A method for brazing glass to metal and a brazed joint

By coating the glass and metal surfaces with gallium and utilizing the eutectic liquefaction effect of tin-based solder, the problem of glass-metal connection at low temperatures was solved, achieving high-strength and low-cost brazing results.

CN123103103APending Publication Date: 2026-11-17SUZHOU NUCLEAR POWER RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235771.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve highly reliable glass-metal connections at low temperatures, and traditional high-temperature brazing methods suffer from problems such as excessively high welding temperatures leading to glass cracking and high costs.

Method used

A combination of gallium coating and tin-based solder is used to achieve connection by pre-coating the glass and metal surfaces with gallium coating and brazing at low temperature, utilizing the eutectic liquefaction effect of gallium and tin-based solder.

Benefits of technology

Achieving high-strength, crack-free bonding between glass and metal at low temperatures reduces welding temperature and cost, while improving welding quality and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103103A_ABST
    Figure CN123103103A_ABST
Patent Text Reader

Abstract

This invention provides a method for brazing glass and metal, and a brazed joint, specifically relating to the field of welding technology. The brazing method includes: pretreating the surfaces of the glass substrate and the metal substrate to be brazed; preheating the pretreated glass and metal substrates to 25°C~40°C, and heating gallium to melt it into liquid gallium; coating the liquid gallium onto the surfaces of the glass and metal substrates to be brazed, and cooling to room temperature to form a gallium coating; aligning and assembling the glass substrate and metal substrate with the gallium coating, and placing tin-based solder between the surfaces to be brazed to form a brazed joint; and brazing the joint to be brazed, causing the tin-based solder to melt and interact with the gallium coating to achieve a brazed connection between the glass substrate and the metal substrate. This invention enables low-temperature, low-cost, and highly reliable connections between glass and metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of welding technology, and more particularly to a brazing method for glass and metal and a brazed joint. Background Technology

[0002] The joining of dissimilar materials, such as glass and metal, has broad application prospects in electronic packaging, optoelectronic devices, aerospace, and medical equipment. To achieve highly reliable connections between these materials, brazing technology is considered an effective method due to its relatively simple process and high connection strength. Glass-metal brazing utilizes liquid filler metal to wet the surfaces of both the glass and the metal substrate. Through the filling and solidification of the liquid filler metal, a metallurgically bonded joint is formed, thus achieving an effective connection between the two dissimilar materials.

[0003] Currently, the most common method for brazing glass to metal is high-temperature vacuum brazing. This method typically uses silver-copper (Ag-Cu) based brazing filler metal, which is heated in a vacuum environment above 600°C to melt the filler metal, thereby wetting the glass and metal surfaces and forming a joint. However, due to the strong chemical inertness of the glass surface, it is difficult to wet the surface, usually requiring pre-metallization treatment of the glass surface or activation modification of the Ag-Cu based brazing filler metal. Common metal layers for glass surface pre-metallization include Ag layers, Au layers, and Mn-Mo sintered layers. The preparation of pre-metallization layers is expensive, increasing the manufacturing cost of the glass-metal brazed joint. Activation modification of Ag-Cu based brazing filler metal usually involves adding active elements such as Ti and Cr. Although direct brazing of glass to metal can be achieved, the high welding temperature poses a risk of post-weld joint or glass substrate cracking.

[0004] Tin (Sn)-based brazing filler metals, due to their low melting point, can typically be used at welding temperatures below 300°C, making low-temperature brazing an effective way to address the aforementioned issues. However, under low-temperature brazing conditions, liquid Sn-based filler metals exhibit high surface tension and low chemical activity, making it difficult for them to directly penetrate the chemically inert surface of glass to achieve effective wetting and spreading. To address this problem, existing technologies have proposed ultrasonic-assisted low-temperature brazing methods, which involve applying ultrasonic vibrations to the liquid filler metal and utilizing the ultrasonic cavitation effect to break down the oxide film or adsorbed layer on the glass surface, thereby promoting wetting. However, this technology involves complex equipment, requires an additional ultrasonic energy field, and incurs high investment costs, making it unsuitable for large-scale application in conventional production environments.

[0005] Therefore, there is an urgent need to develop a brazing method that can achieve low-temperature, low-cost, and highly reliable connections between glass and metal. Summary of the Invention

[0006] In view of the shortcomings of the prior art, the present invention provides a brazing method and brazed joint for glass and metal, so as to improve the problems of difficult wetting of glass surface, difficult removal of oxide film on metal surface and high welding stress in the current glass and metal brazing process.

[0007] To achieve the above and other related objectives, the present invention provides a method for brazing glass and metal, the brazing method comprising the following steps: The surfaces of the glass substrate and the metal substrate to be brazed are pretreated separately. The pretreated glass substrate and the metal substrate are preheated to 25°C~40°C, and the metal gallium is heated to melt it into liquid gallium. The liquid gallium is then coated onto the brazing surfaces of the glass substrate and the metal substrate, respectively, and cooled to room temperature to form a gallium coating. A glass substrate with the gallium coating on its surface is aligned and assembled with a metal substrate, and a tin-based solder is placed between the glass substrate and the metal substrate to be brazed to form a brazed part to be processed. The workpiece to be brazed is subjected to brazing treatment, which melts the tin-based soft solder and interacts with the gallium coating to achieve a brazing connection between the glass substrate and the metal substrate.

[0008] In one embodiment of the present invention, the brazing process includes: heating the workpiece to be brazed to a brazing temperature 20°C to 30°C above the melting point of the tin-based solder, and applying pressure for heat preservation brazing, wherein the applied pressure is 0.01MPa-0.1MPa, the heat preservation time is 5 s to 300 s, and the workpiece is cooled to room temperature after the heat preservation is completed.

[0009] In one embodiment of the present invention, the thickness of the gallium coating is 1 μm to 10 μm.

[0010] In one embodiment of the present invention, the pretreatment includes: first, grinding the surfaces of the glass substrate and the metal substrate to be brazed, then cleaning the ground surfaces with alcohol, and finally drying them.

[0011] In one embodiment of the present invention, the polishing process includes sequentially polishing the surface of the glass substrate to be welded and the surface of the metal substrate to be brazed with 50-1000 grit sandpaper until the surface roughness reaches below 5 μm.

[0012] In one embodiment of the present invention, the gallium coating is applied by means of direct application with cotton cloth, application with a soldering iron, or rotary friction application.

[0013] In one embodiment of the present invention, the glass matrix includes any one of quartz glass, soda-lime glass, tempered glass, or sapphire.

[0014] In one embodiment of the present invention, the metal base material includes any one of copper, copper alloy, aluminum, aluminum alloy, titanium, titanium alloy, Invar alloy, or stainless steel.

[0015] In one embodiment of the present invention, the tin-based solder includes any one of tin-zinc alloy, tin-titanium alloy, tin-aluminum alloy, tin-magnesium alloy, tin-zinc-aluminum alloy, tin-silver-titanium alloy, tin-silver-aluminum alloy, or tin-silver-copper-titanium alloy.

[0016] In one embodiment of the present invention, the solder form of the tin-based soft solder includes any one of solder paste, solder foil, solder ring, solder wire, and solder powder.

[0017] The present invention also provides a glass-metal dissimilar brazing joint, wherein the brazing joint is formed by the above-described brazing method and comprises: a glass base material, a metal base material, and a tin-based soft solder layer sandwiched between the glass base material and the metal base material; both the brazing surface of the glass base material and the brazing surface of the metal base material are provided with a gallium coating.

[0018] The beneficial effects of this invention are as follows: This invention proposes a brazing method for glass and metal. In this method, a gallium coating is pre-coated on both the glass substrate and the metal substrate to be brazed. Then, tin-based solder is sandwiched between them to form a sandwich structure, and brazing is performed through low-temperature pressing. This method utilizes the transient liquid phase effect of eutectic liquefaction between gallium and tin-based solder at extremely low temperatures (20.5°C). At temperatures below the melting point of conventional tin-based solder, the tin-based solder can undergo a eutectic reaction with the interfacial gallium coating, achieving liquefaction, mutual dissolution, and sufficient interfacial diffusion. On the one hand, this significantly reduces the actual brazing temperature, shortens the brazing heat preservation and operation time, and effectively avoids performance degradation of the substrate due to accumulated welding heat. On the other hand, it ensures sufficient bonding and uniform diffusion at the welding interface, further improving the bonding strength and overall stability of the brazed joint.

[0019] This invention employs a gallium coating process to modify the glass and metal surfaces to be brazed before brazing. The gallium coating can effectively remove the oxide film on the metal surface to be brazed and purify the welding interface. At the same time, it can improve the wettability of the glass surface under normal temperature and low temperature conditions without additional energy field input such as ultrasound or heat source assistance, thereby solving the technical problem that traditional tin-based soft solders are difficult to directly wet glass substrates and realizing efficient low-temperature brazing of glass and metal.

[0020] This invention uses tin-based soft solder to achieve low-temperature brazing of glass and metal. Compared with the traditional high-temperature brazing process of Ag-Cu-based solder, the overall welding temperature is significantly reduced, which can effectively reduce the difference in thermal stress between the glass base material and the metal base material during the brazing process. It can also greatly avoid defects such as glass cracking, joint cracking, and thermal damage to the base material caused by high-temperature welding, and effectively improve the forming quality and structural reliability of the brazed joint.

[0021] This invention eliminates the expensive pre-metallization process of traditional glass surface Ag layer, Au layer, Mn-Mo sintering layer, etc., and does not require complex metallization preparation equipment and consumables. It simplifies the overall welding process, significantly reduces the processing and manufacturing cost of glass-metal dissimilar joints, and has stronger process adaptability and industrialization promotion. Attached Figure Description

[0022] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application. It is obvious that the drawings described below are merely some embodiments of this application, and those skilled in the art can obtain other drawings based on these drawings without any inventive effort.

[0023] In the attached diagram: Figure 1 This is a flowchart of a glass-to-metal brazing method provided in one embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of the glass substrate after a gallium coating is formed on the surface to be brazed, according to one embodiment of the present invention. Figure 3 This is a schematic diagram of the assembled brazing part to be processed provided in one embodiment of the present invention; Figure 4 This is a microstructure diagram of the quartz glass and aluminum alloy after brazing in Example 1 of the present invention; Figure 5 This is a microstructure diagram of the quartz glass and 4J36 after brazing in Example 2 of the present invention; Figure 6 The image shows the microstructure and quantitative analysis of the brazed joint location under a transmission electron microscope in Embodiment 1 of the present invention.

[0024] The attached figures are labeled as follows: 1. Glass substrate; 2. Metal substrate; 3. Gallium coating; 4. Tin-based solder. Detailed Implementation

[0025] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. Various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0026] It should be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of the present invention. The drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0028] The terms or phrases used in this article have the following meanings: In this article, the terms "multiple," "various," and "multiple times" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0029] In this document, terms such as “preferred,” “ideal,” “further,” “even more,” and “particularly” are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of this invention.

[0030] In this document, when referring to numerical ranges, unless otherwise specified, the distribution of selectable values ​​within a numerical range is considered continuous, including the two endpoints of the range (i.e., the minimum and maximum values), and every value between these two endpoints. When multiple numerical ranges are provided to describe a feature or property, these numerical ranges can be combined.

[0031] Glass-metal heterogeneous brazing joints are widely used in high-vacuum electronic devices, aerospace optical windows, semiconductor hermetic packaging, and precision joining of dissimilar materials. These applications typically require a strong, hermetic connection between an inorganic non-metallic glass substrate and a metallic substrate. However, the chemical inertness of the glass substrate surface and its three-dimensional network of silicon-oxygen bonds make it extremely difficult to wet with conventional low-melting-point tin-based brazing filler metals. Simultaneously, the metallic substrate surface generally possesses a dense and chemically stable natural oxide film, hindering direct atomic-level contact between the brazing filler metal and the metal matrix. While traditional high-temperature vacuum brazing can force a connection by adding active elements, the extremely high welding temperature (typically above 600 °C) causes catastrophic residual thermal stress during post-weld cooling due to the significant difference in the coefficients of thermal expansion (CTE), directly leading to brittle cracking of the glass substrate. Traditional low-temperature soldering, lacking sufficient interface activation energy, must rely on extremely complex ultrasonic energy fields or expensive pre-metallization coatings.

[0032] To address the shortcomings of the aforementioned related technologies, this application utilizes the physicochemical effect of eutectic liquefaction of liquid gallium metal with tin-based solder at low temperatures. Without the need for any external ultrasonic energy field or expensive pre-metallization layer, the dense oxide film on the metal surface is peeled off in situ and the glass surface is activated, thereby achieving a high-strength, crack-free, and firmly wetted bond between glass and metal heteromaterials at low temperatures.

[0033] Please see Figures 1 to 3 This invention provides a method for brazing glass and metal, the brazing method comprising the following steps: S1. The surfaces of the glass substrate 1 and the metal substrate 2 to be brazed are pretreated respectively. S2. Preheat the pretreated glass substrate 1 and metal substrate 2 to 25℃~40℃, and heat the metal gallium to melt it into liquid gallium. Coat the liquid gallium onto the brazing surfaces of the glass substrate 1 and the metal substrate 2 respectively, and cool it to room temperature to form gallium coating 3. S3. Align and assemble the glass base material 1 with gallium coating 3 on its surface and the metal base material 2, and place the tin-based soft solder 4 between the surfaces of the glass base material 1 and the metal base material 2 to be brazed to form the brazed part to be processed. S4. Perform brazing treatment on the workpiece to be brazed, so that the tin-based soft solder 4 melts and interacts with the gallium coating 3 to achieve brazing connection between the glass base material and the metal base material.

[0034] Specifically, step S1 is first performed to pre-treat the surfaces of the glass substrate 1 and the metal substrate 2 to be brazed.

[0035] In one specific embodiment of this application, the pretreatment process is carried out as follows: First, the surfaces to be brazed are polished: based on the initial flatness of the interface to be brazed, sandpaper with grits from coarse to fine is used to progressively polish the surfaces to be brazed of the glass substrate 1 and the metal substrate 2. Specifically, 50- to 1000-grit metallographic sandpaper is selected. During the polishing process, the polishing direction is kept consistent until the microscopic geometry of the surface to be brazed changes, resulting in a surface roughness of 5 μm or less.

[0036] After polishing, a cleaning and drying process is performed. Alcohol is used to remove residual polishing debris, adsorbed organic oil, and airborne impurities. Specifically, the polished glass substrate 1 and metal substrate 2 are immersed in an ultrasonic cleaning tank containing anhydrous ethanol as the cleaning medium. The ultrasonic cleaning equipment is turned on, and ultrasonic cleaning is performed at room temperature for, for example, 5 to 15 minutes. After ultrasonic cleaning, the substrates are removed, and their surfaces are rapidly dried using cold air or dry nitrogen. They are then placed in an oven for further drying, resulting in a pre-treated substrate with an extremely clean surface and a microscopic rough structure.

[0037] Next, step S2 is performed, where a liquid gallium coating 3 is applied to the surfaces of the glass substrate 1 and the metal substrate 2 to be brazed. See [link to previous step]. Figure 2 .

[0038] In one specific embodiment of this application, in order to construct a uniform and stable gallium coating 3 in situ on the surfaces of the glass substrate 1 and the metal substrate 2, a substrate preheating step is first performed. The pretreated glass substrate 1 and the metal substrate 2 are placed on a constant temperature heating platform and preheated to 25°C to 40°C, for example, 25°C, 30°C, 35°C, or 40°C. This preheating temperature ensures that the molten liquid gallium does not undergo rapid solidification and crystallization due to temperature drop upon contact with the substrate surface, thereby maintaining excellent fluidity and spreadability of the liquid gallium during the coating process.

[0039] After preheating, the gallium heating and melting and coating steps are performed. The gallium is heated using a heating device until it is completely melted into liquid gallium, and then the liquid gallium is uniformly coated onto the brazing surfaces of the glass substrate 1 and the metal substrate 2.

[0040] In some optional embodiments, the coating methods for liquid gallium include: direct application with cotton cloth, soldering iron application, or rotary friction coating. The direct application with cotton cloth involves uniformly applying high-purity liquid gallium onto a clean, soft cotton cloth, maintaining the temperature of the cloth and the substrate at 25°C to 40°C, and repeatedly wiping with slight and uniform pressure on the substrate surface. The micro-friction of the cotton fibers breaks down the surface tension of the liquid gallium, causing it to transfer and adhere evenly to the substrate surface. The soldering iron application method uses a copper tip on a soldering iron with a temperature controlled at 25°C to 40°C to directly apply a small amount of liquid gallium to the substrate surface, dragging and spreading it using the localized micro-heat and shearing force of the soldering iron tip. The rotary friction coating method involves fixing the substrate in the center of a rotating table, and dripping a small amount of liquid gallium onto the surface during rotation. The centrifugal force generated by the high-speed rotation and the friction of the scraper spread an extremely thin gallium coating 3 in situ on the substrate surface.

[0041] This invention overcomes the extremely high interfacial tension between liquid gallium and the non-metallic glass surface through the synergistic effect of the aforementioned preheating temperature and physical coating method. Under constant temperature conditions, physical friction force can forcibly break down the microscopic oxide layer on the liquid gallium surface, promoting the physical-chemical adsorption of liquid gallium atoms with oxygen atoms on the glass surface, forming a gallium coating 3 with extremely uniform thickness, continuity, and no breaks. This not only reduces the probability of interfacial defects caused by uneven coating, local accumulation, or local omissions, but also lays the technological foundation for a uniform low-temperature eutectic reaction with the tin-based solder layer 4 in subsequent steps.

[0042] After coating is completed, a cooling to room temperature step is performed. That is, after uniformly coating the liquid gallium metal onto the surfaces to be brazed on the glass substrate 1 and the metal substrate 2, the temperature of the substrate is reduced to room temperature.

[0043] In some optional embodiments, the thickness of the gallium coating 3 applied to the surfaces of the glass substrate 1 and the metal substrate 2 to be brazed is controlled between 1 μm and 10 μm. Specifically, it can be 1 μm, 5 μm, 8 μm, or 10 μm, etc. Gallium exhibits extremely strong grain boundary penetration at low temperatures, especially for metal substrates 2 such as aluminum alloys and copper alloys. Excessive liquid gallium will rapidly diffuse along the grain boundaries of the metal, disrupting the atomic bonds at the grain boundaries and inducing a liquid metal embrittlement effect, leading to a sharp decrease in the strength of the substrate. Limiting the thickness of the gallium coating 3 to between 1 μm and 10 μm can ensure perfect wetting and bonding at the interface while reducing the risk of grain boundary erosion and embrittlement of the substrate, thus significantly improving the mechanical properties of the joint.

[0044] Next, step S3 is performed: the glass substrate 1 with a gallium coating 3 on its surface is aligned and assembled with the metal substrate 2 with a gallium coating 3 on its surface, and the tin-based solder 4 is placed between the surfaces of the two substrates to be soldered, thus assembling them as follows. Figure 3The brazed component with a sandwich structure is shown. The brazed component is then placed in a dedicated brazing fixture and placed as a whole into a heating furnace or on a heating platform.

[0045] Finally, perform step S4, brazing: heat the workpiece to be brazed to a brazing temperature 20°C to 30°C above the melting point of the tin-based solder 4, and apply pressure for heat brazing. The applied pressure is 0.01MPa to 0.1MPa, and the holding time is 5 s to 300 s. After the heat holding time is completed, cool to room temperature. The brazing temperature can be 20°C, 25°C, or 30°C above the melting point of the tin-based solder, etc.; the applied pressure can be 0.01MPa, 0.05MPa, 0.08MPa, or 0.1MPa, etc.; and the holding time can be 5 s, 50 s, 100 s, 200 s, or 300 s, etc.

[0046] In some optional embodiments of this application, the glass base material 1 can specifically be any one of quartz glass, soda-lime glass, tempered glass, or sapphire. The metal base material 2 can specifically be any one of copper, copper alloy, aluminum, aluminum alloy, titanium, titanium alloy, Invar alloy, or stainless steel. The tin-based soft solder 4 can specifically be any one of tin-zinc (Sn-Zn) alloy, tin-titanium (Sn-Ti) alloy, tin-aluminum (Sn-Al) alloy, tin-magnesium (Sn-Mg) alloy, tin-zinc-aluminum (Sn-Zn-Al) alloy, tin-silver-titanium (Sn-Ag-Ti) alloy, tin-silver-aluminum (Sn-Ag-Al) alloy, or tin-silver-copper-titanium (Sn-Ag-Cu-Ti) alloy, and its physical form can be any one of solder paste, solder foil, solder ring, solder wire, or solder powder.

[0047] The aforementioned material system exhibits high chemical synergy and eutectic liquefaction response during low-temperature brazing. All the tin-based solders 4 listed above contain active alloying elements with extremely low eutectic temperatures to gallium. For example, the eutectic temperature of gallium with tin is 20.5℃, with zinc it is 15.3℃, and with aluminum it is 26.6℃. When heated, the double-sided pre-coated gallium layer 3 can undergo a multi-element eutectic reaction with the tin, zinc, and aluminum elements in these tin-based solders at extremely low temperatures, generating a highly active transient liquid phase. This liquid phase not only rapidly peels away the dense oxide film on the surface of the aluminum alloy, stainless steel, and other metal substrates 2, exposing fresh metal, but also significantly reduces the contact angle of the solder on the surface of the difficult-to-wet glass substrates 1, such as quartz glass and sapphire. By selecting different physical forms of brazing filler metal (such as using brazing foil for planar overlaps, brazing rings for complex annular joints, and solder paste or powder for filling micro-gap joints), it is possible to ensure that the brazing filler metal achieves perfect capillary flow and interface spreading at low temperatures. This allows for the construction of dense, crack-free, and highly bonded high-quality brazed joints between various heterogeneous material combinations that are extremely difficult to join.

[0048] The present invention also provides a glass-metal dissimilar brazing joint, which can be obtained by the above-described brazing method.

[0049] The aforementioned heterogeneous brazing joint comprises: a glass base material 1, a metal base material 2, and a tin-based soft solder 4 sandwiched between the glass base material 1 and the metal base material 2. The microstructure of both the glass base material 1 and the metal base material 2 is pre-coated with a gallium coating 3 with a thickness of 1 μm to 10 μm. After brazing, the gallium coating 3 partially dissolves into the solder as a trace element, but obvious traces of gallium coating 3 remain at the interface.

[0050] The heterogeneous brazed joint of this application introduces a gallium coating 3 with a thickness of 1 μm to 10 μm at both interfaces. During the brazing process, O, Sn, and Ga react at the glass-side interface to generate a composite oxide film. This composite oxide film is a highly dense and continuous thin film in space. Microscopically, it is formed by strong chemical bonds between gallium elements, tin elements in the brazing filler metal, and oxygen atoms on the surface of the glass substrate 1, thereby locking the glass substrate 1 and the tin-based soft solder 4 together at the atomic scale. Because the joint is formed by pressing at an extremely low brazing temperature (e.g., 200°C), the residual thermal stress inside the joint is greatly released. Scanning electron microscopy (SEM) observation confirms that there are no microscopic cracks, pores, or inclusions inside the joint or on the glass substrate 1 side, and the interfacial metallurgical bonding is extremely tight. Tests have shown that the joint's room temperature shear strength can stably reach 8.6 MPa to 11.2 MPa, exhibiting extremely high structural reliability and thermal cycling stability, and meeting the service requirements under extreme conditions such as high vacuum, high airtightness, and strong mechanical vibration.

[0051] The technical solutions of this application will be described in detail below through several specific embodiments and comparative examples. Unless otherwise stated, the raw materials and reagents used in the following embodiments are commercially available products or can be prepared by conventional methods in the art.

[0052] Example 1 This embodiment provides a brazing method for quartz glass and aluminum alloy, which is carried out according to the following steps: Step 1: Polish the surfaces of the quartz glass to be brazed and the aluminum alloy (specifically 6061 aluminum alloy) to be brazed with metallographic sandpaper ranging from 50 to 1000 grit, respectively, to achieve a surface roughness of 5μm. Then, place them in anhydrous ethanol for ultrasonic cleaning and dry them to obtain the pretreated base material.

[0053] Step 2: Place the pretreated quartz glass and aluminum alloy on a constant-temperature heating platform and preheat to 30°C. Heat the gallium metal to a molten state (approximately 35°C), and use a soft cotton cloth to apply the molten gallium evenly to the preheated surfaces of the quartz glass and aluminum alloy to be welded, controlling the thickness of the gallium coating to be 10μm. Then, cool to room temperature.

[0054] Step 3: Assemble the gallium-coated quartz glass, gallium-coated aluminum alloy, and Sn9Zn brazing foil into a sandwich structure for brazing. The brazing temperature is 200℃, the holding time is 60 seconds, and the assembly is air-cooled to room temperature after brazing. This completes the low-temperature brazing of the quartz glass and aluminum alloy.

[0055] The microstructure of the resulting brazed joint of quartz glass and aluminum alloy is as follows: Figure 4 As shown. By Figure 4 It can be seen that the interface between the brazing filler metal and the base metal on both sides is extremely tight, with no micro-cracks, pores or inclusions, and sufficient element diffusion and dissolution have occurred at the interface.

[0056] Tested with a universal tensile testing machine, the joint achieved a room temperature shear strength of 11.2 MPa, yielding an extremely reliable dissimilar brazed joint of quartz glass and aluminum alloy.

[0057] Example 2 This embodiment provides a brazing method for quartz glass and Invar alloy (4J36), which is carried out according to the following steps: Step 1: Polish the surfaces of the quartz glass and 4J36 metal to be brazed step by step with metallographic sandpaper ranging from 50 to 1000 grit to achieve a surface roughness of 5μm. Then, place them in anhydrous ethanol for ultrasonic cleaning and drying to obtain the pretreated base material.

[0058] Step 2: Place the pretreated quartz glass and 4J36 on a constant-temperature heating platform and preheat to 30°C. Heat the gallium metal to a molten state (approximately 35°C), and use a soft cotton cloth to apply the molten gallium evenly to the preheated quartz glass and aluminum alloy surfaces to be welded, controlling the thickness of the gallium coating to be 10μm. Then, cool to room temperature.

[0059] Step 3: Assemble gallium-coated quartz glass, gallium-coated 4J36 and Sn9Zn brazing foil into a sandwich structure for brazing. The brazing temperature is 200℃, the holding time is 60s, and after brazing, air cool to room temperature to complete the low-temperature brazing of the quartz glass and aluminum alloy.

[0060] The microstructure of the brazed joints of quartz glass and Invar alloy obtained are as follows: Figure 5 As shown. From Figure 5It can be seen that the interface between the brazing filler metal and the base metal on both sides is extremely tight, with no micro-cracks, pores or inclusions, and sufficient element diffusion and dissolution have occurred at the interface.

[0061] The joint was tested with a universal tensile testing machine and the room temperature shear strength reached 8.6 MPa, resulting in an extremely reliable quartz glass and 4J36 dissimilar brazed joint.

[0062] To systematically investigate the effect of gallium coating thickness on welding quality and joint mechanical properties, examples and comparative examples with different gallium coating thicknesses were designed, ensuring that other process conditions were exactly the same as in Example 1. The test results are shown in Table 1. Table 1: Effect of gallium coating thickness on brazing

[0063] Analysis of the experimental data in Table 1 shows that when the thickness of the gallium coating is controlled within the range of 1 μm to 10 μm (as in Examples 1, 3, and 4), the joints can achieve perfect, defect-free forming, and the room temperature shear strength remains stable at a high level of 10.0 MPa to 11.2 MPa. However, once the thickness of the gallium coating is less than 1 μm (as in Comparative Example 1, 0.5 μm), due to insufficient mass of active gallium elements, it is impossible to provide enough transient liquid phase at low temperatures to completely dissolve and peel off the oxide film on the metal surface. At the same time, it is also impossible to form a continuous active transition layer at the glass-side interface, resulting in large-area unbonded defects in the joint, and the shear strength drops directly to 0 MPa. Conversely, if the thickness of the gallium coating exceeds 10 μm (such as 12 μm in Comparative Example 2), the excess liquid gallium cannot be completely diluted and dissolved by the tin-based solder. The excess free gallium will severely penetrate into the grain boundaries of the metal substrate under the drive of gravity and heat, causing grain boundary erosion of the substrate. At the same time, a large number of coarse and brittle intermetallic compounds will be formed inside the weld, resulting in severe embrittlement of the weld. The shear strength of the joint deteriorates sharply to only 5.0 MPa, and the substrate is very prone to intergranular fracture when under stress.

[0064] To systematically investigate the effect of brazing holding time on the mechanical properties of the joint, under the premise that other process conditions are exactly the same as in Example 1, examples with different holding times were designed, and the shear strength of the joint under different examples was sampled and tested multiple times. The test results are shown in Table 2: Table 2: Effect of brazing holding time on joint shear strength

[0065] Analysis of the experimental data in Table 2 shows that when the holding time is only 10 s (as in Example 5), due to the short reaction time, the dissolution and diffusion between gallium and the tin-based solder layer have not yet reached equilibrium, and the active transition layer at the interface cannot be fully constructed, resulting in a low average shear strength of only 5.0 MPa. However, when the holding time is extended to 30 s (as in Example 6), the interface reaction becomes more complete, and the average shear strength of the joint significantly increases to 10.7 MPa. When the holding time is further optimized to 60 s (as in Example 1), perfect metallurgical bonding is achieved inside the joint, and the average shear strength reaches its maximum value of 11.2 MPa. If the holding time is too long, for example, greater than 300 s, it will not only reduce production efficiency but also cause excessive diffusion of gallium into the matrix, leading to grain boundary embrittlement. Therefore, limiting the holding time to between 30 s and 60 s can obtain a dense, high-strength, high-quality heterojunction in a very short time.

[0066] To further demonstrate the decisive and irreplaceable role of double-sided gallium coating and in-situ eutectic liquefaction of the gallium layer in achieving reliable glass-metal bonding, this application designed the following three sets of comparative examples, and conducted comparative experiments while ensuring that other process conditions were exactly the same as in Example 1: Comparative Example 3 The difference between this comparative example and Example 1 is that neither the glass side nor the metal side is coated with gallium, and Sn9Zn solder foil is directly sandwiched in and pressure-bonded at 200°C.

[0067] Experimental results show that at an ultra-low temperature of 200℃, the contact angle between the tin-zinc solder and the quartz glass is close to 180°, and the dense oxide film on the aluminum alloy surface cannot be removed. The solder rolls off completely in a spherical shape, and the two base materials cannot form any connection at all; the joint shear strength is 0 MPa. This proves that without gallium assistance, ultra-low temperature soldering cannot achieve direct wetting bonding between glass and metal.

[0068] Comparative Example 4 The difference between this comparative example and Example 1 is that only the quartz glass side is coated with an 8 μm gallium coating, while the aluminum alloy side is not coated with gallium. After assembly, the aluminum alloy side is subjected to pressure brazing at 200°C.

[0069] Experimental results show that although partial wetting was achieved at the glass side interface with the assistance of gallium, the dense oxide film on the aluminum alloy side could not be peeled off at a low temperature of 200℃ due to the lack of gallium coating. This resulted in large-area unbonded defects at the aluminum alloy side interface, and the joint completely peeled off from the aluminum alloy side under slight external force, failing to achieve effective shear strength. This proves that coating only one side of the glass with gallium cannot solve the problem of low-temperature film removal and metallurgical bonding on the metal side.

[0070] Comparative Example 5 The difference between this comparative example and Example 1 is that only the aluminum alloy side is coated with an 8μm gallium coating, while the quartz glass side is not coated with gallium. After assembly, the materials are pressure-bonded at 200°C.

[0071] Experimental results show that although the oxide film on the aluminum alloy side was successfully peeled off and well bonded under the eutectic liquefaction of gallium, the lack of gallium coating on the quartz glass side and the absence of ultra-low temperature thermodynamic driving force from active elements meant that the tin-zinc solder could not wet the quartz glass surface at all. The joint completely cracked after leaving the furnace, failing to form any connection. This demonstrates that coating only one side of the metal with gallium cannot solve the problem of low-temperature wetting and surface activation on the glass side.

[0072] In summary, only by coating both the glass and metal sides with an extremely thin gallium layer and utilizing the ultra-low temperature eutectic liquefaction and self-activation mechanism at the interface can the metallurgical bottlenecks of difficult wetting of the glass surface and difficult removal of the oxide film on the metal surface be solved simultaneously, thus obtaining a defect-free, high-strength, high-quality heterojunction.

[0073] The microscopic binding mechanism of this application can be achieved through... Figure 6 In-depth analysis was performed. After low-temperature pressure bonding brazing, the resulting heterojunction was sliced, polished, and then nanoscale thinned using a focused ion beam (FIB). Its interface microstructure was then observed under a high-resolution transmission electron microscope (TEM). Figure 6 As shown in (a), a nanoscale active transition layer exists between the glass substrate and the cured tin-based solder layer. To accurately investigate the elemental distribution of this transition layer, along... Figure 6 (a) Energy Dispersive Spectroscopy (EDS) elemental quantitative line scan analysis was performed on the cyan line scanning path (LG1) spanning the interface. The resulting elemental atomic percentage distribution curve is shown in Figure 1. Figure 6 As shown in (b).

[0074] Figure 6 The energy dispersive spectroscopy (EDS) curves in (b) clearly reveal the in-situ chemical activation and bonding mechanism of the glass surface at ultra-low temperatures. In the region with a scanning distance of 0.00 μm to 0.03 μm, the atomic percentages of oxygen and silicon are at extremely high levels, representing the quartz glass matrix side. In the region with a scanning distance of 0.03 μm to 0.13 μm, corresponding to the nanoscale transition reaction layer, the atomic percentage curves of gallium and zinc show extremely significant segregation enrichment peaks, while the content of tin is at a low level in this region. In the region with a scanning distance greater than 0.13 μm, tin rapidly increases and occupies an absolutely dominant position, representing the tin-based solder layer matrix side.

[0075] This microstructural feature confirms that during the brazing thermal cycle, the pre-coated gallium layer does not simply dissolve and dilute into the solder, but rather undergoes strong thermodynamic segregation and interaction with active elements (such as zinc) in the tin-based solder at the glass interface. Due to the extremely high chemical reactivity of both gallium and zinc, they react in situ at the interface, constructing a gallium- and zinc-rich nanoscale active transition layer. The gallium and zinc atoms in this transition layer can react strongly with oxygen atoms on the glass surface, forming strong gallium-oxygen and zinc-oxygen chemical bonds in situ. This nanoscale chemically bonded transition layer acts as a strong chemical link between the inorganic non-metallic glass and the metallic solder, thus achieving a direct, high-strength metallurgical bond between the glass and the solder without the need for any expensive pre-metallization layer.

[0076] The glass-to-metal brazing method provided by this invention involves pre-coating a gallium coating on both the glass substrate and the metal substrate to be brazed, then sandwiching tin-based solder into a sandwich structure, and finally brazing by low-temperature pressure bonding. This method utilizes the transient liquid phase effect of eutectic liquefaction between gallium and tin-based solder at extremely low temperatures. At temperatures below the melting point of conventional tin-based solder, the tin-based solder can undergo a eutectic reaction with the interfacial gallium coating, achieving liquefaction, mutual dissolution, and sufficient interfacial diffusion. This significantly reduces the actual brazing temperature, shortens the brazing heat treatment and operation time, and effectively avoids performance degradation of the substrate due to accumulated welding heat. Furthermore, it ensures sufficient bonding and uniform diffusion at the weld interface, further improving the bonding strength and overall stability of the brazed joint. Therefore, this invention effectively overcomes some practical problems in the prior art, thus possessing high utilization value and practical significance.

[0077] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for brazing glass to metal, characterized in that, Includes the following steps: The surfaces of the glass substrate and the metal substrate to be brazed are pretreated separately. The pretreated glass substrate and the metal substrate are preheated to 25°C~40°C, and the metal gallium is heated to melt it into liquid gallium. The liquid gallium is then coated onto the brazing surfaces of the glass substrate and the metal substrate, respectively, and cooled to room temperature to form a gallium coating. A glass substrate with the gallium coating on its surface is aligned and assembled with a metal substrate, and a tin-based solder is placed between the glass substrate and the metal substrate to be brazed to form a brazed part to be processed. The workpiece to be brazed is subjected to brazing treatment, which melts the tin-based soft solder and interacts with the gallium coating to achieve a brazing connection between the glass substrate and the metal substrate.

2. The brazing method according to claim 1, characterized in that, The brazing process includes: heating the workpiece to be brazed to a brazing temperature 20°C to 30°C above the melting point of the tin-based solder, and applying pressure for heat preservation brazing, wherein the applied pressure is 0.01MPa to 0.1MPa, the heat preservation time is 5 s to 300 s, and the workpiece is cooled to room temperature after the heat preservation is completed.

3. The brazing method according to claim 1, characterized in that, The thickness of the gallium coating is 1 μm to 10 μm.

4. The brazing method according to claim 1, characterized in that, The pretreatment includes: first, grinding the surfaces of the glass substrate and the metal substrate to be brazed, then cleaning the ground surfaces with alcohol, and finally drying them.

5. The brazing method according to claim 4, characterized in that, The polishing process includes sequentially polishing the surfaces of the glass substrate and the metal substrate to be brazed with 50-1000 grit sandpaper until the surface roughness reaches 5 μm or less.

6. The brazing method according to claim 1, characterized in that, The gallium coating can be applied by direct application with a cotton cloth, application with a soldering iron, or application by rotating friction.

7. The brazing method according to claim 1, characterized in that, The glass substrate includes any one of quartz glass, soda-lime glass, tempered glass, or sapphire; the metal substrate includes any one of copper, copper alloy, aluminum, aluminum alloy, titanium, titanium alloy, Invar alloy, or stainless steel.

8. The brazing method according to claim 1, characterized in that, The tin-based solder includes any one of tin-zinc alloy, tin-titanium alloy, tin-aluminum alloy, tin-magnesium alloy, tin-zinc-aluminum alloy, tin-silver-titanium alloy, tin-silver-aluminum alloy, or tin-silver-copper-titanium alloy.

9. The brazing method according to claim 1, characterized in that, The solder form of the tin-based soft solder includes any one of solder paste, solder foil, solder ring, solder wire, and solder powder.

10. A glass-metal dissimilar brazing joint, characterized in that, Formed by welding using any one of the brazing methods described in claims 1 to 9; The glass-metal heterogeneous brazing joint includes a glass base material, a metal base material, and a tin-based soft solder layer sandwiched between the glass base material and the metal base material; both the brazing surface of the glass base material and the brazing surface of the metal base material are provided with a gallium coating.