A low-temperature lead-free solder welding structure, its interface control method and application
By constructing a graphene interface control layer on the surface of a copper substrate, the problems of uncontrollable interface reaction and unstable solidification during the welding of low-temperature lead-free solder with a copper substrate are solved, achieving high reliability and uniformity of the solder joint, which is suitable for low-temperature packaging of flexible electronic devices.
Patent Information
- Application Number
- CN202611083529.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing low-temperature lead-free solders exhibit uncontrollable interfacial reactions, excessive growth of intermetallic compounds, unstable solidification processes, and poor wettability when soldered to copper substrates, making it difficult to meet the high-quality connection requirements of flexible electronic devices.
A graphene interface control layer is constructed on the surface of a copper substrate. A continuous and dense two-dimensional carbon atom layer is formed by chemical vapor deposition, transfer method or solution coating method to suppress Cu-Sn diffusion reaction and control the wetting, spreading and solidification behavior of solder.
It effectively inhibits the rapid growth of intermetallic compound layers, improves the mechanical reliability and microstructure consistency of solder joints, reduces the risk of brittle cracking, and is suitable for low-temperature packaging of flexible electronic devices.
Smart Images

Figure CN123103246A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the fields of electronic packaging, micro interconnects and advanced soldering materials, specifically to a low-temperature lead-free soldering structure, its interface control method and application. Background Technology
[0002] As electronic devices rapidly develop towards lightweight, miniaturized, flexible and highly integrated directions, traditional high-temperature welding processes are no longer able to meet the emerging packaging requirements. In applications, they often cause the following problems: (1) heat-sensitive chips, polymer flexible substrates and microstructures are damaged by heat; (2) thermal stress accumulation leads to interface cracking; (3) device warping, mismatch and residual stress are aggravated; (4) in multilayer stacked packaging, the previously completed welding structure suffers secondary thermal shock.
[0003] Therefore, low-temperature lead-free solders with low melting temperatures have become key materials for achieving the aforementioned packaging. Among them, Sn-Bi-based solders have attracted widespread attention due to their low melting point, low cost, and moderate process window. Taking Sn57Bi1Ag solder as an example, it maintains a low melting temperature while also possessing certain structural stability and joint strength, making it particularly suitable as a connection material for flexible electronic components.
[0004] Despite the thermodynamic temperature advantage of low-temperature solders such as Sn57Bi1Ag, they still face key technical bottlenecks in the following three aspects when soldering with copper or copper alloy substrates widely used in electronic packaging:
[0005] (1) Interfacial reactions are uncontrollable, and intermetallic compounds grow excessively. During the soldering process, Sn in the solder and Cu in the copper substrate rapidly diffuse into each other, quickly forming an intermetallic compound layer such as Cu6Sn5 at the interface. If this intermetallic compound layer continues to thicken, it will lead to interface embrittlement, decreased joint plasticity, and increased risk of failure due to cyclic bending and thermal cycling. In particular, it is more prone to crack initiation and propagation in flexible electronics, seriously threatening the mechanical reliability of flexible interconnect structures.
[0006] (2) The solidification process is unstable and the microstructure is inconsistent. The final microstructure of low-temperature solders is significantly affected by solidification behavior. When the nucleation temperature of the solder at the interface fluctuates greatly and the supercooling is unstable, it is easy to cause problems such as coarse solder joint structure, Bi-rich phase segregation, uneven distribution of Ag3Sn precipitates, and poor consistency of solder joint mechanical properties.
[0007] To suppress excessive Cu-Sn reactions, existing technologies often use Ni or CuNi alloy layers as diffusion barrier layers. However, experiments show that Sn57Bi1Ag exhibits poor wettability on CuNi substrates, failing to spread and resulting in spherical solder formation. This indicates that while traditional barrier layers effectively suppress diffusion, they often sacrifice the necessary wetting and spreading properties for low-temperature solders, making it difficult to meet the high-quality connection requirements of small solder joints, micro-pitch, and flexible interconnects.
[0008] In summary, existing low-temperature welding systems generally face a set of mutually restrictive contradictions: they need to suppress interfacial reactions but cannot significantly worsen wettability; they need to reduce the thickness of the intermetallic compound layer to improve joint plasticity but cannot weaken joint formation; they need to improve solidification stability but cannot increase process complexity; and they need to be adapted to flexible electronic packaging but cannot introduce high-temperature, high-cost, and brittle intermediate layers.
[0009] Currently available technical solutions mostly focus on localized optimization of single problems (such as focusing only on diffusion blocking or adjusting only the solder composition), and there is no effective strategy that can comprehensively control the interfacial reaction behavior, wetting and spreading characteristics, and solidification precipitation process at the same time. This technological gap seriously restricts the large-scale application of low-temperature lead-free solders in high-reliability packaging scenarios such as flexible electronics, wearable devices, and thermistors.
[0010] Therefore, it is of great significance to develop a novel interface control technology that can both suppress the interfacial reaction between low-temperature solder and copper substrate and maintain good wetting behavior and a stable solidification process. Summary of the Invention
[0011] The present invention aims to solve the problems in the prior art and provide a low-temperature lead-free solder welding structure, its interface control method and application.
[0012] To achieve the above objectives, the first aspect of this application provides a low-temperature lead-free solder welding structure, characterized in that it comprises: A substrate layer, wherein the substrate layer is a copper substrate or a copper alloy substrate; A graphene interface control layer is disposed on the surface of the substrate layer. A low-temperature lead-free solder layer is disposed on the side of the graphene interface control layer away from the substrate layer.
[0013] In the above-mentioned low-temperature lead-free solder welding structure, preferably, an intermetallic compound layer is formed at the interface between the low-temperature lead-free solder layer and the substrate layer, and the thickness of the intermetallic compound layer is not greater than 2.3 μm.
[0014] In the aforementioned low-temperature lead-free solder welding structure, preferably, the graphene interface control layer is a continuous and dense two-dimensional carbon atom layer, and the thickness of the graphene interface control layer is 0.34–3.40 nm.
[0015] In the above-mentioned low-temperature lead-free solder welding structure, preferably, the low-temperature lead-free solder layer is Sn-Bi-based lead-free solder.
[0016] In the aforementioned low-temperature lead-free solder welding structure, preferably, the Sn-Bi-based lead-free solder is at least one of Sn57Bi1Ag solder, Sn58Bi eutectic solder, Sn35Bi solder, Sn-Bi-Ag solder, Sn-Bi-In low-temperature solder, or Sn-Bi-based composite solder with trace rare earth elements or nano-reinforcing phases. All of the above solders use Sn as the main constituent element, and the main interfacial reaction during the welding process is the diffusion reaction between Sn and the Cu substrate to generate Cu6Sn5. The physical blocking mechanism of Cu-Sn diffusion by the graphene layer also applies to the above solder systems; therefore, the method and structure of the present invention are applicable to all of the above solders.
[0017] A second aspect of this application provides a method for regulating the interface reaction of low-temperature lead-free solder using graphene, comprising the following steps: (1) Provide a substrate layer, wherein the substrate layer is a copper substrate or a copper alloy substrate, and perform surface treatment on the substrate layer; (2) A graphene interface control layer is prepared on the surface of the substrate layer; (3) Place the low-temperature lead-free solder on the surface of the graphene interface control layer, perform reflow soldering, and then cool and solidify.
[0018] Preferably, in the above preparation method, the graphene interface control layer is formed by any one of the following methods: Graphene is directly grown on the surface of the substrate layer using chemical vapor deposition. The transfer method transfers the pre-fabricated graphene film onto the surface of the substrate layer; A solution coating method is used to construct a graphene coating on the surface of the substrate layer; The reduced graphene oxide method forms a continuous carbon layer of reduced graphene oxide on the surface of the substrate layer.
[0019] In the above preparation method, preferably, in step (2), the graphene interface control layer is directly grown by chemical vapor deposition, and the number of layers of the graphene interface control layer is 1 to 10, and the thickness is 0.34 to 3.40 nm; preferably 1 to 5 layers, more preferably 1 layer or 3 layers.
[0020] In the above preparation method, preferably, in step (3), the low-temperature lead-free solder is Sn57Bi1Ag solder, its liquidus temperature is 137℃, the peak temperature of the reflow soldering is 145℃~190℃, and the holding time is 30s~600s.
[0021] In the above preparation method, preferably, in step (3), the peak temperature of the reflow soldering is 145℃~175℃.
[0022] A third aspect of this application provides an application of the low-temperature lead-free solder welding structure or the method described above in electronic packaging, wherein the welding structure or method is used in at least one of the following scenarios: Low-temperature interconnection between flexible circuit boards and chips; Welding connection of wearable sensor electrodes; Lead connections for flexible display devices; Assembly of electronic devices on temperature-sensitive packaging materials; Low-damage assembly of medical-attach electronic devices; Welding and packaging of micro sensors and thin-film devices.
[0023] The inventive mechanism of this invention includes: 1. Two-dimensional dense barrier effect sp of graphene 2 The hybrid carbon atoms form a highly dense two-dimensional plane, which can significantly suppress the outward diffusion of Cu atoms and the inward diffusion of Sn atoms, thereby delaying the formation and growth of Cu6Sn5.
[0024] 2. Reduce the driving force of interface reaction The graphene layer partially isolates the solder from the highly reactive copper surface, weakening the violent reaction caused by direct contact and making the reaction more moderate and controllable.
[0025] 3. Alter heterogeneous nucleation behavior The structural characteristics and surface energy state of graphene surface alter the interfacial nucleation conditions during the solidification of liquid solder, thereby increasing the nucleation temperature and reducing the dispersion of supercooling.
[0026] 4. Reduce the risk of failure caused by the brittle layer. After the intermetallic compound layer (IMC layer) is thinned, the solder joints are less prone to brittle cracking during bending, impact and thermal cycling, making them more suitable for flexible electronic devices.
[0027] Compared with the prior art, this application has the following beneficial effects: (1) This invention constructs a graphene interface control layer on the surface of a copper substrate. Utilizing the dense two-dimensional lattice structure of graphene, an effective physical barrier is formed to prevent the diffusion of Cu atoms towards the solder side and Sn atoms towards the substrate side. As an atomic diffusion barrier, the graphene layer significantly reduces the Cu-Sn interface reaction rate, thereby inhibiting the rapid growth of intermetallic compound layers such as Cu6Sn5. Compared to the problems of interface embrittlement, decreased joint plasticity, and crack initiation and propagation under bending loads caused by excessively thick IMC layers in existing technologies, this invention achieves a thinner interface reaction layer, effectively reducing solder joint brittleness and improving the reliability of the joint under cyclic bending and thermal cycling conditions.
[0028] (2) In this invention, the graphene interface control layer changes the outermost interface state of the solder contact, which helps to control the wetting, spreading and local interface reaction kinetics of the molten solder, making the welding process more gentle and uniform.
[0029] (3) In this invention, the graphene interface control layer has a regulatory effect on the heterogeneous nucleation behavior during the solidification stage of the solder, which can increase or concentrate the nucleation temperature, reduce the dispersion of undercooling, and thus improve the consistency of the solder joint structure.
[0030] (4) This invention reduces the risk of solder joint cracking under bending, thermal cycling and mechanical loads by thinning the brittle IMC layer, mitigating interfacial reactions and stabilizing the solder joint structure. Compared with the limitations of existing technologies that are difficult to balance low temperature, low stress and high reliability, this invention is more suitable for applications with high requirements for bending reliability and thermal stability, such as flexible electronics, wearable devices and thermistors.
[0031] (5) The present invention does not require the introduction of a separate Ni / Au diffusion barrier layer and wetting layer. The graphene interface regulation layer can be directly constructed on the surface of the copper substrate to achieve the compatibility of interface reaction suppression and good wettability.
[0032] (6) The welding peak temperature of the present invention can be controlled in a lower heat input range, avoiding the thermal damage to heat-sensitive chips and polymer-based flexible substrates caused by traditional high-temperature welding, as well as the problems of interface cracking, device warping and secondary thermal shock caused by thermal stress accumulation, providing a feasible interconnection solution for low-temperature packaging of heat-sensitive components and flexible electronic devices. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0034] Figure 1 This is a microstructure image of the welded structure (Sn57Bi1Ag / Cu1) of a single-layer graphene copper substrate and Sn57Bi1Ag solder in Embodiment 1 of the present invention. Figure 2 This is a microstructure image of the welded structure (Sn57Bi1Ag / Cu3) of the three-layer graphene copper substrate and Sn57Bi1Ag solder in Embodiment 2 of the present invention. Figure 3 This is a microstructure image of the original copper substrate and Sn57Bi1Ag welded structure (Sn57Bi1Ag / original copper) in Comparative Example 1 of the present invention. Figure 4 This is a microstructure image of the annealed copper substrate and Sn57Bi1Ag welded structure (Sn57Bi1Ag / annealed copper) in Comparative Example 2 of the present invention. Figure 5 This is a microstructure image of the original copper substrate and Sn10Bi1Ag welded structure (Sn10Bi1Ag / original copper) in Comparative Example 3 of the present invention. Figure 6 This is a microstructure image of the annealed copper substrate and Sn10Bi1Ag welded structure (Sn10Bi1Ag / annealed copper) in Comparative Example 4 of the present invention. Figure 7 This is a microstructure image of the Sn10Bi1Ag / Cu3 welded structure of a single-layer graphene copper substrate in Embodiment 3 of the present invention. Figure 8 This is a microstructure image of the 3-layer graphene copper substrate and Sn10Bi1Ag welded structure (Sn10Bi1Ag / Cu1) in Embodiment 4 of the present invention. Figure 9 The solder joints of Sn57Bi1Ag on a 3-layer graphene CuNi substrate (a), a 1-layer graphene CuNi substrate (b), an annealed CuNi substrate (c), and a raw CuNi substrate (d) are shown in Comparative Example 5 of this invention. Figure 10 Comparison of solder joint interface morphology in Examples 1 and 2 and Comparative Examples 1 and 2 of the present invention: (a) (b) Sn57Bi1Ag / Cu3; (c) (d) Sn57Bi1Ag / Cu1; (e) (f) Sn57Bi1Ag / annealed copper; (g) (h) Sn57Bi1Ag / original copper; Figure 11 This is a comparison of the interface morphology of the solder joints in Comparative Examples 1 and 2 of the present invention; Figure 12This is a comparison of the surface morphology and Raman characterization of the original, annealed, and grown graphene copper substrates in Comparative Examples 1, 2, and 1 of the present invention. Figure 13 The morphology and Raman characterization of graphene films with different numbers of layers on a copper substrate according to the present invention. Detailed Implementation
[0035] To facilitate understanding of this application, the following description will be more comprehensive and detailed in conjunction with the accompanying drawings and preferred embodiments, but the scope of protection of this application is not limited to the following specific embodiments.
[0036] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of this application.
[0037] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0038] Example 1: Welding of a single-layer graphene copper substrate with Sn57Bi1Ag solder 1. Materials and Grouping: Single-layer graphene copper substrate samples were prepared as experimental groups, with three parallel samples in each group to ensure good repeatability and reliability of the experimental results.
[0039] The substrate material is a copper substrate (purity ≥ 99.9%, thickness 1 mm). The solder used is Sn57Bi1Ag lead-free solder (by mass percentage: 57% Bi, 1% Ag, balance Sn, liquidus temperature 137.3℃).
[0040] 2. Preparation of graphene layers The copper substrate was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 10 minutes each to remove surface oil and impurities, and then dried with nitrogen.
[0041] The cleaned copper plate was placed in the middle of the quartz liner and then placed in the middle of the tube furnace. First, 300 sccm of argon gas and 30 sccm of hydrogen gas were introduced and the pressure was adjusted to 1 atm. Then, the temperature was increased to 1050°C at a rate of 15°C / min. Subsequently, 0.5 sccm of methane was introduced and reacted at high temperature for 2 hours to grow graphene. After the reaction was completed, the methane was turned off and the temperature was reduced to room temperature at a rate of 30°C / min to obtain a single-layer graphene film with a thickness of 0.34 nm.
[0042] 3. Reflow soldering Sn57Bi1Ag solder was placed on the surface of a copper substrate covered with a single layer of graphene and subjected to low-temperature reflow soldering. The peak reflow temperature was set to 190℃, the holding time was 300s, and the solder was cooled to room temperature in air after soldering.
[0043] 4. Performance Testing Thermal analysis was performed using DSC under a nitrogen atmosphere. Starting at 50°C, the temperature was increased to 190°C at a rate of 10 K / min, held for 10 min, and then cooled to 50°C at 10 K / min. This cycle was repeated six times. For microstructure analysis, samples were cold-mounted, progressively polished with sandpaper, and then finely polished to a mirror finish using a SiO2 / OPS suspension polishing solution before carbon spraying. Backscattered electron microscopy (BSE-SEM) was used for imaging. Figure 1 (As shown) We conducted tissue observations and combined EDS to characterize the interface morphology and element distribution.
[0044] 5. Test Results There were no significant differences in the IMC thickness and DSC test results of the single-layer graphene samples, so the results are expressed as the group average.
[0045] (1) DSC results The results of the three parallel tests are as follows: Sample 1: Average nucleation temperature 133.07±0.55℃, average supercooling 4.23±0.55℃; Sample 2: Average nucleation temperature 132.19±0.52℃, average supercooling 4.62±0.52℃; Sample 3: Average nucleation temperature 132.35±0.42℃, average supercooling 4.94±0.42℃.
[0046] The supercooling fluctuation of the three samples was approximately ±0.49℃.
[0047] (2) Interface IMC thickness The area of the intermetallic compound layer at the interface was measured to be 114.3 µm. 2 The average thickness is 2.2 µm.
[0048] Example 2: Welding of a 3-layer graphene copper substrate with Sn57Bi1Ag solder 1. Materials and Grouping Three-layer graphene copper substrate samples were prepared as experimental groups, with three parallel samples in each group to ensure good repeatability and reliability of the experimental results. The substrate and solder materials were the same as in Example 1.
[0049] 2. Preparation of graphene layers The copper substrate was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 10 minutes each to remove surface oil and impurities, and then dried with nitrogen.
[0050] The cleaned copper plate was placed in the middle of the quartz liner and then placed in the middle of the tube furnace. First, 300 sccm of argon gas and 30 sccm of hydrogen gas were introduced and the pressure was adjusted to 1 atm. Then, the temperature was increased to 1050°C at a heating rate of 15°C / min. Subsequently, 1.5 sccm of methane was introduced and reacted at high temperature for 2 hours to grow graphene. After the reaction was completed, the methane was turned off and the temperature was reduced to room temperature at a cooling rate of 30°C / min to obtain a three-layer graphene film with a thickness of 1.02 nanometers.
[0051] 3. Reflow soldering The reflow soldering process was exactly the same as in Example 1 (peak temperature 190°C, holding time 300 s, cooling in air).
[0052] 4. Testing Methods Same as Example 1.
[0053] 5. Test Results The IMC thickness and DSC test results of the three-layer graphene samples are similar, so the average value of the group is used.
[0054] (1) DSC results The results of the three parallel tests are as follows: Sample 1: Average nucleation temperature 132.82±0.47℃, average supercooling 4.65±0.47℃; Sample 2: Average nucleation temperature 132.94±0.68℃, average supercooling 4.36±0.68℃; Sample 3: Average nucleation temperature 132.00±0.60℃, average supercooling 5.31±0.60℃.
[0055] The supercooling fluctuation of the three samples was approximately ±0.58℃.
[0056] (2) Interface IMC thickness The area of the intermetallic compound layer at the interface was measured to be 119.3 µm², and the average thickness was 2.3 µm.
[0057] SEM microscopy of tissues such as Figure 2As shown in the figure, the cross-sectional microstructure of Sn-57Bi-1Ag low-temperature lead-free solder after soldering to a 3-layer graphene copper substrate is displayed. The solder region consists of Sn phase, Bi phase, and Ag3Sn intermetallic compound, exhibiting typical eutectic / dendritic solidification characteristics. A continuous Cu6Sn5 intermetallic compound layer forms at the interface between the solder and the Cu substrate. This layer grows towards the solder side in a scalloped or blocky shape, indicating that Sn and Cu undergo interdiffusion reaction and form a metallurgical bond during the soldering process. The formation of Cu6Sn5 at the interface indicates that the Sn-Bi-Ag / Cu system has a strong tendency for interfacial reaction. If the reaction layer coarsens further, it may lead to interface embrittlement and reduce the long-term service reliability of the solder joint.
[0058] Comparative Example 1: Direct soldering of original copper substrate / Sn57Bi1Ag 1. Materials Substrate: The original copper substrate is the same as in Example 1; Solder: Sn57Bi1Ag lead-free solder, same as in Example 1.
[0059] 2. Method After cleaning the original copper substrate using the same process as in Example 1, without introducing a graphene layer, Sn57Bi1Ag solder was directly placed for reflow soldering, and the soldering parameters were kept consistent with those in Example 1.
[0060] 3. Results Microscopic morphology of the tissue as shown Figure 3 As shown, the area of the intermetallic compound layer at the interface was measured to be 175.5 µm. 2 The average thickness is 3.4 µm, and the solder solidification undercooling fluctuates significantly (undercooling fluctuation range > ±1.5℃), resulting in poor solder joint microstructure consistency. The figure shows that after Sn-Bi-Ag solder is welded to the Cu substrate, a typical Sn / Bi eutectic structure is formed, with lamellar and network phase distributions within the solder. A continuous Cu6Sn5 intermetallic compound reaction layer is formed at the interface, exhibiting obvious scalloped or blocky growth characteristics. Locally coarse lath-like phases and interface undulations indicate that the interface reaction in this system is relatively complete, and the Cu6Sn5 intermetallic compound shows a tendency for local coarsening, which may adversely affect the reliability of the solder joint interface. Therefore, without the introduction of graphene, the interface reaction between the copper substrate and Sn57Bi1Ag solder is relatively intense, easily forming a thick, brittle reaction layer, and the solidification behavior is unstable, making it difficult to meet the requirements of high-quality interconnection.
[0061] Comparative Example 2: Annealed copper substrate / Sn57Bi1Ag soldering 1. Materials Substrate: The original copper substrate is the same as in Example 1; Solder: Sn57Bi1Ag lead-free solder, same as in Example 1.
[0062] 2. Method The copper substrate was annealed under a protective atmosphere using the same process parameters as in Example 1, but without the introduction of methane gas. First, the cleaned copper plate was placed in the center of a quartz liner and then placed together in the center of a tube furnace. 300 sccm of argon gas + 30 sccm of hydrogen gas was introduced, and the pressure was adjusted to 1 atm. The temperature was then increased to 1050°C at a rate of 15°C / min, and held at this high temperature for 2 hours. The temperature was then reduced to room temperature at a rate of 30°C / min. No methane was introduced throughout the process; only the copper plate underwent annealing under the same conditions. Sn57Bi1Ag solder was then directly applied for reflow soldering, with the soldering parameters remaining consistent with Example 1.
[0063] 3. Results The microstructure of the weld structure after reflow soldering with Sn57Bi1Ag solder directly placed on an annealed copper substrate is shown in the figure below. Figure 4 As shown, the area of the intermetallic compound layer at the interface was measured to be 143.862 µm², with an average thickness of 2.8 µm. Although this thickness is lower than that of Comparative Example 1 (3.4 µm), it is still greater than that of the samples in Example 1 (2.2 µm) and Example 2 (2.3 µm) with graphene layers.
[0064] It can be seen that annealing can improve the interface state and reduce the IMC thickness to a certain extent, but it still cannot achieve the suppression effect of the graphene interface control layer.
[0065] Comparison of the weld joint interface morphology in Embodiments 1 and 2 and Comparative Examples 1 and 2 of the present invention Figure 10 and Figure 11 As shown in the figure, the cross-sectional microstructure of Sn-Bi-Ag low-temperature lead-free solder after soldering to a copper substrate under different treatment conditions is displayed. A continuous or semi-continuous interfacial reaction layer was formed between the solder layer and the copper substrate, indicating that an interdiffusion reaction between Sn and Cu occurred during the soldering process, and Cu-Sn intermetallic compounds were formed at the interface. The interfacial reaction layer exhibited varying degrees of undulation, scalloped, or blocky growth characteristics, indicating that different substrate surface conditions or interfacial control layers have a significant impact on the interfacial reaction. Black circular defects or local discontinuous areas were observed in some samples, which may be related to pores, oxide inclusions, uneven solder wetting, or sample detachment during cross-section preparation. Overall, the thickness, continuity, and coarsening degree of the interfacial reaction layer can serve as important criteria for evaluating the strength of the solder / copper substrate interfacial reaction and the reliability of the joint.
[0066] Figure 13 The images show the morphology and Raman characterization results of graphene films with different numbers of layers on a copper substrate. Figure 13It can be seen that by adjusting the graphene growth parameters, the thickness of graphene films can be controlled from single-layer to multi-layer. As the thickness of the graphene film increases, the contrast of graphene crystal domains becomes more obvious. At the same time, the ratio of the Raman characteristic peak G / 2D gradually changes from less than 1 to greater than 2, which is consistent with the Raman evolution trend of graphene films from single-layer to multi-layer.
[0067] Figure 12 The figures show the surface morphology and Raman characterization results of the original, annealed, and graphene-grown copper substrates in Comparative Examples 1, 2, and 1 of this invention. As can be seen from the figures, the original and annealed copper substrates have no graphene film on their surfaces, while the Raman spectrum of the graphene-grown copper substrate clearly detects graphene characteristic peaks.
[0068] In summary, it can be seen that a single-layer (0.34 nm) graphene can effectively balance diffusion blocking and solidification stabilization—the IMC layer thickness is significantly lower than that of the uncoated control group, and the supercooling dispersion is small, making it the preferred structural option. The three-layer (1.02 nm) graphene also exhibits significant interface control capability, with a significantly lower IMC thickness than the uncoated control group. However, in terms of solidification stability (supercooling fluctuation ±0.58℃), it is slightly inferior to the 0.34 nm thick graphene sample (±0.49℃), indicating that graphene thickness has a non-monotonic effect on solidification behavior.
[0069] As the thickness of graphene increases, the diffusion barrier effect still exists. However, excessively thick graphene or graphene with too many layers may alter the interfacial energy state and heat transfer conditions, thereby slightly reducing the stability of solder nucleation behavior. Considering both suppressing IMC and stabilizing solidification, a graphene thickness of 0.34 nm is the preferred range.
[0070] Comparative Example 3: Welding structure of the original copper substrate and Sn10Bi1Ag solder This comparative example illustrates the interface structure formed when Sn10Bi1Ag solder is directly soldered to the original copper substrate without a graphene interface control layer.
[0071] This comparative example uses a pristine copper substrate as the substrate material and Sn10Bi1Ag solder as the low-temperature lead-free solder. The copper substrate was ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and deionized water, and then dried with nitrogen. After cleaning, instead of preparing a graphene interface control layer on the copper substrate surface, the Sn10Bi1Ag solder was directly placed on the copper substrate surface for reflow soldering (peak temperature 260℃, holding time 300 s, followed by cooling to room temperature in air). After soldering, the solder joint cross-section was ground, polished, and its microstructure was observed.
[0072] Organizational morphology such as Figure 5As shown in the figure, the low-magnification and high-magnification interface morphologies corresponding to the Cu group reveal that after the Sn10Bi1Ag solder comes into direct contact with the original copper substrate, a distinct intermetallic compound layer forms at the interface. This reaction layer grows towards the solder side in a serrated or scalloped shape, and coarse columnar or blocky reaction products can be observed in local areas, indicating a strong interdiffusion reaction between Sn and Cu.
[0073] These results indicate that without a graphene interface control layer, the Cu-Sn interface reaction between the Sn10Bi1Ag solder and the copper substrate is quite intense, easily forming a thick and uneven intermetallic compound layer. This type of coarse interface reaction layer can easily lead to interface embrittlement during service and may become a site for crack initiation and propagation.
[0074] Compared to the uncontrolled interface in Example 1, the introduction of the graphene interface control layer resulted in a more refined and uniform morphology of the reaction layer at the solder / copper substrate interface, suppressing the localized coarsening of Cu-Sn intermetallic compounds. This indicates that the graphene layer can act as a diffusion barrier between the solder and the copper substrate, slowing down the interdiffusion process of Cu and Sn, thereby reducing the risk of excessive growth of interfacial IMC and improving the interface stability and service reliability of low-temperature solder joints.
[0075] Comparative Example 4: Welding structure of annealed copper substrate and Sn10Bi1Ag solder This comparative example illustrates the effect of copper substrate annealing alone, without the addition of a graphene interface control layer, on the Sn10Bi1Ag / Cu welding interface reaction.
[0076] This comparative example uses an annealed copper substrate as the substrate material and Sn10Bi1Ag solder as the low-temperature lead-free solder. After surface cleaning, the copper substrate is placed in a tube furnace and annealed under an argon and hydrogen protective atmosphere. No methane gas is introduced during annealing, thus preventing the formation of a graphene layer on the copper substrate surface. After annealing, Sn10Bi1Ag solder is applied to the annealed copper substrate surface for reflow soldering, with soldering parameters consistent with Comparative Example 3.
[0077] like Figure 6 As shown in the figure, the interface morphology corresponding to the annealed Cu group indicates that after the annealed copper substrate is soldered with Sn10Bi1Ag solder, a distinct Cu-Sn intermetallic compound layer is still formed at the interface. Compared with the original copper substrate, the annealing treatment improves the surface condition of the copper substrate to some extent, causing some changes in the morphology of the interface reaction layer. However, relatively obvious scallop-shaped or blocky reaction products can still be observed at the interface.
[0078] These results indicate that while annealing can alter the surface state and grain structure of the copper substrate, it cannot form an effective two-dimensional diffusion barrier layer and therefore cannot fundamentally suppress the interdiffusion between Sn and Cu. Thus, annealing the copper substrate alone is insufficient to effectively control the Cu-Sn interface reaction.
[0079] Example 3: Welding structure of a single-layer graphene copper substrate and Sn10Bi1Ag solder This embodiment illustrates the effect of setting a graphene interface control layer on the Sn10Bi1Ag solder / Cu welding interface reaction and solder structure on the surface of a copper substrate.
[0080] In this embodiment, a single-layer graphene copper substrate is used as the substrate material, wherein the graphene layer is a continuous or nearly continuous two-dimensional carbon atom layer. After cleaning the copper substrate with acetone, anhydrous ethanol, and deionized water, a single-layer graphene layer is prepared on the surface of the copper substrate using chemical vapor deposition. Subsequently, Sn10Bi1Ag solder is placed on the surface of the single-layer graphene copper substrate for reflow soldering, and the soldering parameters are consistent with those of Comparative Example 3.
[0081] Depend on Figure 7 The low- and high-magnification microstructures of the welded structure of a copper substrate with a single graphene layer and Sn10Bi1Ag solder show that, after adding a single graphene interface control layer, necessary interfacial connections can still be formed at the interface between the solder and the copper substrate, but the morphology of the intermetallic compound layer at the interface is significantly suppressed. Compared with the original copper substrate and the annealed copper substrate, the interfacial reaction layer in this structure is thinner overall, the degree of local coarsening is reduced, and the interface undulations are decreased.
[0082] High-magnification images reveal Ag3Sn precipitates within the solder, and typical Cu-Sn reaction products such as Cu6Sn5 and Cu3Sn at the interface. However, their growth is limited by the graphene interface control layer. The graphene layer forms an atomic-scale diffusion barrier between the copper substrate and the solder, thereby slowing the diffusion of Cu atoms towards the solder side and Sn atoms towards the copper substrate side, and suppressing the excessive formation and coarsening of Cu6Sn5 and Cu3Sn.
[0083] These results demonstrate that a single-layer graphene interface control layer can effectively mitigate the interfacial reaction between Sn10Bi1Ag solder and the copper substrate without completely blocking the weld metallurgical connection, resulting in a finer and more controllable intermetallic compound layer. This structure helps reduce the risk of interface embrittlement and improves the interfacial reliability of low-temperature solder joints.
[0084] Example 4: Welding structure of a 3-layer graphene copper substrate with Sn10Bi1Ag solder This embodiment illustrates the effect of setting three graphene interface control layers on the Sn10Bi1Ag solder / Cu welding interface reaction on the surface of a copper substrate.
[0085] In this embodiment, a three-layer graphene copper substrate is used as the substrate material. After cleaning, a three-layer graphene interface control layer is prepared on the surface of the copper substrate by chemical vapor deposition. Subsequently, Sn10Bi1Ag solder is placed on the surface of the three-layer graphene copper substrate for reflow soldering, and the soldering parameters are consistent with those of Comparative Example 3.
[0086] Depend on Figure 8 The interfacial microstructure of the weld structure between a three-layer graphene copper substrate and Sn10Bi1Ag solder shows that when the number of graphene layers increases to three, the interfacial reaction between the solder and the copper substrate is also significantly suppressed. The intermetallic compound layer at the interface still exists, but its overall thickness and local coarsening degree are lower than those of the copper substrate without graphene. This result indicates that the three-layer graphene can still play a diffusion-blocking role and has a regulatory effect on the Cu-Sn interfacial reaction.
[0087] Meanwhile, due to the increase in the number of graphene layers, the interfacial energy state, heat transfer conditions, and local wetting behavior may change. Therefore, the interfacial morphology of the 3-layer graphene copper substrate sample differs somewhat from that of the 1-layer graphene copper substrate sample. Compared with 1-layer graphene, although 3-layer graphene still has the effect of inhibiting the Cu-Sn reaction, its interface regulation effect may not continuously increase with the increase of the number of layers. Too many layers of graphene may change the heterogeneous nucleation conditions during solder solidification, causing certain fluctuations in the stability of the solder joint structure.
[0088] These results indicate that the number of graphene layers has a significant impact on the interfacial reaction of Sn10Bi1Ag / Cu welding. Both one and three graphene layers can significantly improve the interfacial reaction behavior, with one graphene layer being more beneficial in balancing diffusion blocking, interfacial bonding, and solidification structure stability, and thus can be considered as the preferred range for the number of graphene layers.
[0089] Comparative Example 5: Comparative Verification of the Replacement CuNi Barrier Layer 1. Background When traditional CuNi substrates (Cu-Ni alloys) are used as diffusion barrier layers, Sn57Bi1Ag solder has poor wettability, and the solder forms spherical shapes on the substrate surface without spreading, making it impossible to form effective solder joints.
[0090] 2. First, copper-nickel substrate samples (mass percentage: 58.73% Cu, 40.05% Ni) were prepared. After being cleaned with acetone, anhydrous ethanol, and deionized water, the copper-nickel substrates were divided into four groups for different treatments: Original CuNi substrate: The cleaned copper-nickel substrate was used directly as a control group without any additional treatment.
[0091] Annealing CuNi substrate: The cleaned copper-nickel substrate was placed in a tube furnace and annealed under an Ar / H2 mixed atmosphere. The annealing process was the same as in Comparative Example 2.
[0092] Single-layer graphene CuNi substrate: Graphene was prepared on the surface of a cleaned copper-nickel substrate using chemical vapor deposition (CVD). With other growth conditions remaining consistent with Example 1, the methane flow rate was increased to 2 sccm, and a single-layer graphene film was obtained after 2 hours of growth.
[0093] Three-layer graphene CuNi substrate: Graphene was prepared on the surface of a cleaned copper-nickel substrate using chemical vapor deposition (CVD). While maintaining the same growth conditions as in Example 1, the methane flow rate was increased to 3 sccm, and growth was carried out at the specified temperature for 2 hours to obtain a CuNi substrate covered with a three-layer graphene film.
[0094] Subsequently, Sn57Bi1Ag solder was placed on the surfaces of the four substrates mentioned above for reflow soldering, with the reflow soldering parameters remaining consistent with those in Example 1.
[0095] 3. Experimental Results Figure 9 The figures show the solder joints of Sn57Bi1Ag on single-layer graphene CuNi substrates, three-layer graphene CuNi substrates, annealed CuNi substrates, and pristine CuNi substrates. As can be seen, Sn57Bi1Ag exhibits poor wettability on single-layer, three-layer graphene CuNi substrates, and pristine CuNi substrates, failing to spread and exhibiting a spherical solder structure. While some spreading is achieved on annealed CuNi substrates, the wetting effect is still far inferior to that on pure copper substrates. The graphene layer on the copper substrate also inhibits interfacial reactions, but unlike the CuNi barrier layer, it does not significantly worsen the spreading behavior of the Sn57Bi1Ag solder. On graphene-covered copper substrates, the solder spreads normally and forms good solder joints, meeting the requirements for micro-solder joints and narrow-pitch interconnects.
[0096] This demonstrates the feasibility of this invention in replacing traditional Ni-based barrier layers in industrial applications, and avoids the complex process of requiring an additional Au layer electroplating to ensure wettability of Ni-based barrier layers.
Claims
1. A low-temperature lead-free solder welding structure, characterized in that, include: A substrate layer, wherein the substrate layer is a copper substrate or a copper alloy substrate; A graphene interface control layer is disposed on the surface of the substrate layer. A low-temperature lead-free solder layer is disposed on the side of the graphene interface control layer away from the substrate layer.
2. The low-temperature lead-free solder welding structure according to claim 1, characterized in that, An intermetallic compound layer is formed at the interface between the low-temperature lead-free solder layer and the substrate layer, and the thickness of the intermetallic compound layer is not greater than 2.3 μm.
3. The low-temperature lead-free solder welding structure according to claim 1, characterized in that, The graphene interface control layer is a continuous and dense two-dimensional carbon atom layer; the thickness of the graphene interface control layer is 0.34–3.40 nm.
4. The low-temperature lead-free solder welding structure according to claim 1, characterized in that, The low-temperature lead-free solder layer is Sn-Bi-based lead-free solder.
5. The low-temperature lead-free solder welding structure according to claim 4, characterized in that, The Sn-Bi-based lead-free solder is at least one of Sn57Bi1Ag solder, Sn58Bi eutectic solder, Sn35Bi solder, Sn-10Bi-1Ag solder, Sn-Bi-In low-temperature solder, and Sn-Bi-based composite solder with trace rare earth elements or nano-reinforced phases.
6. A method for regulating the interfacial reaction of low-temperature lead-free solder using graphene, characterized in that, Includes the following steps: (1) Provide a substrate layer, wherein the substrate layer is a copper substrate or a copper alloy substrate, and perform surface treatment on the substrate layer; (2) A graphene interface control layer is prepared on the surface of the substrate layer; (3) Place the low-temperature lead-free solder on the surface of the graphene interface control layer, perform reflow soldering, and then cool and solidify.
7. The preparation method according to claim 6, characterized in that, The graphene interface control layer is formed by any of the following methods: Graphene is directly grown on the surface of the substrate layer using chemical vapor deposition. The transfer method transfers the pre-fabricated graphene film onto the surface of the substrate layer; A solution coating method is used to construct a graphene coating on the surface of the substrate layer; The reduced graphene oxide method forms a continuous carbon layer of reduced graphene oxide on the surface of the substrate layer.
8. The preparation method according to claim 6, characterized in that, In step (2), the graphene interface control layer is directly grown by chemical vapor deposition. The number of layers in the graphene interface control layer is 1 to 10, and the thickness is 0.34 to 3.40 nm.
9. The preparation method according to claim 6, characterized in that, In step (3), the low-temperature lead-free solder is Sn57Bi1Ag solder, its liquidus temperature is 137℃, the peak temperature of the reflow soldering is 145℃~190℃, and the holding time is 30s~600s.
10. The application of a low-temperature lead-free solder welding structure as described in any one of claims 1 to 5 or the method as described in any one of claims 6 to 9 in electronic packaging, characterized in that, The welding structure or method is used in at least one of the following scenarios: Low-temperature interconnection between flexible circuit boards and chips; Welding connection of wearable sensor electrodes; Lead connections for flexible display devices; Assembly of electronic devices on temperature-sensitive packaging materials; Low-damage assembly of medical surface-mount electronic devices; Welding and packaging of micro sensors and thin-film devices.