A welding method for CT tube housing window
By combining hot-forming pre-bending with welding fixtures, the problems of high fixture consumption, high risk of sticking and uneven clamping force in the welding of CT tube shell windows are solved. This achieves efficient welding with reusable fixtures, uniform clamping force, and convenient assembly and disassembly, thereby improving production efficiency and welding quality.
Patent Information
- Application Number
- CN202611519563.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-10
AI Technical Summary
In existing CT tube housing window welding methods, the tooling is a disposable consumable, which is costly, prone to sticking, has uneven clamping force, and is cumbersome to assemble and disassemble, making it difficult to meet the requirements of mass production.
Using hot-forming pre-bending and welding fixtures, positioning is achieved through limiting posts and limiting holes, and uniform clamping force is provided by its own weight. High-temperature resistant and non-wetting materials are used, combined with segmented heat preservation temperature curves and a high-temperature vacuum brazing furnace to achieve reusable high-quality welding.
It reduces the cost of consumables, avoids the risk of sticking during welding, improves production yield and efficiency, and ensures the tightness and consistency of the brazing seam.
Smart Images

Figure CN123060187A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal welding technology, specifically to a welding method for a CT tube housing window. Background Technology
[0002] The CT tube is a core component of computed tomography (CT) scanners, and its housing window requires a highly reliable vacuum seal between the cupronickel housing and the titanium window. Due to the significant differences in the physicochemical properties of cupronickel and titanium, vacuum brazing is typically used to achieve this connection. During the welding process, a constant and uniform clamping force needs to be applied to the interface to ensure sufficient spread of the brazing filler metal and good capillary filling, thereby obtaining a dense, defect-free brazed seam structure that meets the high vacuum and high reliability requirements of the CT tube.
[0003] In existing technologies, vacuum welding of cupronickel titanium windows commonly employs screw-locking fixtures for welding clamping. Specifically, the unbent titanium window is clamped and pressed firmly using a hose clamp before being fed into a vacuum furnace for welding. This method relies on the mechanical locking force of screws or hose clamps to apply pressure to the welding interface. The accompanying fixtures are typically disposable, requiring scrapping or being difficult to reuse after each batch of welding, resulting in high production material costs.
[0004] Furthermore, in high-temperature vacuum welding environments, traditional locking fixtures have the following prominent drawbacks: First, the fixtures are disposable consumables, resulting in high material costs and increasing the manufacturing cost of the CT tube housing window. Second, during high-temperature vacuum welding, the contact area between the fixture and the product is prone to sticking, posing a risk of the fixture adhering to the product, potentially causing workpiece scrap and reducing production yield. Simultaneously, the uneven distribution of clamping force in screw locking methods can easily lead to insufficient or excessive clamping in certain areas, affecting the consistency of the brazing seam quality. The assembly and disassembly process is cumbersome and time-consuming, making it difficult to meet the efficiency requirements of mass production.
[0005] Therefore, there is an urgent need for a welding method for CT tube housing windows that allows for reusable tooling, avoids the risk of sticking during welding, provides uniform and controllable clamping force, and is convenient and efficient for assembly and disassembly, in order to overcome the above-mentioned shortcomings of the existing technology. Summary of the Invention
[0006] To solve the above-mentioned technical problems, the present invention provides a method for welding the window of a CT tube housing.
[0007] The technical solution of the present invention is: a method for welding a CT tube housing window, comprising the following steps: S1, Hot-formed pre-bending: Prepare a titanium window and a CT tube housing with the window. Place the titanium window in a heat-setting fixture and heat it to 600-850℃ under vacuum for 20-60 minutes. Then cool it down to below 100℃ with the furnace and take it out to obtain an arc-shaped titanium window that matches the window of the CT tube housing. S2, Assembly Limit: Align the arc-shaped titanium window obtained in S1 with the CT tube housing window, and place solder between the titanium window and the CT tube housing window; place a welding fixture above the titanium window, and limit the welding fixture by the existing studs on the CT tube housing to obtain the assembled component. S3, Vacuum Brazing: The assembled components are sent into a vacuum brazing furnace, a vacuum is drawn, and the furnace is heated according to a set temperature curve to melt the solder and complete the vacuum brazing. S4. Cooling and demolding: After welding, the furnace is powered off and cooled to 600°C. Nitrogen or argon is then introduced into the vacuum brazing furnace to a pressure of 0.05-0.1 MPa. Subsequently, the furnace is forced to cool to 50°C using a fan before being removed from the furnace. After removal from the furnace, the welding fixtures are removed to obtain the welded CT tube housing window assembly.
[0008] Furthermore, the heat-adjusting fixture mentioned in S1 includes a titanium window heat-adjusting fixture base, on which multiple arc-shaped platforms are provided, and a titanium window heat-adjusting fixture pressure block is provided on each arc-shaped platform. A limiting post is fixedly connected to each of the front and rear sides above the arc-shaped platform, and a limiting hole for fitting the limiting post is provided on each of the front and rear sides below the titanium window heat-adjusting fixture pressure block.
[0009] Description: This hot-forming fixture uses multiple curved platforms and pressure blocks for coordination, and uses limiting posts and limiting holes for positioning, so that the titanium window is subjected to uniform force and accurate position during the hot-forming process, effectively ensuring the consistency of the pre-bending curvature and improving the pre-bending accuracy and efficiency.
[0010] Furthermore, the welding fixture in S2 includes a counterweight block. The lower center of the counterweight block is provided with a pressing surface that fits the curvature of the titanium window. The pressing surface is provided with gap grooves on both sides. The outer sides of the two gap grooves are provided with limiting grooves for engaging with studs on the CT tube housing. The counterweight block is provided with multiple heat dissipation holes for heat dissipation.
[0011] Description: This welding fixture achieves fast, threadless positioning and uniform clamping by using a pressing surface to fit the curvature of the titanium window, a limiting groove to quickly engage with the housing stud, and is equipped with a gap groove and heat dissipation holes. This prevents the fixture from sticking to the brazing filler metal and also facilitates uniform heat dissipation during the welding process, thereby improving welding quality.
[0012] Furthermore, the welding fixture described in S2 weighs 0.2-0.5 kg, and the assembly gap between the titanium window and the CT tube housing window is maintained at 0.03-0.05 mm.
[0013] Explanation: By controlling the weight of the welding fixture and maintaining a reasonable assembly gap, a constant and uniform clamping force can be provided by its own weight, while ensuring sufficient capillary filling of the brazing filler metal, avoiding material shortage due to excessive gap or slag inclusion due to insufficient gap.
[0014] Furthermore, the solder described in S2 is composed of the following components by mass percentage: 25-29% Cu, 2.5-3.8% Ti, 0.8-1.8% Ni, 0.8-2.2% In, with the balance being Ag; Note: This silver-based brazing filler metal, through the synergistic ratio of Ag-Cu-Ti-Ni-In, effectively inhibits the excessive formation of brittle intermetallic compounds while ensuring good wettability and flowability, thereby improving the tightness of the brazing joint, joint strength, and sealing reliability.
[0015] Furthermore, the temperature curve set in S3 is as follows: keep warm at 350℃ for 55-65 minutes; keep warm at 650℃ for 70-100 minutes; keep warm at 850℃ for 95-138 minutes.
[0016] Note: This segmented heat preservation temperature curve allows the brazing filler metal to fully melt, spread and diffuse, reducing welding thermal stress and avoiding defects such as incomplete brazing and porosity caused by excessively rapid heating or insufficient heat preservation, thus obtaining a uniform and dense brazing seam structure.
[0017] Furthermore, the vacuum brazing furnace is an HVF60901Q type high-temperature vacuum brazing furnace, with in-furnace molybdenum strip radiant heating as the heating method. The power supply is a thyristor low-voltage high-current AC power supply, industrial frequency AC, non-polar, and evacuated to 1×10⁻⁶. -2 Heating should be turned on when the pressure is below MPa.
[0018] Description: The HVF60901Q high-temperature vacuum brazing furnace, molybdenum strip radiation heating, and thyristor low-voltage high-current power frequency AC power supply are used to achieve uniform, stable, and precise heating control in a vacuum environment, meeting the high-quality vacuum brazing requirements of CT tube shell windows.
[0019] Furthermore, both the welding fixture and the heat-forming fixture are made of a high-temperature resistant material that does not wet the solder, and the material is selected from one of graphite, boron nitride coated graphite, alumina ceramic, and molybdenum alloy.
[0020] Note: The tooling is made of high-temperature resistant materials such as graphite, boron nitride coated graphite, alumina ceramic, or molybdenum alloy, which do not wet the solder. This effectively prevents the tooling from sticking to the product during high-temperature vacuum welding, ensuring that the tooling can be reused, reducing consumable costs and improving product yield.
[0021] Furthermore, the above-mentioned method for welding the CT tube housing window also includes S5. S5. Post-welding inspection: The welded CT tube housing window assembly was subjected to helium leak testing and ultrasonic testing. The helium leak testing used a helium mass spectrometer to test the overall sealing of the welded CT tube housing window assembly. The ultrasonic testing used water immersion ultrasonic C-scan technology to perform non-destructive testing on the brazed joint of the welded CT tube housing window.
[0022] Note: By performing dual non-destructive testing on the brazed joint using helium leak detection and ultrasonic C-scan, the sealing performance and internal defects of the brazed joint can be accurately assessed, ensuring the high reliability and safety of the CT tube housing window assembly.
[0023] The beneficial effects of this invention are: (1) The welding fixture and heat-forming fixture described in this invention can be directly disassembled and reused after a batch of welding is completed, without having to be scrapped as disposable consumables, thereby significantly reducing the cost of tooling consumables and long-term production costs, and are especially suitable for the mass production of CT tube housing windows.
[0024] (2) The tooling of the present invention does not require threaded locking or hose clamping between the tooling and the product. The tooling is made of high temperature resistant material that does not wet the brazing filler metal, which can effectively avoid the risk of the tooling sticking to the product during high temperature vacuum welding, reduce product damage and scrap, and improve production yield.
[0025] (3) The tooling of the present invention applies a constant and uniform clamping force to the interface to be welded by its own weight. The pressure distribution is controllable, which can avoid local insufficient or excessive clamping, which is conducive to the uniform spreading and capillary filling of the brazing filler metal, and ensures the density and consistency of the brazing seam.
[0026] (4) The tooling of the present invention achieves rapid positioning by limiting or snap-fitting the housing stud. No thread locking operation is required for assembly and disassembly. It is convenient and efficient to assemble and disassemble, which can significantly shorten the assembly and demolding time of the workpiece and improve the mass production efficiency of the CT tube housing window assembly. Attached Figure Description
[0027] Figure 1 This is a three-dimensional view of the thermal alignment tooling of the present invention.
[0028] Figure 2 This is a 3D view of the substrate of the titanium window thermal alignment tooling.
[0029] Figure 3 This is a schematic diagram of the welding fixture of the present invention.
[0030] Figure 4 This is a bottom view of the welding fixture of the present invention.
[0031] Figure 5 This is a schematic diagram of the welding fixture and CT tube housing assembly of the present invention.
[0032] Among them, 1-heat-correcting fixture, 11-titanium window heat-correcting fixture base, 12-arc surface platform, 13-titanium window heat-correcting fixture pressure block, 14-limiting post, 15-limiting hole, 2-welding fixture, 21-counterweight block, 22-pressing surface, 23-gap groove, 24-limiting groove, 25-heat dissipation hole. Detailed Implementation
[0033] Example 1: A method for welding a CT tube housing window, comprising the following steps: S1, Hot-formed pre-bending: Prepare a titanium window and a CT tube housing with the window. Place the titanium window in a heat-setting fixture 1 and heat it to 600°C under vacuum for 20 minutes. Then, cool it to below 100°C with the furnace and take it out to obtain an arc-shaped titanium window that matches the window of the CT tube housing. like Figure 1 , Figure 2 As shown, the heat-forming fixture 1 includes a titanium window heat-forming fixture base 11. Multiple curved platforms 12 are provided on the base 11, and each curved platform 12 is equipped with a titanium window heat-forming fixture pressure block 13. A limiting post 14 is fixedly connected to the front and rear sides of the curved platform 12. A limiting hole 15 for engaging the limiting post 14 is provided on the front and rear sides of the pressure block 13 below. This heat-forming fixture, through the cooperation of multiple curved platforms and pressure blocks, and the positioning by engaging the limiting posts and limiting holes, ensures that the titanium window is subjected to uniform force and accurate positioning during the heat-forming process, effectively guaranteeing the consistency of the pre-bending curvature and improving pre-bending accuracy and efficiency.
[0034] S2, Assembly Limit: like Figure 5 As shown, the arc-shaped titanium window obtained by S1 is aligned with the CT tube housing window, and solder is placed between the titanium window and the CT tube housing window; welding fixture 2 is placed above the titanium window, and welding fixture 2 is limited by the existing studs on the CT tube housing to obtain the assembled component. like Figure 3 , Figure 4As shown, the welding fixture 2 includes a counterweight 21. The lower center of the counterweight 21 is provided with a pressing surface 22 that fits the curvature of the titanium window. The pressing surface 22 is provided with gap grooves 23 on both sides. The outer sides of the two gap grooves 23 are provided with limiting grooves 24 for engaging with the studs on the CT tube housing. The counterweight 21 is provided with multiple heat dissipation holes 25 for heat dissipation.
[0035] This welding fixture achieves threadless, rapid positioning and uniform clamping by using a tight-fitting surface to conform to the curvature of the titanium window, a limiting groove to quickly engage with the housing stud, and is equipped with a gap groove and heat dissipation holes. This prevents the fixture from sticking to the brazing filler metal and also facilitates uniform heat dissipation during the welding process, thereby improving welding quality.
[0036] Both welding fixture 2 and heat-forming fixture 1 are made of a high-temperature resistant material that does not wet the solder; the material is selected from graphite. This material effectively prevents the fixture from sticking to the product during high-temperature vacuum welding, ensuring the fixture can be reused, reducing material costs, and improving product yield.
[0037] The welding fixture 2 weighs 0.2 kg, and the assembly gap between the titanium window and the CT tube housing window is maintained at 0.03 mm. By controlling the weight of the welding fixture and maintaining a reasonable assembly gap, a constant and uniform clamping force can be provided by its own weight, while ensuring sufficient capillary filling of the brazing filler metal, avoiding material shortage due to excessive gap or slag inclusion due to insufficient gap.
[0038] The solder is composed of the following components by mass percentage: 25% Cu, 2.5% Ti, 0.8% Ni, 0.8% In, with the balance being Ag. This silver-based solder, through the synergistic ratio of Ag-Cu-Ti-Ni-In, effectively inhibits the excessive formation of brittle intermetallic compounds while ensuring good wettability and flowability, thereby improving the tightness of the brazing joint, joint strength, and sealing reliability.
[0039] S3, Vacuum Brazing: The assembled components are sent into a vacuum brazing furnace, a vacuum is drawn, and the furnace is heated according to a set temperature curve to melt the solder and complete the vacuum brazing. The temperature profile is set as follows: 350℃ for 55 min; 650℃ for 70 min; and 850℃ for 95 min. This segmented holding temperature profile allows the brazing filler metal to fully melt, spread, and diffuse, reducing welding thermal stress and avoiding defects such as incomplete brazing and porosity caused by excessively rapid heating or insufficient holding, thus obtaining a uniform and dense brazed joint structure.
[0040] The vacuum brazing furnace is an HVF60901Q type high-temperature vacuum brazing furnace. Heating is achieved through in-furnace molybdenum strip radiant heating. The power supply is a thyristor-controlled low-voltage, high-current AC power supply (mains frequency, non-polarity), and the furnace is evacuated to a vacuum level of 0.8 × 10⁻⁶. -2Heating is activated at MPa. The system employs an HVF60901Q high-temperature vacuum brazing furnace with molybdenum strip radiant heating and a thyristor-controlled low-voltage, high-current AC power supply, enabling uniform, stable, and precise heating control under vacuum conditions, meeting the high-quality vacuum brazing requirements for CT tube housing windows.
[0041] S4. Cooling and demolding: After welding, the furnace was powered off and cooled to 600°C. Nitrogen gas was then introduced into the vacuum brazing furnace until the pressure was 0.05 MPa. Subsequently, the furnace was cooled to 50°C by a fan before being removed from the furnace. After removal from the furnace, welding fixture 2 was removed to obtain the welded CT tube housing window assembly.
[0042] Example 2: This example, based on Example 1, further includes S5. S5. Post-welding inspection: The welded CT tube housing window assembly was subjected to helium leak testing and ultrasonic testing. Helium leak testing used a helium mass spectrometer to test the overall sealing of the welded CT tube housing window assembly. Ultrasonic testing used water immersion ultrasonic C-scan technology to perform non-destructive testing on the brazed joint of the welded CT tube housing window.
[0043] Compared to Example 1, this embodiment uses helium leak detection and ultrasonic C-scan to perform dual non-destructive testing on the brazed joint, which can accurately assess the sealing of the brazed joint and internal defects, ensuring the high reliability and safety of the CT tube housing window assembly.
[0044] Example 3: The difference between this example and Example 2 is that in S1, the temperature is heated to 750°C under vacuum and held for 40 minutes, and then cooled to below 100°C in the furnace before being taken out. Example 4: The difference between this example and Example 2 is that in S1, the temperature is heated to 850°C under vacuum and held for 60 minutes, and then cooled to below 100°C in the furnace before being taken out. The performance of the welded CT tube housing window assembly in Examples 2-4 was tested, and the test results are shown in Table 1. Table 1: Performance Comparison of CT Tube Housing Window Assembly After Welding in Examples 2-4
[0045] Comparing the performance of the CT tube housing window assembly after welding in Examples 2-4, Example 3, under the conditions of moderate heat straightening temperature and holding time, achieved the highest brazing rate, the lowest porosity and leakage rate, and the best overall welding effect.
[0046] Example 5: The difference between this example and Example 3 is that in S2, the material is selected from boron nitride coated graphite.
[0047] Example 6: The difference between this example and Example 3 is that in S2, the material is selected from alumina ceramic.
[0048] Example 7: The difference between this example and Example 3 is that in S2, the material is selected from molybdenum alloy.
[0049] The performance of the welded CT tube housing window assembly in Example 3 and Examples 5-7 was tested, and the test results are shown in Table 2. Table 2: Performance Comparison of CT Tube Housing Window Assembly After Welding in Example 3 and Examples 5-7
[0050] Comparing the performance of the CT tube housing window assembly after welding in Examples 3 and Examples 5-7, the boron nitride coated graphite used in Example 5 combines the advantages of graphite's high temperature resistance and easy processing with the excellent non-wetting and anti-sticking properties of boron nitride. It has the least interface contamination and thermal stress, the highest brazing rate, the lowest porosity inside the brazed seam and the lowest overall leakage rate, and the best overall welding effect.
[0051] Example 8: The difference between this example and Example 5 is that in S2, the weight of welding fixture 2 is 0.3kg, and the assembly gap between the titanium window and the CT tube housing window is maintained at 0.04mm.
[0052] Example 9: The difference between this example and Example 5 is that in S2, the weight of welding fixture 2 is 0.5kg, and the assembly gap between the titanium window and the CT tube housing window is maintained at 0.05mm.
[0053] The performance of the welded CT tube housing window assembly in Example 5 was compared with that in Examples 8 and 9. The test results are shown in Table 3. Table 3: Performance Comparison of CT Tube Housing Window Assembly After Welding in Examples 5, 8, and 9
[0054] Comparing the performance of the CT tube housing window assembly welded in Examples 5, 8, and 9, Example 8, based on the boron nitride coated graphite tooling, has better matching of clamping force and gap, sufficient capillary filling of brazing filler metal without excessive extrusion, minimal interface contamination and thermal stress, the highest brazing rate, the lowest porosity inside the brazing seam and the lowest overall leakage rate, and the best overall welding effect.
[0055] Example 10: This example differs from Example 8 in that, in S2, the solder is composed of the following components by mass percentage: 28% Cu, 3.1% Ti, 1.1% Ni, 1.5% In, with the balance being Ag; Example 11: This example differs from Example 8 in that, in S2, the solder is composed of the following components by mass percentage: 29% Cu, 3.8% Ti, 1.8% Ni, 2.2% In, with the balance being Ag; The performance of the welded CT tube housing window assembly in Example 8 was compared with that in Examples 10 and 11. The test results are shown in Table 4. Table 4: Performance Comparison of CT Tube Housing Window Assembly After Welding in Example 8, Example 10, and Example 11
[0056] Comparing the performance of the CT tube housing window assembly after welding in Examples 8, 10, and 11, Example 10 shows that the Ag-Cu-Ti-Ni-In synergistic ratio is better, the brazing filler metal has better wettability and fluidity, effectively inhibits the formation of brittle intermetallic compounds, has the highest brazing rate, the lowest porosity inside the brazing seam and the lowest overall leakage rate, and the best overall welding effect.
[0057] Example 12: The difference between this example and Example 10 is that in S3, the temperature curve is set as follows: keep warm at 350℃ for 60 min; keep warm at 650℃ for 90 min; keep warm at 850℃ for 100 min.
[0058] Example 13: The difference between this example and Example 10 is that in S3, the temperature curve is set as follows: keep warm at 350℃ for 65 minutes; keep warm at 650℃ for 100 minutes; keep warm at 850℃ for 138 minutes.
[0059] The performance of the welded CT tube housing window assembly in Example 10, Example 12, and Example 13 was tested, and the test results are shown in Table 5. Table 5: Performance Comparison of CT Tube Housing Window Assembly After Welding in Example 10, Example 12, and Example 13
[0060] Comparing the performance of the CT tube housing window assembly after welding in Examples 10, 12, and 13, Example 12 appropriately extended the heat preservation time of each section based on Example 10, so that the brazing filler metal melted, spread and diffused more fully, while avoiding excessive heat preservation which would lead to grain coarsening or brazing filler metal loss. As a result, the brazing rate was the highest, the porosity inside the brazing seam was the lowest and the overall leakage rate was the lowest, and the overall welding effect was the best.
[0061] Example 14: This example differs from Example 12 in that, in S3, the vacuum is evacuated to 0.5 × 10⁻⁶. -2 Heating should be turned on when the pressure is below MPa.
[0062] Example 15: This example differs from Example 12 in that, in S3, the vacuum is evacuated to 0.3 × 10⁻⁶. -2 Heating should be turned on when the pressure is below MPa.
[0063] The performance of the welded CT tube housing window assembly in Comparative Example 12 with Examples 14 and 15 was tested, and the test results are shown in Table 6. Table 6: Performance Comparison of CT Tube Housing Window Assembly After Welding in Examples 12, 14, and 15
[0064] Comparing the performance of the CT tube housing window assembly after welding in Examples 12, 14, and 15, Example 15 further improves the vacuum level based on Example 12, effectively reducing residual gas and oxidizing atmosphere in the furnace, keeping the interface between the titanium window and the cupronickel housing to be welded and the surface of the brazing filler metal cleaner, resulting in better brazing wettability and spreadability of the brazing filler metal, more complete interface diffusion, the highest brazing rate, the lowest porosity inside the brazing seam and the lowest overall leakage rate, and the best overall welding effect.
[0065] Example 16: The difference between this example and Example 15 is that in S4, after welding is completed, the furnace is powered off and cooled to 600°C, and then argon gas is introduced into the vacuum brazing furnace to a pressure of 0.08 MPa.
[0066] Example 17: The difference between this example and Example 15 is that in S4, after welding is completed, the furnace is powered off and cooled to 600°C, and then argon gas is introduced into the vacuum brazing furnace to a pressure of 0.1 MPa.
[0067] The performance of the welded CT tube housing window assembly in Examples 15-17 was tested, and the test results are shown in Table 7. Table 7: Performance Comparison of CT Tube Housing Window Assembly After Welding in Examples 15-17
[0068] Comparing the performance of the CT tube housing window assembly after welding in Examples 15-17, Example 17 further increases the cooling protective gas pressure based on Example 15, making the atmosphere protection more sufficient and the cooling more uniform during the cooling process of the high-temperature workpiece, effectively suppressing oxidation and secondary pollution, resulting in the highest brazing rate, the lowest porosity inside the brazing seam and the lowest overall leakage rate, and the best overall welding effect.
Claims
1. A method for welding a CT tube housing window, characterized in that, Includes the following steps: S1. Hot-formed pre-bending: Prepare a titanium window and a CT tube housing with a window. Place the titanium window in a heat-setting fixture (1) and heat it to 600-850℃ under vacuum for 20-60 minutes. Then cool it down to below 100℃ with the furnace and take it out to obtain an arc-shaped titanium window that matches the window of the CT tube housing. S2, Assembly Limit: Align the arc-shaped titanium window obtained in S1 with the CT tube housing window, and place solder between the titanium window and the CT tube housing window; place a welding fixture (2) above the titanium window, and limit the welding fixture (2) by the existing studs on the CT tube housing to obtain the assembled component; S3, Vacuum brazing: The assembled components are sent into a vacuum brazing furnace, a vacuum is drawn, and the furnace is heated according to a set temperature curve to melt the solder and complete the vacuum brazing. S4. Cooling and demolding: After welding, the furnace is powered off and cooled to 600°C. Nitrogen or argon is then introduced into the vacuum brazing furnace to a pressure of 0.05-0.1 MPa. The furnace is then forced to cool to 50°C using a fan before being removed from the furnace. After removal from the furnace, the welding fixture (2) is removed to obtain the welded CT tube housing window assembly.
2. The welding method for a CT tube housing window as described in claim 1, characterized in that, The heat-adjusting fixture (1) described in S1 includes a titanium window heat-adjusting fixture base (11). The titanium window heat-adjusting fixture base (11) is provided with multiple arc-shaped platforms (12). Each arc-shaped platform (12) is provided with a titanium window heat-adjusting fixture pressure block (13). A limiting post (14) is fixedly connected to the front and rear sides above the arc-shaped platform (12). A limiting hole (15) for fitting the limiting post (14) is provided on the front and rear sides below the titanium window heat-adjusting fixture pressure block (13).
3. The welding method for a CT tube housing window as described in claim 1, characterized in that, The welding fixture (2) described in S2 includes a counterweight (21). The counterweight (21) has a pressing surface (22) at the lower center that fits the curvature of the titanium window. The pressing surface (22) has gap grooves (23) on both sides. The outer sides of the two gap grooves (23) are provided with limiting grooves (24) for engaging with the studs on the CT tube housing. The counterweight (21) has multiple heat dissipation holes (25) for heat dissipation.
4. The welding method for a CT tube housing window as described in claim 1, characterized in that, The welding fixture (2) mentioned in S2 weighs 0.2-0.5 kg, and the assembly gap between the titanium window and the CT tube housing window is maintained at 0.03-0.05 mm.
5. The welding method for a CT tube housing window as described in claim 1, characterized in that, The solder described in S2 consists of the following components by mass percentage: 25-29% Cu, 2.5-3.8% Ti, 0.8-1.8% Ni, 0.8-2.2% In, with the balance being Ag.
6. The welding method for a CT tube housing window as described in claim 1, characterized in that, The temperature curves set in S3 are as follows: keep warm at 350℃ for 55-65 minutes; keep warm at 650℃ for 70-100 minutes; keep warm at 850℃ for 95-138 minutes.
7. The welding method for a CT tube housing window as described in claim 1, characterized in that, The vacuum brazing furnace is an HVF60901Q type high-temperature vacuum brazing furnace. The heating method is in-furnace molybdenum strip radiation heating. The power supply is a thyristor low-voltage high-current AC power supply, industrial frequency AC, non-polar, and evacuated to 1×10⁻⁶. -2 Heating should be turned on when the pressure is below MPa.
8. The welding method for a CT tube housing window as described in claim 1, characterized in that, Both the welding fixture (2) and the heat-adjusting fixture (1) are made of a material that is resistant to high temperatures and does not wet the solder. The material is selected from one of graphite, boron nitride coated graphite, alumina ceramic, and molybdenum alloy.
9. A method for welding a CT tube housing window as described in claim 1, characterized in that, Also includes S5, S5. Post-welding inspection: The welded CT tube housing window assembly was subjected to helium leak testing and ultrasonic testing. The helium leak testing used a helium mass spectrometer to test the overall sealing of the welded CT tube housing window assembly. The ultrasonic testing used water immersion ultrasonic C-scan technology to perform non-destructive testing on the brazed joint of the welded CT tube housing window.