Negative electrode active material, negative electrode comprising same, secondary battery comprising same, and method for manufacturing negative electrode active material
A coated silicon-based negative electrode active material with Li, Al, P, and O, and a carbon layer addresses the issues of volume expansion and irreversible capacity in silicon-based electrodes, enhancing battery efficiency and stability by reducing moisture reactivity and improving conductivity.
Patent Information
- Application Number
- CN202380039004.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-09
- Filing Date
- 2023-11-10
- Publication Date
- 2024-12-06
AI Technical Summary
Silicon-based negative electrode active materials in lithium secondary batteries suffer from high volume expansion/contraction and irreversible capacity, leading to reduced initial efficiency and stability due to metal oxide reactions with moisture, affecting the charge-discharge efficiency and pH of the negative electrode paste.
A negative electrode active material comprising silicon-based particles coated with a first layer containing Li, Al, P, and O, and a second layer of carbon, which reduces reactivity with moisture and enhances conductivity, thereby improving the processability and efficiency of the electrode.
The proposed coating structure enhances the discharge capacity, initial efficiency, resistance performance, and life characteristics of the battery by reducing lithium by-product reactions and improving the aqueous processability of the slurry.
Smart Images

Figure CN119096374A_ABST
Abstract
Description
Technical Field
[0001] This application claims the priority and benefit of Korean Patent Application No. 10-2022-0150557, filed with the Korean Intellectual Property Office on November 11, 2022, and Korean Patent Application No. 10-2023-0154177, filed with the Korean Intellectual Property Office on November 9, 2023. The entire contents of the Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a negative electrode active material, a negative electrode including the same, a secondary battery including the negative electrode, and a method for manufacturing the negative electrode active material. Background Art
[0003] Recently, with the rapid popularization of electronic devices using batteries, such as mobile phones, laptop computers, and electric vehicles, the demand for small, lightweight, and relatively high-capacity secondary batteries has increased rapidly. In particular, lithium secondary batteries have become a driving power source for portable devices that have attracted much attention due to their light weight and high energy density. Therefore, research and development efforts to improve the performance of lithium secondary batteries are being actively carried out.
[0004] Generally, a lithium secondary battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrolyte, an organic solvent, and the like. In addition, the positive electrode and the negative electrode can be formed on current collectors each having an active material layer including a positive electrode active material and a negative electrode active material. Generally, for the positive electrode, lithium-containing metal oxides such as LiCoO2 and LiMn2O4 are used as the positive electrode active material, and for the negative electrode, a carbon-based active material or a silicon-based active material without lithium is used as the negative electrode active material.
[0005] Among negative electrode active materials, silicon-based active materials have attracted much attention because they have a higher capacity and excellent high-rate charging characteristics than carbon-based active materials. However, the disadvantages of silicon-based active materials are that the degree of volume expansion / contraction during charge and discharge is high, and the irreversible capacity is high, resulting in low initial efficiency.
[0006] On the other hand, among silicon-based active materials, silicon-based oxides, specifically silicon-based oxides represented by SiO x (0 < x < 2) have the advantage that the degree of volume expansion / contraction during charge and discharge is lower than that of other silicon-based active materials such as silicon (Si). However, the silicon-based oxides also have the disadvantage that the initial efficiency is reduced due to the presence of an irreversible capacity.
[0007] In this regard, research has been conducted to reduce the irreversible capacity and improve the initial efficiency by doping or inserting metals such as Li, Al, and Mg into silicon-based oxides. However, the problem with the negative electrode paste containing silicon-based oxides doped with metals as the negative electrode active material is that the metal oxide formed by doping the metal reacts with moisture, thereby increasing the pH of the negative electrode paste and changing the viscosity. As a result, the state of the manufactured negative electrode is poor, and the charge-discharge efficiency of the negative electrode is reduced.
[0008] Therefore, there is a need to develop a negative electrode active material that can improve the phase stability of the negative electrode paste containing silicon-based oxides and improve the charge-discharge efficiency of the negative electrode manufactured from the paste.
[0009] Prior art documents
[0010] Patent documents
[0011] (Patent Document 1) Korean Patent Application Publication No. 10-2011-0112215 Summary of the Invention
[0012] Technical Problem
[0013] The present invention relates to a negative electrode active material, a negative electrode containing the same, a secondary battery containing the negative electrode, and a method for manufacturing the negative electrode active material.
[0014] Technical Solution
[0015] An exemplary embodiment of the present invention provides a negative electrode active material comprising: silicon-based particles containing SiO x (0 < x < 2) and a Li compound; a first coating provided on at least a part of the silicon-based particles; and a second coating provided on at least a part of the first coating, wherein the first coating contains Li, Al, P, and O, and wherein the second coating contains carbon.
[0016] Another exemplary embodiment of the present invention provides a negative electrode comprising the negative electrode active material.
[0017] Still another exemplary embodiment of the present invention provides a secondary battery comprising the negative electrode.
[0018] Advantageous Effects
[0019] The negative electrode active material according to an exemplary embodiment of the present invention comprises: silicon-based particles containing SiO xSilicon-based particles of (0 < x < 2) and Li compound; a first coating provided on at least a part of the silicon-based particles; and a second coating provided on at least a part of the first coating, wherein the first coating contains Li, Al, P, and O, and wherein the second coating contains carbon. The first coating containing Li, Al, P, and O is provided between the silicon-based particles and the second coating containing carbon, so that the reactivity of silicate with high alkali reactivity can be reduced, and the contact between the silicon-based particles and the outside can be easily blocked, thereby improving the aqueous processability of the slurry.
[0020] In addition, compared with the conventional negative electrode active material in which the coating containing Li, Al, P, and O is provided on the carbon layer, a hydrophobic carbon layer exists at the outermost layer, thereby further blocking the contact between the negative electrode active material and water to improve the aqueous processability of the slurry. In addition, highly conductive carbon exists at the outermost layer, which has an advantageous effect in achieving capacity / efficiency.
[0021] In addition, during the process of forming the first coating, lithium by-products contained in the silicon-based particles can be effectively removed, and the formed first coating effectively coats the unreacted lithium by-products. Thereby, the phenomenon that the lithium by-products or lithium silicate in the silicon-based particles react with the moisture of the slurry to deteriorate the physical properties of the slurry can be prevented. In addition, since the first coating contains Li, the lithium diffusion resistance on the surface of the negative electrode active material is reduced, which has the effect of improving the discharge rate performance.
[0022] Therefore, the negative electrode containing the negative electrode active material according to an exemplary embodiment of the present invention and the secondary battery containing the negative electrode have the effect of improving the discharge capacity, initial efficiency, resistance performance, and / or life characteristics of the battery. Description of the Drawings
[0023] Figure 1 Exemplarily shows the structure of the negative electrode active material according to an exemplary embodiment of the present invention.
[0024] <Symbol Description>
[0025] 1: Silicon-based particles
[0026] 2: First coating
[0027] 3: Li y Al z P w O v Phase
[0028] 4: Carbon
[0029] 5: Second coating Detailed Description
[0030] The present specification will be described in more detail below.
[0031] In the present specification, unless explicitly described to the contrary, when a part is referred to as “comprising” a certain component, this means that the part may further include another component, without excluding the other component.
[0032] Throughout this specification, when a component is referred to as being 'on' another component, the component may be in direct contact with the other component, or an intervening component may also be present.
[0033] It should be understood that the terms or words used throughout this specification should not be interpreted as limited to their ordinary meanings or dictionary meanings, but should be interpreted as having meanings and concepts consistent with the technical ideas of the present invention based on the concepts that the inventor can appropriately define the words or terms in order to explain the principles of the present invention in the best manner.
[0034] As used herein, the singular forms “a”, “an” and “the” are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0035] In the present specification, the crystallinity of the structure contained in the negative electrode active material can be confirmed by X-ray diffraction analysis, and the X-ray diffraction analysis can be performed by using an X-ray diffraction (XRD) analyzer (product name: D4-endavor, manufacturer: Bruker), or by appropriately adopting an apparatus used in the art in addition to the above-mentioned apparatus.
[0036] In the present specification, the presence or absence of elements and the content of the elements in the negative electrode active material may be confirmed by ICP analysis, and the ICP analysis may be performed using an inductively coupled plasma atomic emission spectrometer (ICPAES, Perkin-Elmer 7300).
[0037] In this specification, the average particle size (D 50 ) can be defined as the particle size corresponding to 50% cumulative volume in the particle size distribution curve (curve of particle size distribution graph). Average particle size (D 50 ) can be measured using, for example, the laser diffraction method. In the laser diffraction method, particle sizes from the submicron region to several millimeters can generally be measured, and results with high reproducibility and high resolution can be obtained.
[0038] Hereinafter, preferred embodiments of the present invention will be described in detail. However, it should be understood that the embodiments of the present invention can be modified in various forms, and the scope of the present invention is not limited to the embodiments described below.
[0039] <Negative Electrode Active Material>
[0040] An exemplary embodiment of the present invention provides a negative electrode active material, which comprises: silicon-based particles comprising SiO x (0 < x < 2) and a Li compound; a first coating provided on at least a part of the silicon-based particles; and a second coating provided on at least a part of the first coating, wherein the first coating comprises Li, Al, P, and O, and wherein the second coating comprises carbon.
[0041] The negative electrode active material according to an exemplary embodiment of the present invention comprises silicon-based particles. The silicon-based particles comprise SiO x (0 < x < 2) and a Li compound.
[0042] The SiO x (0 < x < 2) may correspond to the matrix in the silicon-based particles. The SiO x (0 < x < 2) may be in the form of containing Si and / or SiO2, and Si may form a phase. For example, the SiO x (0 < x < 2) may be a composite containing amorphous SiO2 and Si crystals. That is, x corresponds to the number ratio of O to Si contained in the SiO x (0 < x < 2). When the silicon-based particles contain the SiO x (0 < x < 2), the discharge capacity of the secondary battery can be improved.
[0043] The Li compound may correspond to a dopant in the silicon-based particles. The Li compound may exist in the silicon-based particles in at least one form of lithium atoms, lithium silicate, lithium silicide, or lithium oxide. When the silicon-based particles contain a Li compound, the initial efficiency is improved.
[0044] The Li compound may be distributed on the surface and / or inside of the silicon-based particles in a form doped into the silicon-based particles. The Li compound may be distributed on the surface and / or inside of the silicon-based particles so as to control the volume expansion / contraction of the silicon-based particles to an appropriate level and prevent damage to the active material. In addition, in terms of reducing the ratio of the irreversible phase (e.g., SiO2) of the silicon-based oxide particles to improve the efficiency of the active material, the Li compound may be contained.
[0045] In an exemplary embodiment of the present invention, the Li compound may exist in the form of lithium silicate. The lithium silicate is composed of Li a Si b O c(2 ≤ a ≤ 4, 0 < b ≤ 2, 2 ≤ c ≤ 5) represents and can be classified into crystalline lithium silicate and amorphous lithium silicate. The crystalline lithium silicate can exist in the silicon-based particles in the form of at least one lithium silicate selected from the group consisting of Li2SiO3, Li4SiO4, and Li2Si2O5, and the amorphous lithium silicate can have a composite form of Li a Si b O c (2 ≤ a ≤ 4, 0 < b ≤ 2, 2 ≤ c ≤ 5). However, the present invention is not limited thereto.
[0046] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, the content of Li can be 0.1 part by weight to 40 parts by weight or 0.1 part by weight to 25 parts by weight. Specifically, the content of Li can be 1 part by weight to 25 parts by weight, more specifically 2 parts by weight to 20 parts by weight. As the Li content increases, the initial efficiency increases, but the discharge capacity decreases. Therefore, when the above range is satisfied, an appropriate discharge capacity and initial efficiency can be achieved.
[0047] The content of the Li element can be confirmed by ICP analysis. Specifically, a predetermined amount (about 0.01 g) of the negative electrode active material is accurately weighed and transferred to a platinum crucible, and completely decomposed on a hot plate by adding nitric acid, hydrochloric acid, and sulfuric acid thereto. Then, by using an inductively coupled plasma atomic emission spectrometer (ICP-AES, Perkin-Elmer 7300), at the inherent wavelength of the element to be analyzed, a reference calibration curve is obtained by measuring the intensity of a standard liquid prepared using a standard solution (5 mg / kg). Subsequently, the pretreated sample solution and the blank sample are introduced into the spectrometer, and the actual intensity is calculated by measuring their respective intensities. Based on the obtained calibration curve, the concentration of each component is calculated, and conversion is performed so that the sum of the calculated concentrations of the components is equal to the theoretical value, and the element content of the prepared negative electrode active material can be analyzed.
[0048] In an exemplary embodiment of the present invention, the silicon-based particles may contain additional metal atoms. The metal atoms can exist in the silicon-based particles in at least one form of metal atoms, metal silicates, metal silicides, and metal oxides. The metal atoms may include at least one selected from the group consisting of Mg, Li, Al, and Ca. Therefore, the initial efficiency of the negative electrode active material can be improved.
[0049] In an exemplary embodiment of the present invention, a first coating is provided on at least a part of the silicon-based particles, and the first coating contains Li, Al, P, and O.
[0050] The first coating layer containing Li, Al, P and O is provided on the silicon-based particles as described above, so that the reactivity of silicate with high alkali reactivity can be reduced and the contact between the silicon-based particles and the outside can be easily blocked, thereby improving the water-based processability of the slurry.
[0051] Specifically, the first coating layer may be in the form of coating at least a portion of the silicon-based particles. That is, the first coating layer may be partially coated on the surface of the particles, or may be coated on the entire surface of the particles. The shape of the first coating layer may include: island type, thin film type, etc., but the shape of the first coating layer is not limited thereto.
[0052] The first coating layer may be disposed adjacent to the silicon-based particles. That is, the first coating layer may be adjacently coated on the silicon-based particles. The first coating layer may be in a form of completely or partially coating the silicon-based particles.
[0053] In an exemplary embodiment of the present invention, the first coating layer may include Li, Al, P, and O.
[0054] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, the content of Al may be 0.01 parts by weight or more and 1 part by weight or less. Specifically, the content of Al may be 0.02 parts by weight or more and 0.9 parts by weight or less, 0.03 parts by weight or more and 0.85 parts by weight or less, or 0.05 parts by weight or more and 0.8 parts by weight or less. The lower limit of the content of Al may be 0.01 parts by weight, 0.03 parts by weight, 0.05 parts by weight, 0.08 parts by weight, 0.1 parts by weight, 0.12 parts by weight, or 0.15 parts by weight, and the upper limit thereof may be 1 part by weight, 0.9 parts by weight, 0.85 parts by weight, 0.8 parts by weight, 0.7 parts by weight, 0.6 parts by weight, or 0.5 parts by weight.
[0055] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, the content of P may be 0.05 parts by weight or more and 2.5 parts by weight or less. Specifically, the content of P may be 0.1 parts by weight or more and 2 parts by weight or less, 0.15 parts by weight or more and 1.9 parts by weight or less, or 0.18 parts by weight or more and 1.8 parts by weight or less. The lower limit of the content of P may be 0.05 parts by weight, 0.1 parts by weight, 0.15 parts by weight, 0.18 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight, or 0.5 parts by weight, and the upper limit thereof may be 2.5 parts by weight, 2 parts by weight, 1.8 parts by weight, 1.5 parts by weight, 1.2 parts by weight, or 1 part by weight.
[0056] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, the content of Li contained in the first coating may be 0.05 parts by weight or more and 2 parts by weight or less. Specifically, the content of Li may be 0.1 parts by weight or more and 1.5 parts by weight or less, or 0.15 parts by weight or more and 1 part by weight or less. The lower limit of the content of Li contained in the first coating may be 0.05 parts by weight, 0.1 parts by weight, 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight, or 0.5 parts by weight, and the upper limit thereof may be 2 parts by weight, 1.5 parts by weight, 1.2 parts by weight, or 1 part by weight.
[0057] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, the content of O contained in the first coating may be 0.5 parts by weight or more and 2 parts by weight or less. Specifically, the content of O may be 0.6 parts by weight or more and 1.9 parts by weight or less, or 0.7 parts by weight or more and 1.8 parts by weight or less. The lower limit of the content of O contained in the first coating may be 0.5 parts by weight, 0.6 parts by weight, or 0.7 parts by weight, and the upper limit thereof may be 2 parts by weight, 1.9 parts by weight, or 1.8 parts by weight.
[0058] In an exemplary embodiment of the present invention, the first coating may contain a phase containing Li, Al, P, and O.
[0059] In an exemplary embodiment of the present invention, the first coating may contain Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) phase. y, z, w, and v each represent the atomic ratio of each atom.
[0060] In an exemplary embodiment of the present invention, the first coating may contain one or more selected from the group consisting of aluminum oxide, phosphorus oxide, lithium oxide, aluminum phosphate, lithium salt, lithium phosphate, and lithium aluminate. In one example, the Li y Al z P w O v phase may contain a mixture or compound formed by Li3PO4, AlPO4, Al(PO3)3, LiAlO2, etc., but is not limited thereto.
[0061] When the first coating layer including the above-mentioned components is provided, the Li compound included in the silicon-based particles can be prevented from reacting with the moisture of the slurry to reduce the slurry viscosity, which has the effect of improving the stability of the electrode state and / or the charge and discharge capacity.
[0062] In an exemplary embodiment of the present invention, the first coating layer may include an amorphous phase. In an example, the first coating layer may be an amorphous phase. In an example, when an X-ray diffraction analysis is performed on the negative electrode active material according to an exemplary embodiment of the present invention, a crystalline peak derived from the first coating layer may not appear.
[0063] In an exemplary embodiment of the present invention, the first coating layer may further include one or more selected from the group consisting of Li2O, LiOH and Li2CO3. Generally, during the process of doping lithium into the silicon-based particles, the remaining material may be exposed to moisture or air to form lithium byproducts such as Li2O, LiOH and Li2CO3. Therefore, the first coating layer may be in a form further including one or more selected from the group consisting of Li2O, LiOH and Li2CO3.
[0064] In an exemplary embodiment of the present invention, y may satisfy 0 <y≤3。
[0065] In an exemplary embodiment of the present invention, z may satisfy 0 <z≤1。
[0066] In an exemplary embodiment of the present invention, w may satisfy 0.5≤w≤3.
[0067] In an exemplary embodiment of the present invention, v may satisfy 4 <v≤12。
[0068] The first coating layer may be formed by dry-mixing i) silicon-based particles and aluminum phosphate, ii) silicon-based particles, an aluminum precursor and a phosphorus precursor, or iii) silicon-based particles and a Li—Al—PO-based precursor and heat-treating the mixture, or by mixing i), ii) or iii) with a solvent and reacting the mixture while evaporating the solvent.
[0069] In an exemplary embodiment of the present invention, the content of the first coating layer may be greater than 0 parts by weight and less than 10 parts by weight based on a total of 100 parts by weight of the negative electrode active material. Specifically, the content of the first coating layer may be greater than 0.1 parts by weight and less than 10 parts by weight, greater than 0.3 parts by weight and less than 8 parts by weight, or greater than 0.4 parts by weight and less than 5 parts by weight. If the content of the first coating layer is lower than the above range, it is difficult to prevent gas generation in the slurry, and if the content is higher than the above range, it is difficult to achieve capacity or efficiency.
[0070] The upper limit of the content of the first coating may be 10 parts by weight, 8 parts by weight, 6 parts by weight, 5 parts by weight, 4 parts by weight, 3.5 parts by weight, 3 parts by weight or 2 parts by weight, and the lower limit thereof may be 0.1 part by weight, 0.3 part by weight, 0.4 part by weight, 0.5 part by weight, 0.8 part by weight, 1 part by weight, 1.2 parts by weight, 1.4 parts by weight or 1.5 parts by weight.
[0071] In an exemplary embodiment of the present invention, the second coating may be provided on at least a part of the first coating, and the second coating contains carbon.
[0072] Specifically, the second coating may cover at least a part of the surface of the first coating, that is, it may partially cover the surface of the first coating, or may cover the entire surface of the first coating. The shape of the second coating may include: island type, thin film type, etc., but the shape of the second coating is not limited thereto.
[0073] The conductivity is imparted to the negative electrode active material by the second coating containing carbon, thereby improving the initial efficiency, life characteristics and battery capacity characteristics of the secondary battery.
[0074] The second coating may be provided adjacent to the first coating. That is, the second coating is coated adjacent to the first coating, and thus may be provided in the form of particles containing SiO x (0 < x < 2) and Li compound - the first coating - the second coating. The second coating may be in the form of completely or partially covering the first coating.
[0075] In addition, the second coating may be further provided on a region of the surface of the silicon-based particles where the first coating is not provided. That is, the second coating is coated adjacent to a portion of the surface of the silicon-based particles where the first coating is not covered, and thus may be provided in the form of the silicon-based particles - the second coating.
[0076] The second coating may be in the form of covering at least a part of the silicon-based particles. That is, the second coating may partially cover the surface of the silicon-based particles.
[0077] In an exemplary embodiment of the present invention, the second coating may contain amorphous carbon. In addition, the second coating may further contain crystalline carbon.
[0078] The crystalline carbon may further improve the conductivity of the negative electrode active material. The crystalline carbon may contain at least one selected from the group consisting of fullerene, carbon nanotube and graphene.
[0079] The amorphous carbon can appropriately maintain the strength of the carbon layer to inhibit the expansion of the silicon-based particles. The amorphous carbon can be a carbide of at least one selected from the group consisting of tar, pitch, and other organic materials, or can be a carbon-based material formed by using a hydrocarbon as a source for chemical vapor deposition.
[0080] The carbide of the other organic materials can be a carbide of an organic compound selected from sucrose, glucose, galactose, fructose, lactose, mannose, ribose, aldohexose, ketohexose, and combinations thereof.
[0081] The hydrocarbon can be a substituted or unsubstituted aliphatic or alicyclic hydrocarbon or a substituted or unsubstituted aromatic hydrocarbon. The aliphatic or alicyclic hydrocarbon of the substituted or unsubstituted aliphatic or alicyclic hydrocarbon can be methane, ethane, ethylene, acetylene, propane, butane, butene, pentane, isobutane, hexane, etc. The aromatic hydrocarbon of the substituted or unsubstituted aromatic hydrocarbon can be benzene, toluene, xylene, styrene, ethylbenzene, diphenylmethane, naphthalene, phenol, cresol, nitrobenzene, chlorobenzene, indene, coumarone, pyridine, anthracene, phenanthrene, etc.
[0082] In an exemplary embodiment of the present invention, the second coating can be an amorphous carbon layer.
[0083] In an exemplary embodiment of the present invention, the second coating can further contain Li, Al, P, and O. Specifically, the second coating can be a carbon layer further containing Li, Al, P, and O.
[0084] In an exemplary embodiment of the present invention, the second coating can further contain a phase containing Li, Al, P, and O. That is, the second coating is a carbon layer and can have a structure in which a phase containing Li, Al, P, and O is further contained inside the carbon layer.
[0085] Specifically, the second coating can be further contained Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) in the form of a phase.
[0086] The Li y Al z P w O v phase contained in the second coating can be the same as the Li y Al z P w O vThat is, during the process of coating the carbon layer on the silicon-based particles, the components of the first coating layer may be mixed together and coated, or during the process of forming the first coating layer and then carbon coating, the components of the first coating layer (e.g., Li y Al z P w O v phase) can be included in the carbon layer, thereby forming a Li y Al z P w O v Phase second coating.
[0087] In an exemplary embodiment of the present invention, the content of carbon may be 70 parts by weight or more based on 100 parts by weight of the second coating layer. Specifically, the content of carbon may be 80 parts by weight or more, 90 parts by weight or more, 95 parts by weight or more, or 98 parts by weight or more. As described above, the components of the first coating layer may be included during the process of forming the second coating layer, so a small amount of the components of the first coating layer may be included in the second coating layer.
[0088] In an exemplary embodiment of the present specification, the second coating layer may be disposed on the outermost layer of the negative electrode active material. Specifically, the carbon component in the second coating layer may be disposed on the outermost layer of the negative electrode active material. When carbon is present in the outermost layer of the negative electrode active material as described above, the hydrophobicity of the carbon acts more effectively than when carbon is not present in the outermost layer of the negative electrode active material, thereby further blocking the contact between the negative electrode active material and water to further improve the aqueous processability of the slurry. In addition, there is an effect that is conducive to achieving capacity / efficiency due to the conductivity of the carbon.
[0089] In an exemplary embodiment of the present invention, the content of the second coating layer may be 0.1 to 50 parts by weight based on a total of 100 parts by weight of the negative electrode active material. Specifically, the content of the second coating layer may be 1 to 30 parts by weight, 2 to 20 parts by weight, 3 to 10 parts by weight, or 3 to 8 parts by weight. When the above range is met, the capacity and efficiency of the negative electrode active material can be prevented from being reduced.
[0090] The upper limit of the content of the second coating layer can be 50 parts by weight, 40 parts by weight, 30 parts by weight, 20 parts by weight, 15 parts by weight, 10 parts by weight, 8 parts by weight, 7 parts by weight, 6 parts by weight or 5 parts by weight, and the lower limit can be 0.1 parts by weight, 1 part by weight, 2 parts by weight, 3 parts by weight or 4 parts by weight.
[0091] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, the content of carbon contained in the negative electrode active material may be 0.1 part by weight to 50 parts by weight, 0.1 part by weight to 30 parts by weight, or 0.1 part by weight to 20 parts by weight. More specifically, the content of carbon may be 0.5 part by weight to 15 parts by weight, 1 part by weight to 10 parts by weight, 1 part by weight to 8 parts by weight, or 1 part by weight to 5 parts by weight. When the above range is satisfied, a decrease in the capacity and efficiency of the negative electrode active material can be prevented. The upper limit of the content of carbon contained in the negative electrode active material may be 50 parts by weight, 40 parts by weight, 30 parts by weight, 20 parts by weight, 10 parts by weight, 8 parts by weight, 6 parts by weight, or 5 parts by weight, and the lower limit thereof may be 0.1 part by weight, 1 part by weight, 2 parts by weight, 3 parts by weight, or 4 parts by weight.
[0092] In an exemplary embodiment of the present invention, the thickness of the second coating may be 1 nm to 500 nm, specifically 5 nm to 300 nm. When the above range is satisfied, the conductivity of the negative electrode active material is improved, volume change of the negative electrode active material is easily suppressed, side reactions between the electrolyte and the negative electrode active material are suppressed, thereby improving the initial efficiency and / or lifespan of the battery.
[0093] Specifically, the second coating may be formed by chemical vapor deposition (CVD) using at least one hydrocarbon gas selected from the group consisting of methane, ethane, and acetylene.
[0094] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the negative electrode active material, Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) phase content may be 0.1 part by weight or more and 30 parts by weight or less. Specifically, the content of the phase may be 0.1 part by weight or more and 20 parts by weight or less, 0.2 part by weight or more and 15 parts by weight or less, 0.3 part by weight or more and 10 parts by weight or less, or 0.4 part by weight or more and 8 parts by weight or less. Li y Al z P w O v The lower limit of the phase content may be 0.1 part by weight, 0.2 part by weight, 0.3 part by weight, 0.4 part by weight, or 0.5 part by weight, and the upper limit thereof may be 30 parts by weight, 20 parts by weight, 15 parts by weight, 10 parts by weight, 8 parts by weight, 7 parts by weight, 6 parts by weight, 5 parts by weight, 4 parts by weight, 3 parts by weight, or 2 parts by weight. As described above, when Li y Al z P w Ov When the content of the phase satisfies the above range, the reactivity of the silicate with high alkali reactivity can be reduced, and the contact between the silicon-based particles and the outside can be easily blocked, thereby improving the water-based processability of the slurry. On the other hand, if the content exceeds the above range, it has a negative impact on the conductivity, making it difficult to achieve capacity / efficiency during charge and discharge, and if the content is lower than the above range, the reactivity of the silicate cannot be reduced, making it difficult to improve the water-based processability of the slurry.
[0095] In the present invention, the crystallinity of the carbon in the second coating layer can be confirmed by calculating the D / G band ratio according to Raman spectroscopy. Specifically, the measurement can be performed as follows: using a Renishaw 2000 Raman microscope system and 532 nm laser excitation, using a 100x optical lens, using a low laser power density, and an exposure time of 30 seconds to avoid laser thermal effects. In order to reduce the deviation according to the position, a total of 25 points can be measured for an area of 5 μm×5 μm, and a Lorentz function fitting can be used. Thereafter, the average values of the D band and the G band can be calculated.
[0096] Figure 1 The structure of the negative electrode active material according to an exemplary embodiment of the present invention is schematically shown, showing the configuration of the silicon-based particle 1, the first coating layer 2 and the second coating layer 5. Specifically, the first coating layer 2 may be provided on the silicon-based particle 1, and the second coating layer 5 may be provided on the first coating layer 2. In this case, the second coating layer 5 contains carbon 4, and may further contain Li y Al z P w O v Phase 3.
[0097] In an exemplary embodiment of the present invention, based on a total of 100 parts by weight of the first coating and the second coating, the content of carbon may be 45 parts by weight or more and 95 parts by weight or less. Specifically, the content of carbon may be 48 parts by weight or more and 93 parts by weight or less, 49 parts by weight or more and 92 parts by weight or less, 50 parts by weight or more and 91 parts by weight or less, greater than 50 parts by weight or less and 90 parts by weight or less, 60 parts by weight or more and 85 parts by weight or less, or 70 parts by weight or more and 80 parts by weight or less. As described above, when the content of carbon in the entire coating is 45 parts by weight or more, a hydrophobic carbon layer is present at the outermost layer, which can further block contact with water to improve the water-based processability of the slurry. In addition, highly conductive carbon is present at the outermost layer, which has a favorable effect in achieving capacity / efficiency. On the other hand, if the carbon content is lower than the above range, it is difficult to improve the aqueous processability of the slurry because the contact between the negative electrode active material and water cannot be effectively blocked. If the carbon content exceeds the above range, the material becomes excessively hydrophobic, thereby causing a problem of low dispersibility when manufacturing aqueous slurry.
[0098] In an exemplary embodiment of the present invention, the weight ratio of the first coating layer to the second coating layer may be 1:0.5 to 1:30. Specifically, the weight ratio may be 1:0.5 to 1:20, 1:0.5 to 1:15, 1:1 to 1:15, 1:2 to 1:10 or 1:3 to 1:5. By satisfying the above range, the first coating layer and the second coating layer can effectively coat the silicon-based particles, thereby effectively suppressing the side reactions in the slurry and stably achieving capacity and / or efficiency. On the other hand, if the content of the first coating layer is excessively higher than the content of the second coating layer, it is difficult to achieve capacity or efficiency, and if the content of the second coating layer is excessively higher than the content of the first coating layer, it is difficult to prevent gas generation in the slurry.
[0099] In an exemplary embodiment of the present invention, based on 100 parts by weight of the second coating layer, the content of the first coating layer may be 5 parts by weight or more and 150 parts by weight or less. Specifically, based on 100 parts by weight of the second coating layer, the content of the first coating layer may be 120 parts by weight or less, 110 parts by weight or less, 100 parts by weight or less, 90 parts by weight or less, 80 parts by weight or less, 70 parts by weight or less, 60 parts by weight or less, or 50 parts by weight or less. In addition, based on 100 parts by weight of the second coating layer, the content of the first coating layer may be 5 parts by weight or more, 8 parts by weight or more, 10 parts by weight or more, or 20 parts by weight or more. By satisfying the above range, the first coating layer and the second coating layer can effectively coat the silicon-based particles, thereby effectively suppressing the side reactions in the slurry, and stably achieving capacity and / or efficiency.
[0100] In an exemplary embodiment of the present invention, the lithium byproduct may be present on the silicon-based particles. Specifically, the lithium byproduct may be present between the silicon-based particles and the first coating layer, in the first coating layer, or on the first coating layer. In addition, the lithium byproduct may be present between the silicon-based particles and the second coating layer.
[0101] Specifically, the lithium by-product may refer to a lithium compound remaining near the surface of the silicon-based particle or the carbon layer after the silicon-based particle is manufactured.
[0102] The lithium by-product may include one or more selected from the group consisting of Li2O, LiOH, and Li2CO3.
[0103] The presence or absence of the lithium by-product may be confirmed by X-ray diffraction analysis (XRD) or X-ray photoelectron analysis (XPS).
[0104] Based on a total of 100 parts by weight of the negative electrode active material, the content of the lithium by-product may be 5 parts by weight or less. Specifically, the content of the lithium by-product may be 0.01 to 5 parts by weight, 0.05 to 2 parts by weight, or 0.1 to 1 part by weight. More specifically, the content of the lithium by-product may be 0.1 to 0.8 parts by weight or 0.1 to 0.5 parts by weight. When the content of the lithium by-product meets the above range, the side reaction in the slurry can be reduced, and the viscosity change can be reduced, thereby improving the water-based processability characteristics. On the other hand, when the content of the lithium by-product is higher than the above range, the slurry becomes alkaline when formed, which may cause side reactions or viscosity changes, as well as problems in water-based processability.
[0105] The content of the lithium by-product may be calculated by measuring the amount of the HCl solution in a specific interval of pH change during titration of the aqueous solution containing the negative electrode active material with the HCl solution using a titrator, and then calculating the amount of the lithium by-product.
[0106] The average particle size of the negative electrode active material (D 50 ) can be 0.1 μm to 30 μm, specifically 1 μm to 20 μm, and more specifically 1 μm to 10 μm. When the above range is met, the structural stability of the active material during charge and discharge is ensured, and the problem that the level of volume expansion / contraction increases as the particle size becomes too large can be prevented, and the problem that the initial efficiency decreases when the particle size is too small can also be prevented.
[0107] The BET specific surface area of the negative electrode active material can be 1 m 2 / g to 100 m 2 / g, specifically 1 m2 / g to 70 m 2 / g, more specifically 1 m 2 / g to 50 m 2 / g, for example, 2 m 2 / g to 30 m 2 / g. When the above range is satisfied, side reactions between the electrolyte and the negative electrode active material can be reduced during charging and discharging of the battery, and thus the life characteristics of the battery can be improved.
[0108] <Method for manufacturing negative electrode active material>
[0109] An exemplary embodiment of the present invention provides a method for manufacturing a negative electrode active material, the method comprising: manufacturing preliminary silicon-based particles containing SiO x (0 < x < 2); manufacturing silicon-based particles by mixing the preliminary silicon-based particles with a Li precursor and heat-treating the mixture; providing a first coating by mixing and reacting the silicon-based particles with one or more selected from the group consisting of an Al precursor, a P precursor, and a precursor containing Al and P; and forming a second coating of a carbon precursor on the silicon-based particles provided with the first coating.
[0110] When manufacturing the negative electrode active material by the above method, after forming a first coating containing Li, Al, P, and O on the silicon-based particles, a second coating containing carbon can be formed on the silicon-based particles provided with the first coating by a chemical vapor deposition (CVD) method or the like.
[0111] The preliminary silicon-based particles can be manufactured by heating Si powder and SiO2 powder in a vacuum to vaporize them, and then depositing the vaporized mixed gas.
[0112] The Si powder and the SiO2 powder can be included in a weight ratio of 2:8 to 8:2. Specifically, the Si powder and the SiO2 powder can be included in a weight ratio of 4:6 to 6:4 or 5:5.
[0113] Specifically, the mixed powder of the Si powder and the SiO2 powder can be heat-treated in a vacuum at 1300 °C to 1800 °C, 1400 °C to 1800 °C, or 1400 °C to 1600 °C.
[0114] The vaporized mixed gas by heat treatment can be cooled in a vacuum and deposited as a solid phase. In addition, the preliminary silicon-based particles can be manufactured by heat-treating the deposited solid phase in an inert atmosphere. The heat treatment can be performed at 500 °C to 1000 °C or 700 °C to 900 °C.
[0115] The formed preliminary silicon-based particles can be in the form of SiOx in the form of (x = 1).
[0116] Next, the prepared silicon-based particles are mixed with a Li precursor and then heat-treated to produce silicon-based particles containing the Li compound (doped with Li). The Li precursor can be, for example, Li powder.
[0117] The step of mixing the prepared silicon-based particles with Li powder and performing heat treatment can be carried out at 700 °C to 900 °C for 4 hours to 6 hours, specifically at 800 °C for 5 hours.
[0118] The silicon-based particles formed by the heat treatment contain SiO x (0 < x < 2) and Li compounds.
[0119] The silicon-based particles can contain lithium silicate, lithium silicide, lithium oxide, etc. as the Li compounds described above.
[0120] The particle size of the silicon-based particles can be further adjusted by methods such as ball milling, jet milling, or air classification, but the present invention is not limited thereto.
[0121] The lithium compound (lithium by-product) is disposed on at least a part of the surface of the silicon-based particles as described above. Specifically, in the process of forming the prepared silicon-based particles containing SiOx (0 < x < 2) and doping with Li to produce the above silicon-based particles, the lithium compound, that is, the lithium by-product formed by unreacted lithium, remains near the surface of the silicon-based particles.
[0122] Next, a first coating can be disposed on at least a part of the silicon-based particles containing the Li compound.
[0123] The step of disposing the first coating on at least a part of the silicon-based particles can include mixing the silicon-based particles with one or more selected from the group consisting of an Al precursor, a P precursor, and a precursor containing Al and P and reacting them.
[0124] In an exemplary embodiment, the step of disposing the first coating on at least a part of the silicon-based particles can include mixing the silicon-based particles with a precursor containing Al and P and reacting them.
[0125] Based on a total of 100 parts by weight of the mixture, the content of the precursor containing Al and P can be 0.1 part by weight to 5 parts by weight. Specifically, the content of the precursor can be 0.5 part by weight to 4 parts by weight or 1 part by weight to 3 parts by weight.
[0126] The precursor containing Al and P can be aluminum phosphate.
[0127] Specifically, the first coating can be formed on at least a part of the silicon-based particles in the following ways: i) dry-mixing the silicon-based particles with aluminum phosphate and heat-treating the mixture, or ii) mixing the silicon-based particles and aluminum phosphate with a solvent, and then reacting the silicon-based particles with aluminum phosphate while evaporating the solvent by heat treatment. When the first coating is formed using the above methods, the first coating can be easily formed by the reaction of aluminum phosphate with lithium by-products formed or remaining during the process of manufacturing the silicon-based particles.
[0128] The aluminum phosphate can be Al b P c O d in the form of (0 < b ≤ 10, 0 < c ≤ 10, 0 < d ≤ 10). Specifically, the aluminum phosphate can be Al(PO3)3 or AlPO4, but is not limited thereto, and salts used in the art can be appropriately adopted to form the first coating.
[0129] In another exemplary embodiment, the step of disposing the first coating on at least a part of the silicon-based particles may include mixing and reacting the silicon-based particles with a precursor containing Al (aluminum precursor) and a precursor P containing P (phosphorus precursor).
[0130] Specifically, the first coating can be formed on at least a part of the silicon-based particles in the following ways: iii) dry-mixing the silicon-based particles, aluminum precursor, and phosphorus precursor and heat-treating the mixture, or iv) mixing the silicon-based particles, aluminum precursor, and phosphorus precursor with a solvent, and then reacting the silicon-based particles, aluminum precursor, and phosphorus precursor while evaporating the solvent by heat treatment. When the first coating is formed by the above methods, the first coating can be easily formed by the reaction of lithium by-products formed during the process of manufacturing the silicon-based particles, the aluminum precursor, and the phosphorus precursor.
[0131] The aluminum precursor can be Al a O b in the form of aluminum oxide (0 < a ≤ 10, 0 < b ≤ 10), and specifically can be Al2O3.
[0132] Alternatively, the aluminum precursor can be aluminum hydroxide, aluminum nitrate, aluminum sulfide, etc., and specifically can be Al(OH)3, Al(NO3)3·9H2O, or Al2(SO4)3, but is not limited thereto, and aluminum precursors used in the art can be appropriately adopted to form the first coating.
[0133] The phosphorus precursor can be P c O d in the form of phosphorus oxide (0 < c ≤ 10, 0 < d ≤ 10).
[0134] Alternatively, the phosphorus precursor may be ammonium phosphate, diammonium phosphate, phosphoric acid, etc., specifically (NH4)3PO4, (NH4)2HPO4, H3PO4 or NH4H2PO4, but not limited thereto, and phosphorus precursors used in the art may be appropriately employed to form the first coating.
[0135] In another exemplary embodiment, the step of disposing the first coating on at least a part of the silicon-based particles may include mixing and reacting the silicon-based particles with a precursor containing Li, Al, P and O (Li-Al-P-O-based precursor).
[0136] Specifically, the first coating may be formed on at least a part of the silicon-based particles in the following manner: v) dry-mixing the silicon-based particles with the Li-Al-P-O-based precursor and heat-treating the mixture, or vi) mixing the silicon-based particles and the Li-Al-P-O-based precursor with a solvent, and then reacting the silicon-based particles with the Li-Al-P-O-based precursor while evaporating the solvent by heat treatment. When the first coating is formed by the above method, the first coating may be formed by directly adding the Li-Al-P-O-based precursor.
[0137] The Li-Al-P-O-based precursor may be Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10). Specifically, the Li-Al-P-O-based precursor may be a mixture or compound formed by the combination of Li3PO4, AlPO4, Al(PO3)3, LiAlO2, etc., but not limited thereto, and structures used in the art may be appropriately employed to form the first coating.
[0138] In the step of disposing the first coating on at least a part of the silicon-based particles, the heat treatment may be carried out at 500 °C to 700 °C, specifically 550 °C to 650 °C. However, the heat treatment is not limited thereto and may vary depending on the salt or precursor used. If the heat treatment temperature is higher than the above range, the first coating is formed in a crystalline form, making it difficult for Li ions to enter and exit through the first coating, thereby deteriorating the resistance and life characteristics and reducing the capacity and / or efficiency. When the heat treatment temperature satisfies the above range, the reaction between the salt or precursor and the Li by-product occurs well, the first coating contains Li, so the durability of the formed negative electrode active material against moisture increases, and the lithium diffusion resistance on the surface of the negative electrode active material decreases, which has the effect of improving the discharge rate performance.
[0139] In the step of disposing the first coating on at least a part of the silicon-based particles, the heat treatment temperature is preferably lower than the temperature at which the preliminary silicon-based particles are mixed with the Li precursor and then heat treated.
[0140] The solvent may be water or ethanol, but is not limited thereto, and solvents used in the art may be appropriately employed.
[0141] The first coating formed on the silicon-based particles preferably contains Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) phase, Li y Al z P w O v The phase may be an amorphous phase.
[0142] Details of the first coating are the same as described above.
[0143] Next, a second coating may be disposed on the surface of the silicon-based particles.
[0144] The second coating may be a carbon layer, and the carbon layer may be formed by chemical vapor deposition (CVD) using a carbon-based material such as a hydrocarbon gas or by carbonizing a material used as a carbon source.
[0145] Specifically, the carbon layer may be formed by placing the formed preliminary particles in a reactor and then depositing a hydrocarbon gas at 500 °C to 1200 °C by chemical vapor deposition (CVD). The hydrocarbon gas may be at least one hydrocarbon gas selected from the group consisting of methane, ethane, propane, and acetylene, and may be heat treated at 500 °C to 900 °C.
[0146] The heat treatment temperature during chemical vapor deposition is preferably lower than the temperature at which the preliminary silicon-based particles are mixed with the Li precursor and then heat treated.
[0147] Another exemplary embodiment of the present invention provides a method for manufacturing a negative electrode active material, the method comprising: manufacturing preliminary silicon-based particles containing SiOx (0 < x < 2); manufacturing silicon-based particles by mixing the preliminary silicon-based particles with a Li precursor and heat treating the mixture; and mixing the silicon-based particles with one or more selected from the group consisting of an Al precursor, a P precursor, and a precursor containing Al and P, and a carbon source, and heat treating the mixture.
[0148] When the negative electrode active material is manufactured by the above method, the precursor of the first coating layer (Al precursor, P precursor, and precursor containing Al and P) is mixed with the precursor of the second coating layer (carbon source), and then carbonized by heat treatment, thereby forming the first coating layer and the second coating layer on the silicon-based particles at the same time.
[0149] The above details may be applied to the silicon-based particles, the Al precursor, the P precursor, the precursor containing Al and P, and the carbon source.
[0150] In the step of mixing one or more selected from the group consisting of an Al precursor, a P precursor, and a precursor containing Al and P with a carbon source and heat treating the mixture, the heat treatment temperature is preferably lower than the heat treatment temperature after mixing the preliminary silicon-based particles with a Li precursor.
[0151] Specifically, the heat treatment may be performed at 500°C to 700°C, more specifically 550°C to 650°C. However, the heat treatment is not limited thereto and may vary depending on the salt or precursor used. If the heat treatment temperature is higher than the above range, the first coating layer and the second coating layer are formed in a crystalline form, making it difficult for Li ions to enter and exit through the first and second coating layers, thereby deteriorating resistance and life characteristics and reducing capacity and / or efficiency.
[0152] <Negative electrode>
[0153] A negative electrode according to an exemplary embodiment of the present invention may include the above-mentioned negative electrode active material.
[0154] Specifically, the negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer may include the negative electrode active material. In addition, the negative electrode active material layer may further include a binder, a thickener and / or a conductive material.
[0155] The negative electrode active material layer may be formed by applying a negative electrode slurry including a negative electrode active material, a binder, a thickener and / or a conductive material to at least one surface of a current collector, and drying and rolling it.
[0156] The negative electrode slurry may further include additional negative electrode active materials.
[0157] As the additional negative electrode active material, a compound capable of reversibly intercalating and deintercalating lithium can be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metal substances capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metal oxides capable of doping and dedoping lithium, such as SiO β(0<β<2), SnO2, vanadium oxide, lithium titanium oxide and lithium vanadium oxide; or a composite containing a metal substance and a carbonaceous material, such as a Si-C composite or a Sn-C composite, and any one thereof or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon can be used as carbon materials. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include amorphous, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, floating graphite, pyrolytic carbon, mesophase pitch-based carbon fibers, mesophase carbon microbeads, mesophase pitch and high-temperature fired carbon such as coke derived from petroleum or coal tar pitch.
[0158] The additional negative electrode active material may be a carbon-based negative electrode active material.
[0159] In an exemplary embodiment of the present invention, a weight ratio of the negative electrode active material to the additional negative electrode active material included in the negative electrode slurry may be 10:90 to 90:10, specifically 10:90 to 50:50.
[0160] The negative electrode slurry may include a solvent for forming the negative electrode slurry. Specifically, in terms of promoting dispersion of components, the solvent for forming the negative electrode slurry may include at least one selected from the group consisting of distilled water, ethanol, methanol, and isopropanol, specifically distilled water.
[0161] The negative electrode slurry containing the negative electrode active material according to an exemplary embodiment of the present invention may have a pH of 7 to 11 at 25° C. When the pH of the negative electrode slurry satisfies the above range, the rheology of the slurry is stabilized. On the other hand, when the pH of the negative electrode slurry is less than 7 or the pH of the negative electrode slurry exceeds 11, carboxymethyl cellulose (CMC) used as a thickener decomposes, resulting in a decrease in the viscosity of the slurry and a decrease in the dispersion of the active material contained in the slurry.
[0162] There is no particular limitation on the negative electrode current collector as long as it has conductivity without causing chemical changes in the battery. For example, for the current collector, copper, stainless steel, aluminum, nickel, titanium, fired carbon, aluminum or stainless steel each surface-treated with carbon, nickel, titanium, silver, etc., etc. can be used. Specifically, for the current collector, transition metals such as copper and nickel that adsorb carbon well can be used. The thickness of the current collector can be 6 μm to 20 μm. However, the thickness of the current collector is not limited thereto.
[0163] The adhesive may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and the above materials in which hydrogen is replaced by Li, Na, Ca, etc., and may also include various copolymers thereof.
[0164] There is no particular limitation on the conductive material as long as it has conductivity and does not cause chemical changes in the battery. For example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc.
[0165] The thickener may be carboxymethyl cellulose (CMC), but is not limited thereto, and any thickener used in the art may be appropriately used.
[0166] In an exemplary embodiment of the present invention, a weight ratio of the negative electrode active material to the additional negative electrode active material included in the negative electrode slurry may be 1:99 to 30:70, specifically 5:95 to 30:70 or 10:90 to 20:80.
[0167] In an exemplary embodiment of the present invention, the content of all negative electrode active materials contained in the negative electrode slurry may be 60 to 99 parts by weight, specifically 70 to 98 parts by weight, based on 100 parts by weight of the solid content of the negative electrode slurry in total.
[0168] In an exemplary embodiment of the present invention, the binder may be included in an amount of 0.5 to 30 parts by weight, for example 1 to 20 parts by weight, based on 100 parts by weight of the solid content of the negative electrode slurry in total.
[0169] In an exemplary embodiment of the present invention, the conductive material may be contained in an amount of 0.5 to 25 parts by weight, specifically 1 to 20 parts by weight, based on 100 parts by weight of the solid content of the negative electrode slurry in total.
[0170] In an exemplary embodiment of the present invention, the thickener may be included in an amount of 0.5 to 25 parts by weight, specifically 0.5 to 20 parts by weight, and more specifically 1 to 20 parts by weight, based on 100 parts by weight of the solid content of the negative electrode slurry.
[0171] The negative electrode slurry according to an exemplary embodiment of the present invention may further include a solvent for forming the negative electrode slurry. Specifically, in terms of promoting dispersion of components, the negative electrode slurry forming solvent may include at least one selected from the group consisting of distilled water, ethanol, methanol and isopropanol, specifically distilled water.
[0172] In an exemplary embodiment of the present invention, the solid content of the negative electrode slurry may be 20 parts by weight to 75 parts by weight, specifically 30 parts by weight to 70 parts by weight, based on 100 parts by weight in total of the negative electrode slurry.
[0173] <Secondary Battery>
[0174] A secondary battery according to an exemplary embodiment of the present invention may include the negative electrode according to an exemplary embodiment of the present invention described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the negative electrode is the same as the negative electrode described above. Since the negative electrode has been described above, its detailed description is omitted.
[0175] The positive electrode may include a positive electrode current collector, and a positive electrode active material layer formed on the positive electrode current collector and including a positive electrode active material.
[0176] In the positive electrode, there is no particular restriction on the positive electrode collector, as long as it has conductivity and does not cause chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, fired carbon, aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., etc. can be used. In addition, the thickness of the positive electrode collector can generally be 3 μm to 500 μm, and the surface of the collector can be formed with microscopic concave-convex to enhance the adhesion of the positive electrode active material. For example, the positive electrode collector can be used in various shapes, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0177] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) or a compound substituted by one or more transition metals; lithium iron oxide such as LiFe3O4; lithium manganese oxide such as Li 1+c1 Mn 2-c1O4 (0≤c1≤0.33), LiMnO3, LiMn2O3 and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O8, V2O5 and Cu2V2O7; Ni-site lithium nickel oxide, composed of the chemical formula LiNi 1-c2 M c2 O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B and Ga, and satisfies 0.01≤c2≤0.5); lithium manganese composite oxide, represented by the chemical formula LiMn 2-c3 M c3 O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, and satisfies 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); LiMn2O4, wherein a portion of Li in the chemical formula is replaced by an alkaline earth metal ion, etc., but is not limited thereto. The positive electrode may be Li metal.
[0178] The positive electrode active material layer may further include a positive electrode conductive material and a positive electrode binder in addition to the positive electrode active material described above.
[0179] In this case, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without particular limitation, as long as the positive electrode conductive material has electronic conductivity without causing chemical changes in the constituted battery. Specific examples may include graphite, such as natural graphite and artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber, such as copper, nickel, aluminum, and silver; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, and the like, and any one thereof or a mixture of two or more thereof may be used.
[0180] In addition, the positive electrode binder is used to improve the bonding between the positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode collector. Specific examples may include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, etc., and any one thereof or a mixture of two or more thereof may be used.
[0181] The diaphragm is used to separate the negative electrode and the positive electrode and provide a path for lithium ion movement, wherein any diaphragm can be used as the diaphragm without particular limitation, as long as it is commonly used in secondary batteries, in particular, it may be preferred to use a diaphragm having high moisture retention capacity for the electrolyte and low resistance to the movement of electrolyte ions. Specifically, a porous polymer film can be used, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer and an ethylene / methacrylate copolymer, or a laminated structure of more than two layers thereof. In addition, ordinary porous nonwoven fabrics can be used, for example, nonwoven fabrics formed by high melting point glass fibers, polyethylene terephthalate fibers, etc. In addition, a coated diaphragm comprising a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and a diaphragm with a monolayer or multilayer structure can be selectively used.
[0182] Examples of the electrolyte may include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte, which may be used to manufacture a lithium secondary battery, but are not limited thereto.
[0183] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0184] As the nonaqueous organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate or ethyl propionate can be used.
[0185] Especially, in carbonate system organic solvent, ethylene carbonate and propylene carbonate as cyclic carbonate are high viscosity organic solvents and they have high dielectric constant, thereby can dissociate lithium salt well, therefore can preferably use.When cyclic carbonate and linear carbonate with low viscosity and low dielectric constant such as dimethyl carbonate or diethyl carbonate are mixed with use in suitable ratio, can prepare electrolyte with high conductivity, therefore may more preferably use.
[0186] A lithium salt may be used as the metal salt, and the lithium salt is a material that is easily dissolved in a non-aqueous electrolyte, wherein, for example, one or more selected from the group consisting of the following may be used as an anion of the lithium salt: F - , Cl - ,I- 、NO3 - 、N(CN) 2- 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - .
[0187] In order to improve the life characteristics of the battery, inhibit the decline of the battery capacity, improve the discharge capacity of the battery, etc., in addition to the above-mentioned electrolyte components, the electrolyte may also contain one or more additives, such as halogenated alkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme dimethyl ether, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum trichloride.
[0188] Another exemplary embodiment of the present invention provides a battery module including a secondary battery as a unit cell and a battery pack including the battery module. Since the battery module and the battery pack include secondary batteries having high capacity, high rate capability, and high cycle characteristics, the battery module and the battery pack can be used as a power source for medium and large devices selected from the group consisting of: electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.
[0189] Invention Mode
[0190] Preferred embodiments will be provided below to better understand the present invention. It will be apparent to those skilled in the art that the embodiments are provided only to illustrate the present invention, and various modifications and changes can be made within the scope and technical spirit of the present invention. Such modifications and changes naturally fall within the scope of the claims contained herein.
[0191] <Examples and Comparative Examples>
[0192] Example 1
[0193] 100 g of Si and SiO2 powder mixed in a molar ratio of 1:1 was vacuum heated in a reactor to a sublimation temperature of 1,400°C. Then, the mixed gas of vaporized Si and SiO2 was reacted in a cooling zone under a vacuum state at a cooling temperature of 800°C and condensed into a solid phase. Thereafter, heat treatment was performed in an inert atmosphere at a temperature of 800°C to prepare preparatory silicon-based particles. Then, the preparatory silicon-based particles were added and pulverized for 3 hours using a ball mill after adding 15 stainless steel ball media to prepare a 6 μm (D 50 ) of silicon-based particles.
[0194] 10 g of Li metal powder was added to 90 g of the silicon-based particles, which were heat-treated at 800° C. in an inert atmosphere to obtain Li-doped silicon-based particles.
[0195] 98.5 g of the Li-doped silicon-based particles were mixed with 1.5 g of Al(PO 3 ) 3 , and the mixture was heat-treated at 600° C. to prepare silicon-based particles, wherein a first coating layer containing Li, Al, and P was formed on the surface of the silicon-based particles.
[0196] Thereafter, while Ar gas was flowed to maintain an inert atmosphere, the silicon-based particles on which the first coating layer was formed were positioned in a hot zone of a CVD apparatus, and while methane was blown into the hot zone at 700° C. using Ar as a carrier gas, the hot zone was heated at 10° C. -1 The reaction was carried out under support for 20 minutes, thereby forming a second coating layer (carbon layer) on the surface of the silicon-based particles.
[0197] The negative electrode active material D 50 The BET specific surface area is 2.5 m 2 / g.
[0198] The negative electrode active material includes the first coating layer including Li, Al, P and O between the silicon-based particles and the second coating layer including carbon, and as a result of ICP analysis of the negative electrode active material, the contents of Li, Al and P are 9.5 wt %, 0.15 wt % and 0.5 wt %, respectively, based on 100 wt % in total of the negative electrode active material.
[0199] Example 2
[0200] A negative electrode active material was prepared in the same manner as in Example 1, except that 95 g of the Li-doped silicon-based particles and 35 g of Al(PO 3 ) were mixed and the mixture was heat-treated.
[0201] As a result of ICP analysis of the negative electrode active material, the contents of Li, Al, and P were 9.0 wt %, 0.5 wt %, and 1.8 wt %, respectively, based on 100 wt % in total of the negative electrode active material.
[0202] Example 3
[0203] A negative electrode active material was prepared in the same manner as in Example 1, except that 99.5 g of the Li-doped silicon-based particles and 30.5 g of Al(PO 3 ) were mixed and the mixture was heat-treated.
[0204] As a result of ICP analysis of the negative electrode active material, the contents of Li, Al, and P were 9.5 wt %, 0.05 wt %, and 0.18 wt %, respectively, based on 100 wt % in total of the negative electrode active material.
[0205] Comparative Example 1
[0206] A negative electrode active material was prepared in the same manner as in Example 1, except that a carbon layer was first formed on the surface of the silicon-based particles before doping the silicon-based particles with Li.
[0207] In the case of the negative electrode active material of Comparative Example 1, the coating layer including Li, Al, P, and O was formed after the carbon layer was formed, so that the coating layer was formed in the reverse order to that of Examples 1 to 3.
[0208] As a result of ICP analysis of the negative electrode active material, the contents of Li, Al, and P were 9.5 wt %, 0.15 wt %, and 0.5 wt %, respectively, based on 100 wt % in total of the negative electrode active material.
[0209] Comparative Example 2
[0210] A negative electrode active material was prepared in the same manner as in Comparative Example 1, except that 90 g of the Li-doped silicon-based particles and 10 g of Al(PO 3 ) 3 were mixed and the mixture was heat-treated.
[0211] As a result of ICP analysis of the negative electrode active material, the contents of Li, Al, and P were 9.0 wt %, 1.0 wt %, and 3.0 wt %, respectively, based on 100 wt % in total of the negative electrode active material.
[0212] Comparative Example 3
[0213] A negative electrode active material was prepared in the same manner as in Example 1, except that the second coating layer was not formed.
[0214] Comparative Example 4
[0215] 10 g of Li metal powder was added to 90 g of silicon-based particles, and the mixture was heat-treated in an inert atmosphere at a temperature of 800° C. to prepare Li-doped silicon-based particles, the procedure being carried out in the same manner as in Example 1. Then, 5 g of asphalt was added when 1.5 g of Al(PO3)3 was mixed with 98.5 g of silicon-based particles, and the mixture was heat-treated at 600° C., thereby preparing a negative electrode active material, wherein a first coating layer containing Li, Al, P and C was formed on the surface of the silicon-based particles.
[0216] Thereafter, heat treatment was performed in an argon atmosphere at 700° C. for 20 minutes to prepare a negative electrode active material.
[0217]
[0218] The content of the elements was confirmed by ICP analysis using an inductively coupled plasma atomic emission spectrometer (ICP-OES of Perkin-Elmer 7300, AVIO 500).
[0219] The negative electrode active material D 50 The analysis was performed by PSD measurement method using Microtrac equipment.
[0220] The specific surface area was measured by degassing at 200 °C for 8 h and performing N2 adsorption / desorption at 77 K using a BET measurement apparatus (BEL-SORP-MAX, Bell Co., Japan).
[0221] <Experimental Example: Evaluation of Discharge Capacity, Initial Efficiency and Life (Capacity Retention Rate) Characteristics>
[0222] A negative electrode and a battery were prepared using the negative electrode active materials of the example and the comparative example, respectively.
[0223] A mixture was prepared by mixing the negative electrode active material, carbon black as a conductive material, and polyacrylic acid (PAA) as a binder in a weight ratio of 80:10:10. Thereafter, 7.8 g of distilled water was added to 5 g of the mixture, which was then stirred to prepare a negative electrode slurry. The negative electrode slurry was applied to a copper (Cu) metal film having a thickness of 20 μm as a negative electrode collector, and dried. In this case, the temperature of the circulating air was 60°C. Then, the film was rolled and dried in a vacuum oven at 130°C for 12 hours to prepare a negative electrode.
[0224] By cutting the lithium metal foil into 1.7671 cm 2 A lithium (Li) metal thin film obtained by forming a circular shape of a positive electrode was used as a positive electrode. A porous polyethylene separator was interposed between the positive electrode and the above-mentioned negative electrode, and an electrolyte was injected to manufacture a lithium coin half-cell, wherein 0.5 parts by weight of vinylene carbonate was dissolved in a mixed solution in which ethyl methyl carbonate (EMC) and ethylene carbonate (EC) were mixed in a volume ratio of 7:3, and LiPF6 was dissolved to a concentration of 1M.
[0225] The prepared batteries were charged and discharged to evaluate the discharge capacity, initial efficiency, and capacity retention rate, which are shown in Table 2 below.
[0226] The charge and discharge were performed at 0.1 C for the first and second cycles, and at 0.5 C from the third to 49th cycles. At the 50th cycle, the charge and discharge were terminated in the charged state (lithium was contained in the negative electrode).
[0227] Charging conditions: CC (constant current) / CV (constant voltage) (5mV / 0.005C current cutoff)
[0228] Discharge condition: CC (constant current) condition 1.5V
[0229] The discharge capacity (mAh / g) and initial efficiency (%) were derived from the results after one charge and discharge. Specifically, the initial efficiency (%) was derived by the following calculation.
[0230] Initial efficiency (%) = (first discharge capacity / first charge capacity) × 100
[0231] The capacity retention rate is derived by the following calculation.
[0232] Capacity retention rate (%) = (49th discharge capacity / first discharge capacity) × 100
[0233] <Experimental Example: Evaluation of Shear Viscosity Characteristics>
[0234] As part of the processability evaluation, the shear viscosity change of the slurry prepared by mixing graphite, negative electrode active material, carbon black, CMC and SBR at a weight ratio of 77:20:1:1:1 under a shear rate (=1 Hz) was measured and shown in the following Table 2. Specifically, the shear viscosity change (%) was derived from the following calculation formula.
[0235] Shear viscosity change (%) = ((shear viscosity of slurry after 48 hours - shear viscosity of slurry immediately after mixing) / shear viscosity of slurry immediately after mixing) × 100
[0236]
[0237] The negative active material according to the present invention has a structure in which a layer containing Li, Al, P and O is closer to the silicon-based particles than the carbon layer. It can be confirmed that Examples 1 to 3 using the negative active material of the present invention have excellent discharge capacity, initial efficiency and capacity retention rate, and the shear viscosity of the slurry is significantly low, showing excellent processability. This seems to be because the layer containing Li, Al, P and O and close to the surface of the silicon-based particles can easily prevent reaction with moisture in the slurry; the hydrophobic carbon layer exists at the outermost layer to further block the contact between the negative active material and moisture, and improve the water-based processability of the slurry; the highly conductive carbon exists at the outermost layer, which has a favorable effect in achieving overall capacity / efficiency.
[0238] On the other hand, in Comparative Examples 1 and 2, it can be confirmed that since the carbon layer is tightly coated on the silicon-based particles as the first coating layer, and the layer containing Li, Al, P and O is coated on the first coating layer, it is difficult to remove the lithium by-products generated when the silicon-based particles are doped with Li, and since the carbon layer is not present in the outermost layer, side reactions are likely to occur in the slurry, making it difficult to achieve the processability of the slurry and the capacity / efficiency of the battery.
[0239] In addition, Comparative Example 3 corresponds to the case where the layer containing Li, Al, P, and O is coated on the silicon-based particles as a single layer without the second coating layer (carbon layer), and Comparative Example 4 corresponds to the case where a single layer (a layer containing Li, Al, P, O, and C) containing the material of the first coating layer and the material of the second coating layer is coated without distinguishing between the first coating layer and the second coating layer. In Comparative Examples 3 and 4, it can be confirmed that a single layer is formed, and thus contact between the negative electrode active material and water easily occurs, making the processability of the slurry and the capacity / efficiency of the battery worse than Comparative Examples 1 and 2.
[0240] Therefore, the present invention provides a negative electrode active material comprising: silicon-based particles; a first coating layer comprising Li, Al, P and O; and a second coating layer comprising carbon, thereby significantly improving overall aqueous processability, discharge capacity, efficiency and capacity retention.
Claims
1. A negative electrode active material, comprising: Silicon-based particles containing SiOx (0 < x < 2) and a Li compound; A first coating provided on at least a part of the silicon-based particles; and A second coating provided on at least a part of the first coating, wherein the first coating contains Li, Al, P, and O, and wherein the second coating contains carbon.
2. The negative electrode active material according to claim 1, wherein the second coating further contains Li, Al, P, and O.
3. The negative electrode active material according to claim 1, wherein the first coating contains Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) phase.
4. The negative electrode active material according to claim 1, wherein the first coating contains one or more selected from the group consisting of aluminum oxide, phosphorus oxide, lithium oxide, aluminum phosphate, lithium salt, lithium phosphate, and lithium aluminate.
5. The negative electrode active material according to claim 1, wherein the second coating further contains Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) phase.
6. The negative electrode active material according to claim 1, wherein based on a total of 100 parts by weight of the first coating and the second coating, the carbon content is 45 parts by weight or more and 95 parts by weight or less.
7. The negative electrode active material according to claim 1, wherein based on 100 parts by weight of the second coating, the carbon content exceeds 70 parts by weight.
8. The negative electrode active material according to claim 1, wherein the first coating is provided adjacent to the silicon-based particles.
9. The negative electrode active material according to claim 1, wherein the second coating is provided at the outermost layer of the negative electrode active material.
10. The negative electrode active material according to claim 1, wherein the second coating is an amorphous carbon layer.
11. The negative electrode active material according to claim 3, wherein based on a total of 100 parts by weight of the negative electrode active material, the Li y Al z P w Ov (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) The content of the phase is greater than 8 parts by weight and 50 parts by weight or less.
12. The negative electrode active material according to claim 1, wherein based on a total of 100 parts by weight of the negative electrode active material, the content of the second coating is 0.1 part by weight or more and 50 parts by weight or less.
13. The negative electrode active material according to claim 1, wherein based on a total of 100 parts by weight of the negative electrode active material, the content of Li is 0.1 part by weight or more and 40 parts by weight or less.
14. A method for manufacturing the negative electrode active material according to any one of claims 1 to 13, the method comprising: Prepare precursor silicon-based particles containing SiOx (0 < x < 2); Mix the precursor silicon-based particles with a Li precursor and heat-treat the mixture to prepare silicon-based particles; Set a first coating by mixing one or more selected from the group consisting of an Al precursor, a P precursor, and a precursor containing Al and P with the silicon-based particles and reacting them; and Form a second coating of a carbon precursor on the silicon-based particles provided with the first coating.
15. A method for manufacturing the negative electrode active material according to any one of claims 1 to 13, the method comprising: Prepare precursor silicon-based particles containing SiOx (0 < x < 2); Mix the precursor silicon-based particles with a Li precursor and heat-treat the mixture to prepare silicon-based particles; and Mix the silicon-based particles with one or more selected from the group consisting of an Al precursor, a P precursor, and a precursor containing Al and P and a carbon source, and heat-treat the mixture.
16. A negative electrode comprising the negative electrode active material according to any one of claims 1 to 13.
17. A secondary battery comprising the negative electrode according to claim 16.