate structure (30), the width of the pressure stress dielectric layer (61) is gradually reduced in the first direction, and the width of the tensile stress dielectric layer (62) is gradually reduced in the second direction. The width of the tensile stress dielectric layer (62) is gradually increased, and the compressive stress dielectric layer (61) is connected with the tensile stress dielectric layer (62) in a second direction intersecting with the first direction, through the arrangement, the problem that the electric field intensity of the edge of the end, close to the drain electrode (50), of the grid electrode (32) is too high, and consequently device breakdown is easily caused can be solved; and the effect of not increasing or even reducing the overall on-resistance of the device is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a gallium nitride power device and a method for preparing the same. Background Art

[0002] Gallium nitride (GaN) has attracted widespread attention in the field of high-voltage power devices due to its wide bandgap and high electron mobility. However, one of the important factors limiting the application of GaN HEMT (High Electron Mobility Transistor) devices in the high-voltage field is the device breakdown caused by the excessively high electric field strength at the gate near the drain end.

[0003] Therefore, how to reduce the peak electric field at the gate edge close to the drain end in the GaN HEMT device without increasing the on-resistance of the device, thereby increasing the breakdown voltage of the device, is an urgent problem to be solved. Summary of the invention

[0004] The gallium nitride power device and the preparation method thereof provided in the present application can solve the problem in existing GaN HEMT devices that the device is easily broken down due to the excessively high electric field strength near the drain end edge of the gate.

[0005] In order to solve the above technical problems, a technical solution provided by the present application is to provide a gallium nitride power device, including:

[0006] substrate;

[0007] An epitaxial layer is disposed on one side of the substrate;

[0008] A gate structure, a source electrode and a drain electrode are arranged at intervals on a side of the epitaxial layer away from the substrate, and the source electrode and the drain electrode are located on both sides of the gate structure; wherein the epitaxial layer between the gate structure and the drain electrode is defined as a first region of the epitaxial layer, and the epitaxial layer between the gate structure and the source electrode is defined as a second region of the epitaxial layer;

[0009] A first dielectric layer is arranged on a side of the epitaxial layer away from the substrate and located in the first region, wherein the first dielectric layer includes a compressive stress dielectric layer and a tensile stress dielectric layer arranged in the same layer and extending along a first direction;

[0010] Among them, in the first direction, the width of the compressive stress dielectric layer gradually decreases, and the width of the tensile stress dielectric layer gradually increases; in the second direction, the compressive stress dielectric layer is connected to the tensile stress dielectric layer, the first direction is the direction in which the gate structure points to the drain, and the second direction intersects with the first direction.

[0011] In order to solve the above technical problems, another technical solution provided by the present application is: to provide a method for preparing a gallium nitride power device, comprising:

[0012] providing a substrate;

[0013] An epitaxial layer is formed on one side of the substrate; wherein the epitaxial layer is defined with a gate structure region, a source region and a drain region, and the source region and the drain region are located on both sides of the gate structure region; and the epitaxial layer located between the gate structure region and the drain region is defined as a first region of the epitaxial layer, and the epitaxial layer located between the gate structure region and the source region is defined as a second region of the epitaxial layer;

[0014] A first dielectric layer is formed on a side of the epitaxial layer corresponding to the first region away from the substrate, wherein the first dielectric layer includes a compressive stress dielectric layer and a tensile stress dielectric layer which are arranged in the same layer and extend along a first direction, and in the first direction, the width of the compressive stress dielectric layer gradually decreases, and the width of the tensile stress dielectric layer gradually increases; in the second direction, the compressive stress dielectric layer is connected to the tensile stress dielectric layer; the first direction is the direction from the gate structure region to the drain region, and the second direction intersects with the first direction.

[0015] Beneficial effects of the present application: Different from the prior art, the gallium nitride power device and the preparation method thereof provided by the present application, the gallium nitride power device comprises a substrate, an epitaxial layer, a gate structure, a source, a drain and a first dielectric layer; wherein the epitaxial layer is arranged on one side of the substrate; the gate structure, the source and the drain are arranged at intervals on the side of the epitaxial layer away from the substrate; wherein the epitaxial layer located between the gate structure and the drain is defined as the first region of the epitaxial layer, and the epitaxial layer located between the gate structure and the source is defined as the second region of the epitaxial layer; the first dielectric layer is arranged on the side of the epitaxial layer away from the substrate and is located in the first region, wherein the first dielectric layer comprises a compressive stress dielectric layer and a tensile stress dielectric layer arranged in the same layer and extending along a first direction layer, and in a first direction from the gate structure to the drain, the width of the compressive stress dielectric layer gradually decreases, the width of the tensile stress dielectric layer gradually increases, and in a second direction intersecting with the first direction, the compressive stress dielectric layer is connected to the tensile stress dielectric layer, so that in the drift region at the edge of the gate, the width occupied by the compressive stress dielectric is wider, so the 2DEG concentration below the gate edge is small, which can effectively reduce the peak electric field, thereby solving the problem that the electric field intensity of the gate near the drain end edge is too high and easily causes device breakdown, and in the drift region at the edge of the drain, the width occupied by the tensile stress dielectric is wider, so the 2DEG concentration below the drain edge is high, achieving the effect of not increasing or even reducing the overall on-resistance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0017] Figure 1 is a schematic diagram of a portion of the structure of a gallium nitride power device provided in the first embodiment of the present application at a first viewing angle;

[0018] Figure 2 is a schematic diagram of a portion of the structure of the gallium nitride power device provided by the first embodiment of the present application at a second viewing angle after the passivation layer is omitted;

[0019] Figure 3 The first embodiment of the present application is as follows Figure 2 Partial structural cross-sectional view along line AA;

[0020] Figure 4 The first embodiment of the present application is as follows Figure 2 Partial structural cross-sectional view along line BB;

[0021] Figure 5 is a partial structural schematic diagram of a gallium nitride power device provided in the second embodiment of the present application at a second viewing angle;

[0022] Figure 6 is a partial structural schematic diagram of a gallium nitride power device provided in the third embodiment of the present application at a second viewing angle;

[0023] Figure 7 is a partial structural schematic diagram of a gallium nitride power device provided in the fourth embodiment of the present application at a second viewing angle;

[0024] Figure 8 It is a schematic diagram of a process for preparing a gallium nitride power device provided in an embodiment of the present application;

[0025] Fig. 9 yes Figure 8 A schematic diagram of a flow chart of an embodiment of step S3;

[0026] Fig.10 yes Figure 8 Schematic diagram of an intermediate product of a gallium nitride power device after step S1;

[0027] Fig.11 yes Figure 8 A schematic diagram of an intermediate product of a gallium nitride power device after step S2;

[0028] Fig.12 yes Figure 8 A schematic diagram of an intermediate product of a gallium nitride power device having a gate structure, a source electrode and a drain electrode prepared after step S2 and before step S3;

[0029] Fig.13 yes Fig. 9 A schematic diagram of an intermediate product of a gallium nitride power device after step S31;

[0030] Fig.14 yes Fig. 9 A schematic diagram of an intermediate product of a gallium nitride power device after step S32;

[0031] Fig.15 yes Fig. 9 A schematic diagram of an intermediate product of a gallium nitride power device after step S33;

[0032] Fig.16 yes Fig. 9 A product schematic diagram of a gallium nitride power device after step S34.

[0033] Figure Number:

[0034] Substrate-10; base-11; transition layer-12; epitaxial layer-20; first semiconductor layer-21; second semiconductor layer-22; gate structure-30; cap layer-31; gate-32; first dielectric layer-60; compressive stress dielectric layer-61; tensile stress dielectric layer-62; second dielectric layer-70; passivation layer 80;

[0035] Tensile stress dielectric material layer-601; Compressive stress dielectric material layer-602;

[0036] First region-A1; second region-A2; gate structure region-B1; source region-B2; drain region-B3. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0038] In the following description, for the purpose of explanation rather than limitation, specific details such as specific system structures, interfaces, and technologies are provided to facilitate a thorough understanding of the present application.

[0039] The terms "first", "second" and "third" in this application are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second" and "third" may explicitly or implicitly include at least one of the features. All directional indications (such as up, down, left, right, front, back...) in the embodiments of the present application are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. The terms "including" and "having" in the embodiments of the present application and any of their variations are intended to cover non-exclusive inclusions.

[0040] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0041] The present application is described in detail below with reference to the accompanying drawings and embodiments.

[0042] See also Figure 1-Figure 7 , Figure 1 is a schematic diagram of a portion of the structure of a gallium nitride power device provided in the first embodiment of the present application at a first viewing angle; Figure 2 is a schematic diagram of a portion of the structure of the gallium nitride power device provided by the first embodiment of the present application at a second viewing angle after the passivation layer is omitted; Figure 3 The first embodiment of the present application is as follows Figure 2 Partial structural cross-sectional view along line AA; Figure 4 The first embodiment of the present application is as follows Figure 2 Partial structural cross-sectional view along line BB; Figure 5 is a partial structural schematic diagram of a gallium nitride power device provided in the third embodiment of the present application at a second viewing angle; Figure 6 is a partial structural schematic diagram of a gallium nitride power device provided in the fourth embodiment of the present application at a second viewing angle; Figure 7 It is a schematic diagram of a partial structure of a gallium nitride power device provided in the fourth embodiment of the present application at a second viewing angle.

[0043] Specifically, the gallium nitride power device provided in the present application includes a substrate 10 , an epitaxial layer 20 , a gate structure 30 , a source 40 , a drain 50 and a first dielectric layer 60 .

[0044] In one embodiment, the substrate 10 includes a base 11 and a transition layer 12. Silicon (Si) material or sapphire (Al2O3) material can be used as the base 11, and AlGaN material can be used as the transition layer 12.

[0045] In other embodiments, the substrate 10 may also only include the base 11 .

[0046] The epitaxial layer 20 includes a first semiconductor layer 21 and a second semiconductor layer 22. The first semiconductor layer 21 is disposed on one side of the substrate 10 as a buffer layer of the device, and the second semiconductor layer 22 is disposed on the side of the first semiconductor layer 21 away from the substrate 10 as a barrier layer of the device.

[0047] A two-dimensional electron gas (2DEG) is formed between the interfaces of the first semiconductor layer 21 and the second semiconductor layer 22 to serve as a channel layer of the device.

[0048] In the embodiment of the present application, the material of the first semiconductor layer 21 includes GaN; the material of the second semiconductor layer 22 includes AlGaN.

[0049] The gate structure 30 , the source 40 , and the drain 50 are spaced apart on the side of the epitaxial layer 20 away from the substrate 10 , and are specifically arranged on the surface of the second semiconductor layer 22 away from the first semiconductor layer 21 . The source 40 and the drain 50 are located on opposite sides of the gate structure 30 .

[0050] In one embodiment, see Figure 3 or Figure 4 The gate structure 30 includes a cap layer 31 and a gate 32. The cap layer 31 is disposed between the gate 32 and the second semiconductor layer 22. Taking the gallium nitride power device as an enhancement-mode device as an example, the cap layer 31 is used as a P-type nitride gate layer. The cap layer 31 is also used to deplete the 2DEG under the gate structure 30 to form an enhancement-mode device. Specifically, the material of the cap layer 31 includes but is not limited to p-GaN, p-AlGaN, p-InGaN or p-InAlGaN, etc., which are not limited here.

[0051] The gate 32, source 40 and drain 50 are made of conductive metal materials for electrical connection with an external circuit. In some embodiments, the conductive metal system of the gate 32, source 40 and drain 50 includes but is not limited to Ti, Al, Ni, Au or Ta, etc., and alloys or compounds containing the above metal systems.

[0052] Among them, combined Figure 1 , Figure 2 , Figure 5-Figure 7In the embodiment of the present application, the epitaxial layer 20 between the gate structure 30 and the drain 50 is defined as the first region A1 of the epitaxial layer 20, and the epitaxial layer 20 between the gate structure 30 and the source 40 is defined as the second region A2 of the epitaxial layer 20; the first dielectric layer 60 is disposed on the side of the epitaxial layer 20 away from the substrate 10 and is located in the first region A1, wherein the first dielectric layer 60 includes a compressive stress dielectric layer 61 and a tensile stress dielectric layer 62 disposed in the same layer and extending in a first direction from the gate structure 30 to the drain 50. In the first direction, the width of the compressive stress dielectric layer 61 gradually decreases, and the width of the tensile stress dielectric layer 62 gradually increases, and in the second direction intersecting with the first direction, the compressive stress dielectric layer 61 is connected to the tensile stress dielectric layer 62.

[0053] The first direction may be understood as the length direction, and the second direction may be understood as the width direction.

[0054] The term “gradually decrease” in the present application means a linear decrease or a step-by-step decrease; the term “gradually increase” in the present application means a linear increase or a step-by-step increase.

[0055] In this application, “the compressive stress dielectric layer 61 is in contact with the tensile stress dielectric layer 62 ” means that the edges of the compressive stress dielectric layer 61 and the tensile stress dielectric layer 62 close to each other are in contact with each other without any gap therebetween.

[0056] In some embodiments, the material of the compressive stress dielectric layer 61 is one or a combination of silicon nitride, silicon oxide, and silicon oxynitride, and the compressive stress dielectric layer 61 is used to form compressive stress on the underlying film layer. The material of the tensile stress dielectric layer 62 is one or a combination of silicon nitride, silicon oxide, and silicon oxynitride, and the tensile stress dielectric layer 62 is used to form tensile stress on the underlying film layer.

[0057] Specifically, the 2DEG concentration is closely related to the intensity of polarization. The compressive stress dielectric layer 61 will offset the tensile stress on the barrier layer, thereby reducing the piezoelectric polarization, and then the 2DEG concentration below the compressive stress dielectric layer 61 is reduced, and the threshold voltage of the device is increased. At the same time, because the 2DEG concentration is reduced, the depletion region formed by the device in the off state is larger, the electric field strength is reduced, and the peak electric field at the edge of the gate 32 close to the drain 50 end is also reduced. The current collapse of the device is closely related to the electric field strength. The stronger the electric field, the more serious the current collapse. Therefore, the compressive stress dielectric layer 61 can improve the current collapse of the device. On the other hand, the tensile stress dielectric layer 62 can enhance the piezoelectric polarization, thereby increasing the 2DEG concentration, and then reducing the resistance of the channel. Therefore, the gallium nitride device provided in the present application can more effectively adjust the electric field distribution in the drift region by disposing a compressive stress dielectric layer 61 and a tensile stress dielectric layer 62 whose widths gradually increase or decrease along the first direction on the first area A1, thereby improving the breakdown voltage of the device, and can achieve the effect of not increasing or even reducing the on-resistance of the device by adjusting the widths of the compressive stress dielectric layer 61 and the tensile stress dielectric layer 62.

[0058] It can be understood that in the first direction, the width of the compressive stress dielectric layer 61 gradually decreases, and the width of the tensile stress dielectric layer 62 gradually increases, and in the second direction intersecting with the first direction, the compressive stress dielectric layer 61 is connected to the tensile stress dielectric layer 62, so that in the drift region at the edge of the gate 32, the width occupied by the compressive stress dielectric is wider, so the 2DEG concentration below the edge of the gate 32 is small, which can effectively reduce the peak electric field, thereby solving the problem that the electric field strength at the edge of the gate 32 close to the drain 50 is too high and easily causes device breakdown, and in the drift region at the edge of the drain 50, the width occupied by the tensile stress dielectric is wider, so the 2DEG concentration below the edge of the drain 50 is high, achieving the effect of not increasing or even reducing the overall on-resistance of the device.

[0059] In one embodiment, the stress value of the compressive stress dielectric layer 61 ranges from -0.1 to -2 GPa (where "-" represents compressive stress). For example, the stress value of the compressive stress dielectric layer 61 is -0.1 GPa, -0.5 GPa, -1 GPa, -1.5 GPa or -2 GPa, etc., which is not limited here and is selected according to actual conditions.

[0060] In one embodiment, the tensile stress of the tensile stress dielectric layer 62 ranges from 0.1 to 2 GPa. For example, the stress value of the tensile stress dielectric layer 62 is 0.1 GPa, 0.5 GPa, 1 GPa, 1.5 GPa or 2 GPa, etc., which is not limited here and is selected according to actual conditions.

[0061] In some embodiments, the number of the compressive stress dielectric layer 61 and the tensile stress dielectric layer 62 may be one or more.

[0062] For example, see Figure 5 , the number of the compressive stress dielectric layer 61 and the number of the tensile stress dielectric layer 62 may both be one.

[0063] Alternatively, see Figure 6 The number of the compressive stress dielectric layer 61 may be one, the number of the tensile stress dielectric layer 62 may be two, and the two tensile stress dielectric layers 62 are located on both sides of the compressive stress dielectric layer 61 and connected to the compressive stress dielectric layer 61 .

[0064] Alternatively, see Figure 7 The number of the tensile stress dielectric layer 62 may be one, the number of the compressive stress dielectric layer 61 may be two, and the two compressive stress dielectric layers 61 are located on both sides of the tensile stress dielectric layer 62 and connected to the tensile stress dielectric layer 62 .

[0065] Alternatively, see Figure 2 The number of the compressive stress dielectric layers 61 and the number of the tensile stress dielectric layers 62 are both multiple, and the multiple compressive stress dielectric layers 61 and the multiple tensile stress dielectric layers 62 are alternately arranged and connected along a second direction perpendicular to the first direction.

[0066] The shape of each compressive stress dielectric layer 61 and each tensile stress dielectric layer 62 can be a trapezoid (isosceles trapezoid, right-angled trapezoid) or a triangle (such as an isosceles triangle, right-angled triangle). The figure in this application takes the trapezoid as an example.

[0067] Specifically, the arrangement of the multiple compressive stress dielectric layers 61 and the multiple tensile stress dielectric layers 62 in alternation can make the 2DEG in the drift region between the gate structure 30 and the drain 50 evenly distributed in the second direction, with a lower electric field peak.

[0068] This application takes the case where there are a plurality of compressive stress dielectric layers 61 and tensile stress dielectric layers 62 as an example for description.

[0069] For details, see Figure 2 In the second direction, the adjacent compressive stress dielectric layer 61 and tensile stress dielectric layer 62 are arranged in contact with each other, and there is no gap between them. Compared with the scheme with a gap between the compressive stress dielectric layer 61 and the tensile stress dielectric layer 62, the embodiment of the present application does not need to etch the barrier layer (second semiconductor layer 22) corresponding to the gap area, so the process window is better. And more drift areas in the device can be used.

[0070] In the present application, at one end near the gate structure 30, the total width of the plurality of compressive stress dielectric layers 61 along the second direction is the first total width, and the total width of the plurality of tensile stress dielectric layers 62 along the second direction is the second total width, and the first total width is greater than the second total width. In this way, the width occupied by the compressive stress dielectric is wider in the drift region at the edge of the gate structure 30, so the 2DEG concentration under the edge of the gate 32 is small, which can effectively reduce the peak electric field, thereby solving the problem that the electric field strength at the edge of the gate 32 near the drain 50 end is too high and easily causes device breakdown.

[0071] At one end close to the drain 50, the total width of the plurality of tensile stress dielectric layers 62 along the second direction is the third total width, and the total width of the plurality of compressive stress dielectric layers 61 along the second direction is the fourth total width, and the third total width is greater than the fourth total width. In this way, the width occupied by the tensile stress dielectric in the drift region at the edge of the drain 50 is wider, so that the 2DEG concentration below the edge of the drain 50 is high, achieving the effect of not increasing or even reducing the overall on-resistance of the device.

[0072] The following description will be made by taking an example that in the first direction, the width of the compressive stress dielectric layer 61 decreases linearly and the width of the tensile stress dielectric layer 62 increases linearly.

[0073] For details, see Figure 2 Since in the first direction, the width of the compressive stress dielectric layer 61 gradually decreases, and the width of the tensile stress dielectric layer 62 gradually increases, and in the second direction intersecting the first direction, the compressive stress dielectric layer 61 is connected to the tensile stress dielectric layer 62, therefore, when the number of the compressive stress dielectric layers 61 and the tensile stress dielectric layers 62 is multiple and alternates and is connected, at one end close to the gate structure 30, the width of each compressive stress dielectric layer 61 is the same and is the first width w1, and the width of each tensile stress dielectric layer 62 is the same and is the second width w2; the first width w1 is greater than the second width w2; the distance between two adjacent compressive stress dielectric layers 61 is equal to the second width w2, and the distance between two adjacent tensile stress dielectric layers 62 is equal to the first width w1. At one end close to the drain 50, the width of each compressive stress dielectric layer 61 is the same and is the third width w3, the width of each tensile stress dielectric layer 62 is the same and is the fourth width w4, and the fourth width w4 is greater than the third width w3; the distance between two adjacent compressive stress dielectric layers 61 is equal to the fourth width w4; the distance between two adjacent tensile stress dielectric layers 62 is equal to the third width w3.

[0074] And it can be understood that the first width w1 is equal to the fourth width w4, and the second width w2 is equal to the third width w3.

[0075] It should be noted that due to Figure 2The shape of the compressive stress dielectric layer 61 shown is an isosceles trapezoid. Due to the device structure design, the compressive stress dielectric layer 61 located at the edge of the device is not complete along the width direction. Specifically, the width of the end of the compressive stress dielectric layer 61 located at the edge of the device close to the edge of the gate structure 30 is less than the first width w1, and the width of the end of the compressive stress dielectric layer 61 located at the edge of the device close to the edge of the drain 50 is less than or equal to the third width w3. Similarly, the width of the end of the tensile stress dielectric layer 62 located at the edge of the device close to the edge of the gate structure 30 is less than or equal to the second width w2, and the width of the end of the tensile stress dielectric layer 62 located at the edge of the device close to the edge of the drain 50 is less than the fourth width w4.

[0076] It can be understood that when the shape of the compressive stress dielectric layer 61 is a right-angled trapezoid or a right-angled triangle, the above situation can be avoided by arranging the right-angled side of the right-angled trapezoid or the right-angled triangle at the edge of the device.

[0077] In one embodiment, the first width w1 and the fourth width w4 are both in the range of 0.1 um to 1 mm, and the second width w2 and the third width w3 are both in the range of 0 to 1 mm.

[0078] For example, the first width w1 and the fourth width w4 are the same and are both 0.1um, 5um, 50um, 200um, 500um, 700um or 1mm, etc. The second width w2 and the third width w3 are the same and are both 0um (triangle), 0.1um, 5um, 50um, 200um, 500um, 700um or 1mm, etc., and are not limited here, as long as the first total width is greater than the second total width, and the third total width is greater than the fourth total width.

[0079] Specifically, by adjusting the specific parameters of the first width w1, the second width w2, the third width w3 and the fourth width w4, the electric field distribution in the drift region can be more effectively adjusted, thereby improving the breakdown voltage of the device and achieving the effect of not increasing or even reducing the on-resistance of the device.

[0080] In one embodiment, the compressive stress dielectric layer 61 and the tensile stress dielectric layer 62 have the same thickness and have a first thickness H1, wherein the first thickness H1 ranges from 10 to 1000 nm. For example, the first thickness H1 may be 10 nm, 100 nm, 300 nm, 500 nm, 700 nm or 1000 nm, etc., which is not limited here and is set according to actual conditions.

[0081] Specifically, if the first thickness H1 is too thin, the passivation effect of the dielectric layer is poor. If the first thickness H1 is too thick, the field plate metal subsequently deposited on the dielectric layer is too far away from the 2DEG, and the regulating effect on the 2DEG is poor.

[0082] In one embodiment, see Figure 1 , Figure 3 and Figure 4 The gallium nitride power device further includes a second dielectric layer 70, which is disposed on the side of the epitaxial layer 20 away from the substrate 10 and located in the second region A2. The second dielectric layer 70 is a tensile stress dielectric layer, which can be made of the same material as the tensile stress dielectric layer 62. Specifically, the second dielectric layer 70 is a tensile stress dielectric layer, which can increase the 2DEG concentration between the source and the gate and reduce the on-resistance.

[0083] Furthermore, the periphery of the gate structure 30 and a certain range thereof are defined as a gate structure region, and the gate structure region has a passivation layer 80 that wraps the gate structure 30, and the material of the passivation layer 80 is the same as the material of the tensile stress dielectric layer 62, thereby increasing the 2DEG concentration under the gate structure 30 and reducing the on-resistance.

[0084] Specifically, the gallium nitride power device provided by the present application is arranged in a first direction, the width of the compressive stress dielectric layer 61 in the first dielectric layer 60 gradually decreases, and the width of the tensile stress dielectric layer 62 gradually increases, and in a second direction intersecting with the first direction, the compressive stress dielectric layer 61 is connected to the tensile stress dielectric layer 62, so that in the drift region at the edge of the gate 32, the width occupied by the compressive stress dielectric is wider, so the 2DEG concentration below the edge of the gate 32 is small, which can effectively reduce the peak electric field, thereby solving the problem that the electric field strength at the edge of the gate 32 close to the drain 50 is too high and easily causes device breakdown, and in the drift region at the edge of the drain 50, the width occupied by the tensile stress dielectric is wider, so the 2DEG concentration below the edge of the drain 50 is high, achieving the effect of not increasing or even reducing the overall on-resistance of the device.

[0085] See also Figure 8-Figure 16 , Figure 8 It is a schematic diagram of a process for preparing a gallium nitride power device provided in an embodiment of the present application; Fig. 9 yes Figure 8 A schematic diagram of a flow chart of an embodiment of step S3; Fig.10 yes Figure 8 Schematic diagram of an intermediate product of a gallium nitride power device after step S1; Fig.11 yes Figure 8 A schematic diagram of an intermediate product of a gallium nitride power device after step S2; Fig.12 yes Figure 8 A schematic diagram of an intermediate product of a gallium nitride power device having a gate structure, a source electrode and a drain electrode prepared after step S2 and before step S3; Fig.13 yes Fig. 9 A schematic diagram of an intermediate product of a gallium nitride power device after step S31; Fig.14 yes Fig. 9A schematic diagram of an intermediate product of a gallium nitride power device after step S32; Fig.15 yes Fig. 9 A schematic diagram of an intermediate product of a gallium nitride power device after step S33; Fig.16 yes Fig. 9 A product schematic diagram of a gallium nitride power device after step S34.

[0086] Specifically, the present application also provides a method for preparing a gallium nitride power device, comprising:

[0087] Step S1: providing a substrate 10 .

[0088] In one embodiment, see Fig.10 The substrate 10 includes a base 11 and a transition layer 12. Silicon (Si) material or sapphire (Al2O3) material can be used as the base 11; AlGaN material can be used as the transition layer 12.

[0089] In other embodiments, the substrate 10 may also only include the base 11 .

[0090] Step S2: forming an epitaxial layer 20 on one side of the substrate 10; wherein the epitaxial layer 20 is defined with a gate structure region B1, a source region B2 and a drain region B3, and the source region B2 and the drain region B3 are located on both sides of the gate structure region B1; and the epitaxial layer 20 located between the gate structure region B1 and the drain region B3 is defined as a first region A1 of the epitaxial layer 20, and the epitaxial layer 20 located between the gate structure region B1 and the source region B2 is defined as a second region A2 of the epitaxial layer 20.

[0091] See Fig.11 , wherein the epitaxial layer 20 includes a first semiconductor layer 21 and a second semiconductor layer 22. The first semiconductor layer 21 is disposed on one side of the substrate 10 as a buffer layer of the device, and the second semiconductor layer 22 is disposed on the side of the first semiconductor layer 21 away from the substrate 10 as a barrier layer of the device. Specifically, a two-dimensional electron gas (2DEG) is also formed between the interface of the first semiconductor layer 21 and the second semiconductor layer 22 to serve as a channel layer of the device.

[0092] In the embodiment of the present application, the material of the first semiconductor layer 21 includes GaN; the material of the second semiconductor layer 22 includes AlGaN.

[0093] Step S3: forming a first dielectric layer 60 on the side of the epitaxial layer 20 corresponding to the first region A1 away from the substrate 10, wherein the first dielectric layer 60 includes a compressive stress dielectric layer 61 and a tensile stress dielectric layer 62 which are arranged in the same layer and extend along a first direction, and in the first direction, the width of the compressive stress dielectric layer 61 gradually decreases, and the width of the tensile stress dielectric layer 62 gradually increases, and in the second direction, the compressive stress dielectric layer 61 is connected to the tensile stress dielectric layer 62.

[0094] The first direction is the direction from the gate structure region B1 to the drain region B3, and the second direction intersects the first direction. The first direction can be understood as the length direction, and the second direction can be understood as the width direction.

[0095] In some embodiments, the number of the compressive stress dielectric layer 61 and the tensile stress dielectric layer 62 may be one or more, which will not be described in detail herein. Figure 2 , Figure 5-Figure 7 .

[0096] The present application takes a plurality of compressive stress dielectric layers 61 and tensile stress dielectric layers 62 as an example for description.

[0097] Among them, at one end close to the gate structure 30, the total width of the plurality of compressive stress dielectric layers 61 along the second direction is the first total width, the total width of the plurality of tensile stress dielectric layers 62 along the second direction is the second total width, and the first total width is greater than the second total width. In this way, the width occupied by the compressive stress dielectric in the drift region at the edge of the gate structure 30 is wider, so the 2DEG concentration under the edge of the gate 32 is small, which can effectively reduce the peak electric field, thereby solving the problem that the electric field strength at the edge of the gate 32 close to the drain 50 is too high and easily causes device breakdown.

[0098] At one end close to the drain 50, the total width of the plurality of tensile stress dielectric layers 62 along the second direction is the third total width, and the total width of the plurality of compressive stress dielectric layers 61 along the second direction is the fourth total width, and the third total width is greater than the fourth total width. In this way, the width occupied by the tensile stress dielectric in the drift region at the edge of the drain 50 is wider, so that the 2DEG concentration below the edge of the drain 50 is high, achieving the effect of not increasing or even reducing the overall on-resistance of the device.

[0099] Specifically, the 2DEG concentration is closely related to the intensity of polarization. The compressive stress dielectric layer 61 will offset the tensile stress on the barrier layer, thereby reducing the piezoelectric polarization, and then the 2DEG concentration below the compressive stress dielectric layer 61 is reduced, and the threshold voltage of the device is increased. At the same time, because the 2DEG concentration is reduced, the depletion region formed by the device in the off state is larger, the electric field strength is reduced, and the peak electric field at the edge of the gate 32 close to the drain 50 end is also reduced. The current collapse of the device is closely related to the electric field strength. The stronger the electric field, the more serious the current collapse. Therefore, the compressive stress dielectric layer 61 can improve the current collapse of the device. On the other hand, the tensile stress dielectric layer 62 can enhance the piezoelectric polarization, thereby increasing the 2DEG concentration, and then reducing the resistance of the channel.

[0100] Therefore, in the preparation method provided by the present application, in a first direction, the width of the compressive stress dielectric layer 61 gradually decreases, and the width of the tensile stress dielectric layer 62 gradually increases, and in a second direction intersecting with the first direction, the compressive stress dielectric layer 61 is connected to the tensile stress dielectric layer 62, so that in the drift region at the edge of the gate 32, the width occupied by the compressive stress dielectric is wider, so the 2DEG concentration below the edge of the gate 32 is small, which can effectively reduce the peak electric field, thereby solving the problem that the electric field strength at the edge of the gate 32 close to the drain 50 is too high and easily causes device breakdown, and in the drift region at the edge of the drain 50, the width occupied by the tensile stress dielectric is wider, so the 2DEG concentration below the edge of the drain 50 is high, achieving the effect of not increasing or even reducing the overall on-resistance of the device.

[0101] In one embodiment, see Fig.12 Before forming the first dielectric layer 60 on the side of the epitaxial layer 20 corresponding to the first region A1 away from the substrate 10 , a gate structure 30 is formed on the surface of the epitaxial layer 20 corresponding to the gate structure region B1 away from the substrate 10 .

[0102] Of course, in other embodiments, not shown, after forming the first dielectric layer 60 on the side of the epitaxial layer 20 corresponding to the first region A1 away from the substrate 10, a gate structure 30 may be formed on the surface of the epitaxial layer 20 corresponding to the gate structure region B1 away from the substrate 10, which is not limited here.

[0103] The gate structure 30 includes a cap layer 31 and a gate 32. Taking the gallium nitride power device as an enhancement-mode device as an example, the cap layer 31 is also used to deplete the 2DEG under the gate structure 30 to form an enhancement-mode device. Specifically, the material of the cap layer 31 includes p-GaN, p-AlGaN, p-InGaN or p-InAlGaN, etc., which is not limited here.

[0104] Among them, the materials of the gate 32, the source 40 and the drain 50 are all conductive metal materials, which are used to electrically connect the device with the external circuit. Therefore, the source 40 and the drain 50 can be formed in the same step as the gate 32 in the gate structure 30. For example, before or after the first dielectric layer 60 is formed on the side of the epitaxial layer 20 corresponding to the first region A1 that faces away from the substrate 10, the gate structure 30 is formed on the surface of the epitaxial layer 20 corresponding to the gate structure region B1 that faces away from the substrate 10, and at the same time, the source 40 is formed on the surface of the epitaxial layer 20 corresponding to the source region B2 that faces away from the substrate 10, and the drain 50 is formed on the surface of the epitaxial layer 20 corresponding to the drain region B3 that faces away from the substrate 10. This can simplify the process.

[0105] In other embodiments, before the first dielectric layer 60 is formed on the side of the epitaxial layer 20 corresponding to the first area A1 facing away from the substrate 10, the gate structure 30 may be formed on the surface of the epitaxial layer 20 corresponding to the gate structure area B1 facing away from the substrate 10, and after the first dielectric layer 60 is formed on the side of the epitaxial layer 20 corresponding to the first area A1 facing away from the substrate 10, the source 40 may be formed on the surface of the epitaxial layer 20 corresponding to the source area B2 facing away from the substrate 10, and the drain 50 may be formed on the surface of the epitaxial layer 20 corresponding to the drain area B3 facing away from the substrate 10.

[0106] Alternatively, before forming the first dielectric layer 60 on the side of the epitaxial layer 20 corresponding to the first region A1 away from the substrate 10, the source 40 is formed on the surface of the epitaxial layer 20 corresponding to the source region B2 away from the substrate 10, and the drain 50 is formed on the surface of the epitaxial layer 20 corresponding to the drain region B3 away from the substrate 10, and after forming the first dielectric layer 60 on the side of the epitaxial layer 20 corresponding to the first region A1 away from the substrate 10, the gate structure 30 is formed on the surface of the epitaxial layer 20 corresponding to the gate structure region B1 away from the substrate 10. The specific selection can be made according to the actual device design and is not limited here.

[0107] The conductive metal system of the gate 32 , the source 40 and the drain 50 includes but is not limited to Ti, Al, Ni, Au or Ta, etc., and alloys or compounds containing the above metal systems.

[0108] In one embodiment, the first region A1 includes a compressive stress dielectric layer region (not labeled in the figure) and a tensile stress dielectric layer region (not labeled in the figure); a first dielectric layer 60 is formed on a surface of the epitaxial layer 20 corresponding to the first region A1 that is away from the substrate 10, including:

[0109] Step S31 : growing a tensile stress dielectric material layer 601 on the entire surface of the epitaxial layer 20 facing away from the substrate 10 .

[0110] See Fig.13, wherein the tensile stress dielectric material layer 601 can be formed by MOCVD / LPCVD / PECVD and other methods.

[0111] The material of the tensile stress dielectric material layer 601 may be one or a combination of silicon nitride, silicon oxide and silicon oxynitride.

[0112] The tensile stress of the tensile stress dielectric material layer 601 ranges from 0.1 to 2 GPa. For example, the stress value of the tensile stress dielectric material layer 601 is 0.1 GPa, 0.5 GPa, 1 GPa, 1.5 GPa or 2 GPa, etc., which is not limited here and is selected according to actual conditions.

[0113] In one embodiment, the thickness of the tensile stress dielectric material layer 601 is in the range of 10 to 1000 nm, for example, 10 nm, 100 nm, 300 nm, 500 nm, 700 nm or 1000 nm, etc., which is not limited here and is set according to actual conditions.

[0114] Step S32: pattern-etching the tensile stress dielectric material layer 601 to remove the tensile stress dielectric material layer 601 in the region corresponding to the compressive stress dielectric layer and retaining the tensile stress dielectric material layer 601 in the region corresponding to the tensile stress dielectric layer to form a tensile stress dielectric layer 62 in the first region A1.

[0115] See Fig.14 At one end close to the gate structure 30, each tensile stress dielectric layer 62 has the same width and is the second width w2; the distance between two adjacent tensile stress dielectric layers 62 is equal to the first width w1. At one end close to the drain 50, each tensile stress dielectric layer 62 has the same width and is the fourth width w4, and the distance between two adjacent tensile stress dielectric layers 62 is equal to the third width w3.

[0116] In one embodiment, after the tensile stress dielectric material layer 601 is patterned and etched, the tensile stress dielectric material layer 601 on the second region A2 and the gate structure region B1 is retained to form a second dielectric layer 70 on the second region A2 and a passivation layer 80 on the gate structure 30 .

[0117] It can be understood that since the tensile stress dielectric layer 62, the second dielectric layer 70 and the passivation layer 80 are formed by etching the tensile stress dielectric material layer 601, the tensile stress dielectric layer 62, the second dielectric layer 70 and the passivation layer 80 have the same property parameters as the tensile stress dielectric material layer 601, which will not be described in detail here.

[0118] Specifically, the second dielectric layer 70 and the passivation layer 80 are tensile stress dielectric layers, which can increase the 2DEG concentration between the source and the gate and reduce the on-resistance.

[0119] Step S33 : Continue to grow a compressive stress dielectric material layer 602 on the entire surface of the epitaxial layer 20 facing away from the substrate 10 .

[0120] See Fig.15 , wherein the compressive stress dielectric material layer 602 can be formed by MOCVD / LPCVD / PECVD and other methods.

[0121] In some embodiments, the material of the compressive stress dielectric material layer 602 may be one or a combination of silicon nitride, silicon oxide, and silicon oxynitride.

[0122] In one embodiment, the stress value of the compressive stress dielectric material layer 602 ranges from -0.1 to -2 GPa (where "-" represents compressive stress). For example, the stress value of the compressive stress dielectric material layer 602 is -0.1 GPa, -0.5 GPa, -1 GPa, -1.5 GPa or -2 GPa, etc., which is not limited here and is selected according to actual conditions.

[0123] In one embodiment, the thickness of the compressive stress dielectric material layer 602 is the same as the thickness of the tensile stress dielectric material layer 601, and the thickness ranges from 10 to 1000 nm, for example, 10 nm, 100 nm, 300 nm, 500 nm, 700 nm or 1000 nm, etc., which is not limited here and is set according to actual conditions.

[0124] Step S34: patterning the compressive stress dielectric material layer 602 or chemical mechanical polishing to remove the compressive stress dielectric material layer 602 in the region corresponding to the tensile stress dielectric layer and retain the compressive stress dielectric material layer 602 in the region corresponding to the compressive stress dielectric layer to form a compressive stress dielectric layer 61 in the first region A1.

[0125] See Fig.16 At one end close to the gate structure 30, the width of each compressive stress dielectric layer 61 is the same and is the first width w1; the distance between two adjacent compressive stress dielectric layers 61 is equal to the second width w2. At one end close to the drain 50, the width of each compressive stress dielectric layer 61 is the same and is the third width w3, and the distance between two adjacent compressive stress dielectric layers 61 is equal to the fourth width w4.

[0126] In other embodiments, step S33 and step S34 may be located before step S31 and step S32, which are not limited here. That is, a compressive stress dielectric material layer 602 may be first grown on the side of the epitaxial layer 20 facing away from the substrate 10, and then patterned to form a compressive stress dielectric layer 61, and then a tensile stress dielectric material layer 602 may be grown on the side of the epitaxial layer 20 facing away from the substrate 10 after the compressive stress dielectric layer 61 is formed, and then patterned to form a tensile stress dielectric layer 62, a second dielectric layer 70, and a passivation layer 80.

[0127] The above are only implementation methods of the present application, and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A gallium nitride power device, characterized in that: include: substrate; An epitaxial layer is disposed on one side of the substrate; A gate structure, a source electrode and a drain electrode are arranged at intervals on a side of the epitaxial layer away from the substrate, and the source electrode and the drain electrode are located on both sides of the gate structure; wherein the epitaxial layer between the gate structure and the drain electrode is defined as a first region of the epitaxial layer, and the epitaxial layer between the gate structure and the source electrode is defined as a second region of the epitaxial layer; A first dielectric layer is arranged on a side of the epitaxial layer away from the substrate and located in the first region, wherein the first dielectric layer includes a compressive stress dielectric layer and a tensile stress dielectric layer arranged in the same layer and extending along a first direction; Among them, in the first direction, the width of the compressive stress dielectric layer gradually decreases, and the width of the tensile stress dielectric layer gradually increases; in the second direction, the compressive stress dielectric layer is connected to the tensile stress dielectric layer, the first direction is the direction in which the gate structure points to the drain, and the second direction intersects with the first direction.

2. The gallium nitride power device according to claim 1, characterized in that: The stress value of the compressive stress dielectric layer ranges from -0.1 to -2 GPa; The stress value of the tensile stress dielectric layer ranges from 0.1 to 2 GPa.

3. The gallium nitride power device according to claim 1 or 2, characterized in that: The number of the compressive stress dielectric layers and the number of the tensile stress dielectric layers are both multiple, and the multiple compressive stress dielectric layers and the multiple tensile stress dielectric layers are alternately arranged and connected along the second direction.

4. The gallium nitride power device according to claim 3, characterized in that: In the first direction, the width of the compressive stress dielectric layer decreases linearly, and the width of the tensile stress dielectric layer increases linearly; At one end close to the gate structure, the width of each of the compressive stress dielectric layers is the same and is a first width, the width of each of the tensile stress dielectric layers is the same and is a second width, and the first width is greater than the second width; the distance between two adjacent compressive stress dielectric layers is equal to the second width, and the distance between two adjacent tensile stress dielectric layers is equal to the first width; At one end close to the drain, the width of each compressive stress dielectric layer is the same and is the third width, the width of each tensile stress dielectric layer is the same and is the fourth width, and the fourth width is greater than the third width; the distance between two adjacent compressive stress dielectric layers is equal to the fourth width; and the distance between two adjacent tensile stress dielectric layers is equal to the third width.

5. The gallium nitride power device according to claim 4, characterized in that: The first width and the fourth width are both in the range of 0.1 um to 1 mm; the second width and the third width are both in the range of 0 to 1 mm.

6. The gallium nitride power device according to claim 4, characterized in that: The compressive stress dielectric layer and the tensile stress dielectric layer have the same thickness and a first thickness, and the first thickness ranges from 10 to 1000 nm.

7. The gallium nitride power device according to claim 1, characterized in that: The gallium nitride power device further comprises: The second dielectric layer is arranged on a side of the epitaxial layer away from the substrate and located in the second region. The second dielectric layer is a tensile stress dielectric layer.

8. A method for preparing a gallium nitride power device, characterized in that: include: providing a substrate; An epitaxial layer is formed on one side of the substrate; wherein the epitaxial layer is defined with a gate structure region, a source region and a drain region, and the source region and the drain region are located on both sides of the gate structure region; and the epitaxial layer located between the gate structure region and the drain region is defined as a first region of the epitaxial layer, and the epitaxial layer located between the gate structure region and the source region is defined as a second region of the epitaxial layer; A first dielectric layer is formed on a side of the epitaxial layer corresponding to the first region away from the substrate, wherein the first dielectric layer includes a compressive stress dielectric layer and a tensile stress dielectric layer which are arranged in the same layer and extend along a first direction, and in the first direction, the width of the compressive stress dielectric layer gradually decreases, and the width of the tensile stress dielectric layer gradually increases; in the second direction, the compressive stress dielectric layer is connected to the tensile stress dielectric layer; the first direction is the direction from the gate structure region to the drain region, and the second direction intersects with the first direction.

9. The preparation method according to claim 8, characterized in that: The first region includes a compressive stress dielectric layer region and a tensile stress dielectric layer region; The forming of a first dielectric layer on a surface of the epitaxial layer corresponding to the first region away from the substrate comprises: Growing a tensile stress dielectric material layer on the entire surface of the epitaxial layer on a side away from the substrate; Performing patterned etching on the tensile stress dielectric material layer to remove the tensile stress dielectric material layer corresponding to the compressive stress dielectric layer region and retaining the tensile stress dielectric material layer corresponding to the tensile stress dielectric layer region to form the tensile stress dielectric layer in the first region; Continue to grow a compressive stress dielectric material layer on the entire surface of the epitaxial layer on a side away from the substrate; The compressive stress dielectric material layer is patterned etched or chemically mechanically polished to remove the compressive stress dielectric material layer corresponding to the tensile stress dielectric layer region and retain the compressive stress dielectric material layer corresponding to the compressive stress dielectric layer region to form the compressive stress dielectric layer in the first region.

10. The preparation method according to claim 8, characterized in that: Before forming the first dielectric layer on the side of the epitaxial layer corresponding to the first region away from the substrate, the method further includes: forming a gate structure on a surface of the epitaxial layer corresponding to the gate structure region and facing away from the substrate; Alternatively, after forming the first dielectric layer on the side of the epitaxial layer corresponding to the first region away from the substrate, the method further includes: A gate structure is formed on a surface of the epitaxial layer corresponding to the gate structure region and facing away from the substrate.