High-viscosity anti-slip heating-free non-curing rubber asphalt waterproof coating

By developing a high-viscosity, anti-slip, heat-free non-curing rubber asphalt waterproof coating containing specific ingredients and optimized processes, the problem of open flames required for waterproof coil construction is solved, and construction convenience and safety without heating is achieved, and environmental protection is improved.

CN119505705APending Publication Date: 2025-02-25YUNNAN KUNMING YUBA BUILDING WATERPROOF MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411781590.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-05
Publication Date
2025-02-25

AI Technical Summary

Technical Problem

The construction of existing waterproof coils requires open flames, which limits the convenience and safety of construction. Especially when labor is expensive, there is a lack of heat-free waterproof material.

Method used

A high viscosity, anti-slip, heat-free non-curing rubber asphalt waterproof coating was developed, including national standard 70# asphalt, aromatic base oil, modifier SBS, styrene butadiene rubber SBR, temperature control agent and 325 mesh heavy calcium. Through specific stirring processes and equipment design, waterproof coatings can be constructed without heating.

Benefits of technology

The waterproof coating can realize the interface connection of the waterproof coil and fix the waterproof surface without heating, reducing dangerous operations, improving construction convenience and safety, and avoiding dust rising and improving environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119505705A_ABST
    Figure CN119505705A_ABST
Patent Text Reader

Abstract

The invention relates to the field of asphalt materials, in particular to a high-viscosity anti-slip heating-free non-curing rubber asphalt waterproof coating. The non-cured rubber asphalt waterproof coating comprises the following substances in parts by weight: 30 parts of national standard 70 # asphalt, 5 parts of aromatic base oil, 5 parts of a modifier SBS, 2 parts of butadiene styrene rubber SBS, 3 parts of a temperature control agent and 52 parts of 325-mesh coarse whiting. The high-shear emulsifying machine motor (7) is a power part of the high-shear emulsifying machine; the high-shear emulsifying machine is provided with an emulsifying barrel; an upper cover (8) is further included, a hole (9) is formed in the middle of the upper cover (8), and the high-shear emulsifying machine motor (7) penetrates through the hole (9); and the upper cover (8) can cover the stirring shell (1) to prevent dust from rising. Dangerous operation is reduced, and the use convenience is improved. And scientific investigation is safer. The upper cover (8) can cover the stirring shell (1) to prevent dust from rising; therefore, the high-speed stirring process is environment-friendly as much as possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of asphalt materials, in particular to a high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating. Background Art

[0002] Waterproof membranes are mainly used in building walls, roofs, tunnels, roads, landfills, etc. Compared with brush-on waterproof coatings, waterproof membranes have good stability and long service life.

[0003] The construction of waterproof membranes requires open flames, so their construction has certain limitations. In the current situation where labor is becoming more and more expensive, if waterproof materials that do not require heating can be provided, it will greatly facilitate the use of waterproof membranes.

[0004] On November 25, 2024, a search was conducted in the Chinese Patent Publication Database with "asphalt and aromatic and free and heating and SBS and SBR and calcium" as abstract keywords, and the option of allowing synonym expansion was checked, but no relevant literature was found.

[0005] On November 25, 2024, an abstract search for "asphalt and aromatic and free and heating and SBS and SBR and calcium" was conducted on China National Knowledge Infrastructure, and no relevant literature was found.

[0006] On November 25, 2024, Aromatic base asphalt with no heating SBS, SBR, and calcium "A search on the USPTO website did not find any relevant literature; the search URL is https: / / ppubs.uspto.gov / pubwebapp / .

[0007] On November 25, 2024, Asphalt, aromatic base, no heating, SBS SBR, and calcium "A search on the Korean Patent Office found no relevant literature; the search URL is engpat.kipris.or.kr.

[0008] On November 25, 2024, Asphalt, aromatic base, no heating, SBS SBR, and calcium "A search on WIPO's https: / / patentscope2.wipo.int / did not find any relevant documents.

[0009] On November 25, 2024, Asphalt, aromatic base, no heating, SBS SBR, and calcium "A search on the Japan Patent Office website https: / / www.j-platpat.inpit.go.jp / did not find any relevant literature.

[0010] Completely different from the concept of this patent. Summary of the invention

[0011] Purpose of the invention: To provide a high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating with better effect. The specific purpose can be seen in the multiple substantial technical effects in the specific implementation part.

[0012] In order to achieve the above purpose, the present invention adopts the following technical solutions: The high-viscosity, anti-skid, heat-free non-curing rubber asphalt waterproof coating is characterized in that the non-curing rubber asphalt waterproof coating contains the following substances in parts by weight: 30 parts of national standard 70# asphalt, 5 parts of aromatic base oil, 5 parts of modifier SBS, 2 parts of styrene-butadiene rubber SBR, 3 parts of temperature control agent, and 52 parts of 325 mesh heavy calcium.

[0013] The method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating as claimed in claim 1 is characterized in that: First, pump in 30 parts of national standard 70# asphalt and aromatic base oil; Start stirring when the temperature reaches 140 degrees Celsius; When the temperature reaches 185 degrees Celsius, add the modifier SBS and styrene-butadiene rubber SBR and carry out constant temperature modification for 3 hours; Add 325 mesh heavy calcium, stir for 40 minutes, and cool to 150 degrees Celsius; Add temperature control agent, stir for 1 hour, and slightly cool down to 130 degrees Celsius to prepare for discharging.

[0014] A further technical solution of the present invention is that the stirring device is implemented by a dust-free mixing production shear emulsification device, and the dust-free mixing production shear emulsification device comprises a stirring shell 1, and the stirring shell 1 is supported on the ground by supporting legs 2; it is characterized in that: The motor fixing plate 6 can be provided with a high shear emulsifier motor 7; The high shear emulsifier motor 7 is the power part of the high shear emulsifier; The high shear emulsifier is arranged with an emulsifying cylinder; A stirring shaft is arranged in the emulsifying cylinder, and the stirring shaft can be driven to rotate by the high shear emulsifying machine motor 7; It also includes an upper cover 8, the middle of which includes a hole 9, and the hole 9 is used to pass the high shear emulsifier motor 7; the upper cover 8 can cover the stirring shell 1 to prevent dust from being raised.

[0015] The solution is a mechanical structure capable of independent protection.

[0016] A further technical solution of the present invention is that a corresponding mounting plate 4 is arranged on the shell of the mixing shell 1, two groups of clamping walls are arranged at the edge of the corresponding mounting plate 4, and a wall gap 5 is arranged between the two groups of clamping walls; The wall gap 5 can be buckled on the upper edge of the mixing shell 1; A motor fixing plate 6 is arranged on the mounting corresponding plate 4 .

[0017] A further technical solution of the present invention is that the mounting corresponding plates 4 include two groups; and the upper cover 8 includes a circle of covering edge 10 .

[0018] A further technical solution of the present invention is that the covering edge 10 is made of rubber.

[0019] A further technical solution of the present invention is that a discharge pipe 3 is arranged below the stirring shell 1 .

[0020] Application of high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating in the construction of bonding membranes.

[0021] The present invention adopting the above technical solution has the following beneficial effects compared with the prior art: it allows the existing waterproof coiled material to achieve interface connection and fixation on the waterproof surface without spraying fire. First, it reduces dangerous operations, and second, it improves the convenience of use. Safer scientific research. The upper cover 8 can cover the mixing shell 1 to prevent dust from being raised; therefore, the high-speed mixing process can be as environmentally friendly as possible. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to further illustrate the present invention, the following is further described in conjunction with the accompanying drawings: Figure 1 A schematic diagram of the structure of the invention; Figure 2 This is the structural diagram of the high shear emulsifier; Figure 3 A stereogram of the invention; Figure 4 To invent a stereogram from another perspective; Figure 5 A side view of the invention; Figure 6 Another side view of the invention; Figure 7 A flowchart of the invention; Figure 8 and Figure 9 For test reports; Among them: 1. stirring shell; 2. supporting legs; 3. discharge pipe; 4. mounting corresponding plate; 5. wall gap; 6. motor fixing plate; 7. high shear emulsifier motor; 8. upper cover; 9. hole; 10. covering edge; 71. lower hole; 72. upper hole. DETAILED DESCRIPTION

[0023] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In the description of the present invention, it should be noted that the orientation or position relationship indicated by the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", "top", "bottom", etc. is based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood in specific circumstances.

[0024] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0025] This patent provides a variety of parallel solutions. The different expressions are improved solutions or parallel solutions based on the basic solution. Each solution has its own unique characteristics. In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other. The fixing method not described in the text can be any fixing method such as thread fixing, bolt fixing or glue bonding.

[0026] Embodiment 1: In combination with all the drawings; A highly viscous, anti-skid, and heat-free non-curing rubber asphalt waterproof coating, characterized in that the non-curing rubber asphalt waterproof coating comprises the following substances in parts by weight: 30 parts of national standard 70# asphalt, 5 parts of aromatic base oil, 5 parts of modifier SBS, 2 parts of styrene-butadiene rubber SBR, 3 parts of temperature control agent, and 52 parts of 325 mesh heavy calcium carbonate.

[0027] The substantial technical effects and implementation process of the technical solution provided by this department, i.e. the basic functions, are as follows: the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating provided by this solution allows existing waterproof membranes to achieve interface connection and fixation on the waterproof surface without spraying fire. The first is to reduce dangerous operations, and the second is to improve the convenience of use. Safer scientific expeditions.

[0028] The temperature control agent is a non-curing waterproof asphalt temperature control agent; The aromatic base oil is aromatic oil.

[0029] Embodiment 2: As a further improved scheme or parallel scheme or optional independent scheme, a method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating as claimed in claim 1 is characterized in that: First, pump in 30 parts of national standard 70# asphalt and aromatic base oil; Start stirring when the temperature reaches 140 degrees Celsius; When the temperature reaches 185 degrees Celsius, add the modifier SBS and styrene-butadiene rubber SBR and carry out constant temperature modification for 3 hours; Add 325 mesh heavy calcium, stir for 40 minutes, and cool to 150 degrees Celsius; Add temperature control agent, stir for 1 hour, and slightly cool down to 130 degrees Celsius to prepare for discharging.

[0030] As a more specific implementation structure, the stirring device is implemented by a dust-free mixing production shear emulsification device, and the dust-free mixing production shear emulsification device includes a stirring shell 1, and the stirring shell 1 is supported on the ground by a supporting leg 2; it is characterized in that: The motor fixing plate 6 can be provided with a high shear emulsifier motor 7; The high shear emulsifier motor 7 is the power part of the high shear emulsifier; The high shear emulsifier is arranged with an emulsifying cylinder; A stirring shaft is arranged in the emulsifying cylinder, and the stirring shaft can be driven to rotate by the high shear emulsifying machine motor 7; It also includes an upper cover 8, the middle of which includes a hole 9, and the hole 9 is used to pass the high shear emulsifier motor 7; the upper cover 8 can cover the stirring shell 1 to prevent dust from being raised.

[0031] This solution is a mechanical structure that can be independently protected. The upper cover 8 can cover the stirring shell 1 to prevent dust from being raised; therefore, the high-speed stirring process can be as environmentally friendly as possible.

[0032] Embodiment 3: As a further improved solution or a parallel solution or an optional independent solution, a corresponding plate 4 is arranged on the shell of the mixing shell 1, two groups of clamping walls are arranged on the edge of the corresponding plate 4, and a wall gap 5 is arranged between the two groups of clamping walls; The wall gap 5 can be buckled on the upper edge of the mixing shell 1; The motor fixing plate 6 is arranged on the mounting corresponding plate 4. The substantial technical effect and implementation process of the technical solution here, i.e. the basic function, are as follows: the significant feature of this embodiment is that the high shear emulsifier above can be quickly disassembled for cleaning, because after each production, the equipment must be cleaned for the quality of the next product. This structure can allow the overall power part to be quickly separated from the mixing shell 1 and can be quickly cleaned. However, when working, it can be quickly fixed and installed back.

[0033] Embodiment 4: As a further improved solution or parallel solution or optional independent solution, the corresponding plates 4 are installed to include two groups; the upper cover 8 includes a circle of covering edges 10. The substantial technical effects and the implementation process of the technical solution here, i.e. the basic functions, are as follows: the covering edge 10 has a better covering effect, a better environmental protection effect, and is more friendly to workers.

[0034] Embodiment 5: As a further improved solution or parallel solution or optional independent solution, the covering edge 10 is made of rubber. The substantial technical effect and implementation process of the technical solution here, i.e., the basic function, are as follows: Similar materials are within the protection scope of this patent.

[0035] Embodiment 6: As a further improved solution or a parallel solution or an optional independent solution, a discharge pipe 3 is arranged below the stirring shell 1 .

[0036] Application of high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating in the construction of bonding membranes.

[0037] High-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating has important uses in the construction of adhesive membranes, mainly in the following aspects: 1. Excellent waterproof performance This waterproof coating has good adhesion and sealing properties, and can be closely combined with various membranes to form a seamless waterproof system. It can effectively prevent water penetration and prevent buildings from being damaged by water erosion. Its high viscosity ensures that it can be firmly attached to various complex base surfaces, and maintains a good waterproof effect even when there are tiny cracks or deformations in the base.

[0038] 2. Construction convenience Heating-free feature: Construction can be carried out without heating, which greatly simplifies the construction process, improves construction efficiency, and also reduces safety risks during construction.

[0039] Easy to operate: It can be applied in a variety of ways, such as spraying and scraping, to adapt to different construction environments and requirements. It is also very convenient to bond with the coiled material, without the need for special tools and techniques, and can be completed by ordinary construction workers.

[0040] 3. Basic Data Viscosity: Usually has a higher viscosity, usually tens of thousands of centipoise or even higher, which can ensure a strong bond with the coil.

[0041] Anti-slip performance: The surface has a certain degree of anti-slip properties, which can prevent people from slipping on the waterproof surface after construction. The specific anti-slip coefficient will vary depending on the product, and is generally within a certain range of friction coefficient.

[0042] Elongation: With a high elongation, it can adapt to the deformation and cracks of the base layer and ensure the durability of the waterproof effect. The elongation is usually several hundred% or even higher.

[0043] Durability: It has good durability and can maintain stable performance during long-term use. Its service life can generally reach several years or even longer, depending on the use environment and maintenance.

[0044] It should be noted that the multiple solutions provided by this patent include the basic solution itself, which are independent of each other and do not restrict each other, but they can also be combined with each other without conflict to achieve multiple effects together.

[0045] The basic principle, main features and advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the protection required.

Claims

1. High-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating, characterized in that: The non-curing rubber asphalt waterproof coating contains the following materials in parts by weight: 30 parts of national standard 70# asphalt, 5 parts of aromatic base oil, 5 parts of modifier SBS, 2 parts of styrene-butadiene rubber SBR, 3 parts of temperature control agent, and 52 parts of 325 mesh heavy calcium carbonate.

2. A method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating as claimed in claim 1, characterized in that: First, pump in 30 parts of national standard 70# asphalt and aromatic base oil; Start stirring when the temperature reaches 140 degrees Celsius; When the temperature reaches 185 degrees Celsius, add the modifier SBS and styrene-butadiene rubber SBR and carry out constant temperature modification for 3 hours; Add 325 mesh heavy calcium, stir for 40 minutes, and cool to 150 degrees Celsius; Add temperature control agent, stir for 1 hour, and slightly cool down to 130 degrees Celsius to prepare for discharging.

3. The method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating according to claim 1, characterized in that: The stirring device is implemented by using a dust-free mixing production shear emulsification device, and the dust-free mixing production shear emulsification device comprises a stirring shell (1), and the stirring shell (1) is supported on the ground by supporting legs (2); it is characterized in that: A high shear emulsifier motor (7) can be arranged on the motor fixing plate (6); The high shear emulsifier motor (7) is the power part of the high shear emulsifier; The high shear emulsifier is arranged with an emulsifying cylinder; A stirring shaft is arranged in the emulsifying cylinder, and the stirring shaft can be driven by the high shear emulsifying machine motor (7) to rotate; It also includes an upper cover (8), the middle part of which includes a hole (9), and the hole (9) is used to pass the high shear emulsifier motor (7); the upper cover (8) can cover the stirring shell (1) to prevent dust from being raised.

4. The method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating according to claim 3, characterized in that: A mounting corresponding plate (4) is arranged on the shell of the mixing shell (1), two groups of clamping walls are arranged at the edge of the mounting corresponding plate (4), and a wall gap (5) is arranged between the two groups of clamping walls; The wall gap (5) can be buckled on the upper edge of the mixing shell (1); A motor fixing plate (6) is arranged on the mounting corresponding plate (4).

5. The method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating according to claim 3, characterized in that: The mounting corresponding plates (4) include two groups; the upper cover (8) includes a circular covering edge (10).

6. The method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating according to claim 5, characterized in that: The cover edge (10) is made of rubber.

7. The method for preparing the high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating according to claim 3, characterized in that: A discharge pipe (3) is arranged below the stirring shell (1).

8. The use of high-viscosity, anti-skid, heat-free, non-curing rubber asphalt waterproof coating in the construction of bonding membranes.

Citation Information

Patent Citations

  • Batch-type high shear emulsifying machine

    CN103055741A

  • Non-cured rubber asphalt waterproof coating, preparation method of coating and root puncture resistant waterproof material

    CN110724455A

  • Asphalt base material stirring cutter

    CN205627740U

  • Mortar mixing and stirring device

    CN219404798U