A method for recovering niobium ingot chips based on molten salt purification
By treating niobium ingot chips using a molten salt purification method, the problems of low recovery rate and environmental pollution of niobium ingot chips in existing technologies have been solved. This method achieves high-purity and high-recovery-rate niobium ingot chip recovery and is suitable for the production of high-purity niobium materials for aerospace and electronics.
Patent Information
- Application Number
- CN202611446332.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for recycling niobium ingot chips do not completely remove oil and impurities from the chip surface, resulting in low niobium recovery rates. Furthermore, the process generates high-COD wastewater, which fails to meet the standards for high-purity niobium materials used in aerospace and electronics.
The molten salt purification method removes surface metal impurities and oil by screening and treating niobium ingot chips in molten salt. The chips are then pressed and vacuum sintered, avoiding aqueous solution cleaning and electron beam melting. The molten salt complexation reaction and electrolytic regeneration process are used to achieve the purification and densification of niobium ingot chips.
It significantly improves the recovery rate of niobium to 96.5% and the purity to 99.35%, reduces energy consumption and waste treatment costs, and is suitable for continuous production of high-purity niobium materials for aerospace and electronics.
Smart Images

Figure CN123108577A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of niobium recycling technology, and specifically to a method for recycling niobium ingot chips based on molten salt purification. Background Technology
[0002] During the machining of niobium ingots (such as turning and milling), a large amount of chips are generated, which usually account for 10%-30% of the total mass of the raw material. Since the surface of the chips is covered with oil, coolant and processing impurities (such as iron, aluminum and other metal fragments), directly discarding them not only causes a serious waste of niobium resources, but also pollutes the environment.
[0003] Existing methods for recovering niobium ingot chips mostly involve simple cleaning followed by direct smelting. This fails to completely remove oil and oxide films from the chip surface, resulting in slabs with excessive levels of oxygen, iron, and aluminum impurities, which cannot meet the standards for high-purity niobium materials used in aerospace and electronics. Furthermore, the chips are loose and easily oxidized and burned during smelting, resulting in a recovery rate typically below 85%. Some other methods exist, such as the one disclosed in CN121046659A, which involves classifying and screening the niobium ingot chips before performing degreasing, cleaning, drying, pressing, and vacuum smelting. Pressing and vacuum smelting address the issues of loose chips and oxidation. However, water-based cleaning generates large amounts of high-COD, waste acid, and waste alkali; finer chips are easily lost during the washing process, leading to a low niobium recovery rate. Summary of the Invention
[0004] The purpose of this invention is to completely avoid the aqueous solution acid-base cleaning and electron beam liquid phase melting processes, and to directly prepare malleable and dense niobium billets using a short-process solid phase method, thereby improving the niobium recovery rate and reducing energy consumption.
[0005] To achieve the above-mentioned technical objectives, this invention provides a method for recovering niobium ingot chips based on molten salt purification, comprising: Niobium ingot chips are immersed in molten salt to remove metallic impurities and oil from the surface of the chips, resulting in clean niobium chips.
[0006] Furthermore, the niobium ingot chips are sieved into ultrafine chips with a particle size of <1mm, medium chips with a particle size of 1-3mm, and coarse chips with a particle size of ≥3mm before being mixed with molten salt. The treatment times for the ultrafine chips, the medium chips, and the coarse chips in the molten salt are 15-20 min, 20-30 min, and 35-40 min, respectively.
[0007] Furthermore, the molten salt is obtained by mixing at least two alkali metal chloride salts; The treatment is carried out at a temperature of 350-450°C.
[0008] Furthermore, after obtaining clean niobium chips, they are pressed and vacuum sintered.
[0009] Further, the compression molding process includes loading clean niobium chips into a mold at 280-320°C, applying a molding pressure of 180-280 MPa, holding the pressure for 3-6 minutes, and then demolding the mold after cooling it to below 100°C to obtain a density ≥7.0 g / cm³. 3 The blank.
[0010] Furthermore, the vacuum sintering is performed at a vacuum degree <5×10⁻⁶. -2 Two segments are performed under Pa; The first stage of sintering is carried out at a temperature of 550-650℃ for 1-3 hours; the second stage of sintering is carried out at 1500-1700℃ for 40-90 minutes, during which an intermittent pulse current is applied, with a pulse conduction time of 10-30ms and an interval time of 60-100ms.
[0011] Furthermore, during the process of immersing niobium ingot chips in molten salt, the generated gas is collected and condensed for recovery.
[0012] Furthermore, obtaining clean niobium chips includes purging the niobium ingot chips after molten salt treatment with a non-oxidizing gas to remove the molten salt and other impurities adhering to their surface.
[0013] Furthermore, the molten salt electrolysis process after processing niobium ingot chips will remove dissolved metal impurities, and the molten salt will be regenerated and processed with the next batch of niobium ingot chips.
[0014] Furthermore, the electrolytic treatment is carried out at a temperature of 350-450℃ and a voltage of 2.2-2.8V.
[0015] Compared with the prior art, the beneficial effects of the present invention include: 1. The niobium ingot chip recycling method based on molten salt purification provided by the present invention uses molten salt treatment to remove metal impurities and oil from the surface of niobium ingot chips, with no high COD acid and alkali wastewater discharge, and cutting oil and molten salt can be recycled and reused, reducing the cost of waste treatment by more than 90%.
[0016] 2. The niobium ingot chip recovery method based on molten salt purification provided by this invention can significantly reduce chip loss of niobium ingots with fine particle size, and the comprehensive recovery rate of niobium metal is ≥96.5%; in addition, the purity of the recycled niobium billet is ≥99.35%, and the oxygen content is ≤420ppm.
[0017] 3. The niobium ingot chip recycling method based on molten salt purification provided by this invention has a simple processing method and is suitable for continuous production of high-purity niobium materials in aerospace and electronics.
[0018] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0019] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.
[0020] Figure 1 A flowchart of the niobium ingot chip recovery method based on molten salt purification of the present invention is shown. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the invention, are intended to cover non-exclusive inclusion.
[0023] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0024] For niobium ingot chip recycling, chemical cleaning followed by smelting is currently the most common technical approach. A typical process involves removing surface oil using alkaline degreasing agents or strong acids (such as a mixture of nitric acid and hydrofluoric acid), then pressing the cleaned chips into shape, followed by purification through vacuum melting or electron beam melting to finally obtain niobium ingots. However, problems remain, such as incomplete impurity removal and niobium recovery rates below 85%.
[0025] Molten salts have numerous applications in the niobium field, but most focus on preparation or electrolytic refining. For example, niobium is electrolytically refined in chloride molten salts, and niobate powders are prepared in molten salts. There is almost no research on cleaning niobium ingot chips.
[0026] In view of this, the present invention provides a method for recovering niobium ingot chips based on molten salt purification, comprising: Niobium ingot chips are immersed in molten salt to remove metallic impurities and oil from the surface of the chips, resulting in clean niobium chips.
[0027] The mechanism of molten salt treatment is as follows: the removal of metal impurities is a coordination dissolution equilibrium reaction without electron transfer. It relies on the high concentration of anions in the molten salt to form stable and soluble complexes with metal ions to reduce the Gibbs free energy of the system. The spontaneous complexation reaction removes metal impurities from the surface of niobium ingot chips, and the oil is vaporized by the heat of the molten salt.
[0028] In some preferred embodiments, the niobium ingot chips are sieved into ultrafine chips with a particle size of <1 mm, medium chips with a particle size of 1-3 mm, and coarse chips with a particle size of ≥3 mm before being mixed with molten salt. The processing times for the ultrafine chips, medium chips, and coarse chips in the molten salt are 15-20 min, 20-30 min, and 35-40 min, respectively. Finer-particle-size niobium ingot chips have better contact with the molten salt, thus reducing the corresponding processing time.
[0029] In some preferred embodiments, the molten salt is obtained by mixing at least two alkali metal chlorides; for example, LiCl-NaCl, LiCl-KCl, NaCl-KCl, LiBr-NaCl, LiBr-KCl, etc. More preferably, the molten salt is composed of LiCl and KCl in a mass ratio of 40-50:50-60.
[0030] The treatment is carried out at a temperature of 350-450°C. More preferably, at least one of a non-oxidizing gas, such as nitrogen, argon, or helium, is introduced during the treatment to isolate oxygen and prevent niobium from being oxidized again.
[0031] In some preferred embodiments, after obtaining clean niobium chips, they are further subjected to pressing and vacuum sintering.
[0032] In some preferred embodiments, the compression molding includes loading clean niobium chips into a mold at 280-320°C, applying a molding pressure of 180-280 MPa, holding the pressure for 3-6 minutes, and then demolding after cooling the mold to below 100°C to obtain a density ≥7.0 g / cm³. 3 The blank.
[0033] In some preferred embodiments, the vacuum sintering is performed at a vacuum degree <5×10⁻⁶.-2 Two segments are performed under Pa; The first stage of sintering is carried out at 550-650℃ for 1-3 hours to remove adsorbed hydrogen, nitrogen, and carbon impurities from the green block. The second stage of sintering is conducted at 1500-1700℃ for 40-90 minutes, during which an intermittent pulsed current is applied, with a pulse on-time of 10-30 ms and an intermittent time of 60-100 ms. The temperature is controlled below the melting point of niobium throughout the sintering process to achieve solid-state metallurgical bonding at the material-powder interface, enabling rapid densification of the powder material under vacuum conditions while avoiding liquid phase formation and maintaining the micro-nano structure of the material.
[0034] In some preferred embodiments, during the process of immersing niobium ingot chips in molten salt, the generated gas is collected and condensed for recovery. The recovered gas is a cutting lubricant, which can be reused in metal cutting after simple filtration.
[0035] In some preferred embodiments, obtaining clean niobium chips includes purging the niobium ingot chips after molten salt treatment with a non-oxidizing gas to remove the molten salt and other impurities adhering to their surface.
[0036] In some preferred embodiments, the molten salt after processing niobium ingot chips is further subjected to electrolytic treatment to remove dissolved metal impurities. The molten salt is then regenerated and used to process the next batch of niobium ingot chips. Extensive practical experience has shown that the regenerated molten salt obtained after electrolytic treatment can be recycled more than 12 times. After multiple cycles, soluble niobium will accumulate in the molten salt, at which point the molten salt is no longer suitable for processing niobium ingot chips. These molten salts that have been recycled multiple times are then collected and processed to recover the niobium.
[0037] In some preferred embodiments, the electrolysis is performed at a temperature of 350-450°C and a voltage of 2.2-2.8V.
[0038] The present invention will be further described in detail below through specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0039] Example 1 A method for recovering niobium ingot chips based on molten salt purification includes the following steps: S1, Screening Using a closed negative pressure sieve, 5 kg of niobium ingot chips were graded to obtain 1.1 kg of ultrafine chips with a particle size <1 mm, 1.8 kg of medium chips with a particle size of 1-3 mm, and 2.1 kg of coarse chips with a particle size ≥3 mm, which were then stored in different containers.
[0040] S2, Molten Salt Treatment Take 1 kg each of ultrafine, medium, and coarse chips and put them into molten salt mixed with LiCl and KCl at 350℃ in a mass ratio of 45:55. Argon gas is introduced above the molten salt at a flow rate of 8 L / min to isolate oxygen. The treatment times for ultrafine, medium, and coarse chips are 15 min, 20 min, and 35 min, respectively. The gas generated during the treatment is condensed and recovered.
[0041] S3, Impurity Removal and Molten Salt Regeneration After molten salt treatment, the ultrafine, medium, and coarse chips are collected and purged with 380℃ high-purity argon gas to remove residual salt from their surfaces. The molten salt after processing the niobium ingot chips is then filtered through a ceramic filter to remove floating metal chlorides, and subsequently fed into a 400℃ electrolytic cell at 2.2V to remove dissolved metal impurities, purify and regenerate the molten salt, and then used to process the next batch of niobium ingot chips. The regenerated molten salt obtained after electrolytic treatment is recycled up to 15 times, after which it is treated as waste salt, and the niobium is recovered from it using a wet process.
[0042] S4, Compression Molding The ultrafine, medium, and coarse chips obtained in step S3 were mixed in equal mass and placed into a mold preheated to 280°C. A molding pressure of 280 MPa was applied and held for 3 minutes. The mold was then cooled to below 100°C by water cooling. The blank temperature at discharge was 92°C, yielding a density of 7.05 g / cm³. 3 The blank.
[0043] S5, Vacuum Sintering The billet was transferred to a vacuum of 5×10⁻⁶. -3 In the Pa pulse sintering furnace, the first stage of sintering is carried out, and the impurities adsorbed on the green body are removed by holding at 600℃ for 1.5h. The second stage of sintering is carried out at 1500℃ for 40min, with a pulse amplitude of 800A, a pulse conduction time of 20m, and an interval time of 80ms. The temperature throughout the process is lower than the melting point of niobium.
[0044] S6, Cooling Set the cooling water flow rate to 45 L / min and maintain a vacuum degree of 5 × 10⁻⁶. -3 Pa, after cooling to room temperature, discharge the material.
[0045] The contents of soluble niobium, iron, and aluminum in the molten salt after processing niobium ingot chips were determined by inductively coupled plasma atomic emission spectrometry (ICP-AES), and were found to be 3.12 g / L, 1.76 g / L, and 1.41 g / L, respectively. Combined with the contents of Nb₂O₅, Fe₂O₃, and Al₂O₃ in the raw material, the dissolution conversion rates of the metal oxides Nb₂O₅, Fe₂O₃, and Al₂O₃ were found to be 98.3%, 98.6%, and 98.2%, respectively. No niobium, iron, or aluminum were detected in the blank fresh molten salt. These results also demonstrate that molten salt treatment can spontaneously generate soluble metal chloride complexes from oxides without the addition of external redox agents.
[0046] In the entire process of Example 1, the overall niobium recovery rate of a single batch of directly produced niobium billets was 96.5%. This figure does not include the niobium components recovered by subsequent wet smelting of the spent molten salt. After adding the waste molten salt wet niobium extraction, the total metal recovery rate of the entire process can reach over 98.2%. The resulting finished niobium billet has a purity of 99.35%, an oxygen content of 410 ppm, and impurities of 120 ppm iron and 85 ppm aluminum. The oxygen content of the product meets the control index of ≤500 ppm for aerospace niobium materials, and can be used for high-purity niobium components in aerospace applications and niobium materials in the electronics industry.
[0047] Example 2 A method for recovering niobium ingot chips based on molten salt purification includes the following steps: S1, Screening Using a closed negative pressure sieve, 6 kg of niobium ingot chips were graded to obtain 1.4 kg of ultrafine chips with a particle size <1 mm, 2.2 kg of medium chips with a particle size of 1-3 mm, and 2.4 kg of coarse chips with a particle size ≥3 mm, which were then stored in different containers.
[0048] S2, Molten Salt Treatment Take 1 kg each of ultrafine chips, medium chips, and coarse chips, and put them into molten salt mixed with LiCl and KCl at 45:55 by mass at 400℃. Argon gas is introduced above the molten salt at a flow rate of 8 L / min to isolate oxygen. The treatment times for ultrafine chips, medium chips, and coarse chips are 18 min, 25 min, and 38 min, respectively. The gas generated during the treatment is condensed and recovered.
[0049] S3, Impurity Removal and Molten Salt Regeneration After molten salt treatment, the ultrafine, medium, and coarse chips are collected and purged with 380℃ high-purity argon gas to remove residual salt from their surfaces. The molten salt after processing the niobium ingot chips is then filtered through a ceramic filter to remove floating metal chlorides, and subsequently fed into a 400℃ electrolytic cell at 2.5V to remove dissolved metal impurities, purify and regenerate the molten salt, and then used to process the next batch of niobium ingot chips. The regenerated molten salt obtained after electrolytic treatment is recycled up to 18 times, and then treated as waste salt for wet recovery of niobium.
[0050] S4, Compression Molding The ultrafine, medium, and coarse chips obtained in step S3 were mixed in equal mass and placed into a mold preheated to 300°C. A molding pressure of 230 MPa was applied and held for 4 minutes. The mold was then cooled to below 100°C by water cooling. The blank temperature at discharge was 86°C, yielding a density of 7.12 g / cm³. 3 The blank.
[0051] S5, Vacuum Sintering The billet was transferred to a vacuum of 5×10⁻⁶. -3 In the Pa pulse sintering furnace, the first stage of sintering is carried out, and the impurities adsorbed on the green body are removed by holding at 700℃ for 1.5h. The second stage of sintering is carried out at 1600℃ for 60min, with a pulse amplitude of 1000A, a pulse conduction time of 20m, and an interval time of 80ms. The temperature throughout the process is lower than the melting point of niobium.
[0052] S6, Cooling Set the cooling water flow rate to 48 L / min and maintain a vacuum degree of 5 × 10⁻⁶. -3 Pa, after cooling to room temperature, discharge the material.
[0053] The contents of soluble niobium, iron, and aluminum in the molten salt after processing niobium ingot chips were tested by ICP-AES and found to be 3.26 g / L, 1.83 g / L, and 1.47 g / L, respectively. Combined with the contents of Nb2O5, Fe2O3, and Al2O3 in the raw materials, the dissolution conversion rates of metal oxides Nb2O5, Fe2O3, and Al2O3 were found to be 98.7%, 99.1%, and 98.9%, respectively.
[0054] In the entire process of Example 2, the overall recovery rate of niobium was 97.2%. The purity of the resulting tantalum billet was 99.42%, the oxygen content was 360 ppm, and the contents of impurities iron and aluminum were 93 ppm and 68 ppm, respectively.
[0055] Example 3 A method for recovering niobium ingot chips based on molten salt purification includes the following steps: S1, Screening Using a closed negative pressure sieve, 7 kg of niobium ingot chips were graded to obtain 1.6 kg of ultrafine chips with a particle size <1 mm, 2.5 kg of medium chips with a particle size of 1-3 mm, and 2.9 kg of coarse chips with a particle size ≥3 mm, which were then stored in different containers.
[0056] S2, Molten Salt Treatment Take 1 kg each of ultrafine, medium, and coarse chips and put them into molten salt mixed with LiCl and KCl at a mass ratio of 45:55 at 450℃. Argon gas is introduced above the molten salt at a flow rate of 12 L / min to isolate oxygen. The treatment time for ultrafine, medium, and coarse chips is 20 min, 30 min, and 40 min, respectively. The gas generated during the treatment is condensed and recovered.
[0057] S3, Impurity Removal and Molten Salt Regeneration After molten salt treatment, the ultrafine, medium, and coarse chips are collected and purged with 380℃ high-purity argon to remove residual salt from their surfaces. The molten salt after processing the niobium ingot chips is then filtered through a ceramic filter to remove floating metal chlorides, and subsequently fed into a 400℃ electrolytic cell at 2.8V to remove dissolved metal impurities, purify and regenerate the molten salt, and then used to process the next batch of niobium ingot chips. The regenerated molten salt obtained after electrolytic treatment is recycled up to 20 times, and then treated as waste salt for wet recovery of niobium.
[0058] S4, Compression Molding The ultrafine, medium, and coarse chips obtained in step S3 were mixed in equal mass and placed into a mold preheated to 300°C. A molding pressure of 280 MPa was applied and held for 6 minutes. The mold was then cooled to below 100°C by water cooling. The blank temperature at discharge was 81°C, yielding a density of 7.31 g / cm³. 3 The blank.
[0059] S5, Vacuum Sintering The billet was transferred to a vacuum of 1×10⁻⁶. -3 In the Pa pulse sintering furnace, the first stage of sintering is carried out, and the impurities adsorbed on the green body are removed by holding at 800℃ for 1.5h. The second stage of sintering is carried out at 1700℃ for 90min, with a pulse amplitude of 1200A, a pulse conduction time of 20m, and an interval time of 80ms. The temperature throughout the process is lower than the melting point of niobium.
[0060] S6, Cooling Set the cooling water flow rate to 50 L / min and maintain a vacuum degree of 5 × 10⁻⁶. -3 Pa, after cooling to room temperature, discharge the material.
[0061] The contents of soluble niobium, iron, and aluminum in the molten salt after processing niobium ingot chips were tested by ICP-AES and found to be 3.41 g / L, 1.91 g / L, and 1.53 g / L, respectively. Combined with the contents of Nb2O5, Fe2O3, and Al2O3 in the raw materials, the dissolution conversion rates of metal oxides Nb2O5, Fe2O3, and Al2O3 were found to be 99.0%, 99.3%, and 99.1%, respectively.
[0062] In the entire process of Example 3, the overall recovery rate of niobium was 97.8%. The purity of the resulting tantalum billet was 99.48%, the oxygen content was 310 ppm, and the contents of impurities iron and aluminum were 67 ppm and 49 ppm, respectively.
[0063] Comparative Example 1 A method for recycling niobium ingot chips includes the following steps: S1, Screening Using a closed negative pressure sieve, 7 kg of niobium ingot chips were graded to obtain 1.6 kg of ultrafine chips with a particle size <1 mm, 2.5 kg of medium chips with a particle size of 1-3 mm, and 2.9 kg of coarse chips with a particle size ≥3 mm, which were then stored in different containers.
[0064] S2, Compression Molding Take 1 kg each of ultrafine, medium, and coarse chips, mix them evenly, and put them into a mold preheated to 300℃. Apply a molding pressure of 280 MPa and hold for 6 minutes. Cool the mold to below 100℃ with water. The billet temperature at discharge is 81℃, yielding a density of 6.42 g / cm³. 3 The blank.
[0065] S3, Vacuum Sintering The billet was transferred to a vacuum of 1×10⁻⁶. -3 In the Pa pulse sintering furnace, the first stage of sintering is carried out, and the impurities adsorbed on the green body are removed by holding at 800℃ for 1.5h. The second stage of sintering is carried out at 1700℃ for 90min, with a pulse amplitude of 1200A, a pulse conduction time of 20m, and an interval time of 80ms. The temperature throughout the process is lower than the melting point of niobium.
[0066] S4, Cooling Set the cooling water flow rate to 50 L / min and maintain a vacuum degree of 5 × 10⁻⁶. -3 Pa, after cooling to room temperature, discharge the material.
[0067] The tantalum billet obtained in Comparative Example 1 had a purity of 98.12%, an oxygen content of 1250 ppm, and impurities of 1120 ppm iron and 960 ppm aluminum. The impurities were severely excessive, making it unsuitable for use in high-purity niobium materials for aerospace and electronics applications.
[0068] Comparative Example 2 Compared with Example 3, the difference is that in step S4, the mold is not preheated, and a molding pressure of 280 MPa is applied directly at room temperature and held for 6 minutes to obtain a density of 6.10 g / cm³. 3 The blank.
[0069] The green body prepared in Comparative Example 2 had a density of only 6.10 g / cm³. 3 The billet is porous and loose; oxidation loss is aggravated during sintering, and the overall niobium recovery rate is 92.3%. The oxygen content of the finished niobium billet is 780 ppm, the iron content of impurities is 820 ppm, and the aluminum content of impurities is 710 ppm, which are significantly higher than the products of the embodiments of the present invention.
[0070] Comparative Example 3 Compared with Example 3, the difference is that the second stage of sintering in step S5 adopts conventional DC constant temperature holding for 90 minutes without pulse discharge treatment.
[0071] Compared with Example 3, the finished niobium billet prepared in Comparative Example 3 has a large number of interconnected pores inside, a room temperature tensile strength of only 110 MPa, an iron impurity content of 210 ppm, an aluminum impurity content of 152 ppm, and a local oxygen content of 650 ppm. The material has poor mechanical properties and cannot be directly forged and rolled.
[0072] Table 1 summarizes the strength and impurity content of the finished tantalum blanks obtained from the above embodiments and comparative examples.
[0073] Table 1
[0074] As shown in Table 1, the finished tantalum billet prepared in Example 1 of the present invention has a room temperature tensile strength of 245 MPa and impurities of 120 ppm iron and 85 ppm aluminum; the finished tantalum billet prepared in Example 2 has a room temperature tensile strength of 262 MPa and impurities of 93 ppm iron and 68 ppm aluminum; the finished tantalum billet prepared in Example 3 has a room temperature tensile strength of 278 MPa and impurities of 67 ppm iron and 49 ppm aluminum; the finished tantalum billet prepared in Comparative Example 1 has a room temperature tensile strength of 153 MPa and impurities of 1120 ppm iron and 960 ppm aluminum; the finished tantalum billet prepared in Comparative Example 2 has a room temperature tensile strength of 142 MPa and impurities of 820 ppm iron and 710 ppm aluminum; the finished tantalum billet prepared in Comparative Example 3 has a room temperature tensile strength of 110 MPa and impurities of 210 ppm iron and 152 ppm aluminum.
[0075] Compared to Examples 1-3, Comparative Example 1 showed a significant decrease in strength and a significant increase in impurity content in the prepared tantalum billet. This indicates that simply grading niobium ingot chips without further processing cannot meet the requirements for recycling. Molten salt treatment allows the high concentration of anions in the molten salt to form stable and soluble complexes with metal ions, lowering the Gibbs free energy of the system. The spontaneous complexation reaction removes metal impurities from the surface of the niobium ingot chips, while the oil is vaporized by the heat of the molten salt.
[0076] Combining the treatment methods of Comparative Example 2 and Example 3, it was demonstrated that warm pressing at a certain temperature can significantly improve the density of the blank, reduce sintering oxidation loss, and increase the recovery rate of niobium.
[0077] Compared to Example 3, the strength of the finished tantalum billet prepared in Comparative Example 3 decreased significantly and the impurity content increased significantly. This is because intermittent pulsed current sintering can instantly break through the trace oxide film and achieve dense solid-phase bonding of the scrap material by relying on local Joule heating, thereby obtaining a recycled niobium billet with high density, high mechanical properties, low impurity content, and forgeability.
[0078] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A method for recovering niobium ingot chips based on molten salt purification, characterized in that, include, Niobium ingot chips are immersed in molten salt to remove metallic impurities and oil from the surface of the chips, resulting in clean niobium chips.
2. The method for recovering niobium ingot chips based on molten salt purification according to claim 1, characterized in that, The niobium ingot chips are sieved into ultrafine chips with a particle size of <1 mm, medium chips with a particle size of 1-3 mm, and coarse chips with a particle size of ≥3 mm before being mixed with molten salt. The treatment times for the ultrafine chips, the medium chips, and the coarse chips in the molten salt are 15-20 min, 20-30 min, and 35-40 min, respectively.
3. The method for recovering niobium ingot chips based on molten salt purification according to claim 1, characterized in that, The molten salt is obtained by mixing at least two alkali metal chlorides; The treatment is carried out at a temperature of 350-450°C.
4. The method for recovering niobium ingot chips based on molten salt purification according to claim 1, characterized in that, After obtaining clean niobium chips, they are further pressed and vacuum sintered.
5. The method for recovering niobium ingot chips based on molten salt purification according to claim 4, characterized in that, The compression molding process includes loading clean niobium chips into a mold at 280-320°C, applying a molding pressure of 180-280 MPa, holding the pressure for 3-6 minutes, and then demolding the mold after cooling it to below 100°C to obtain a product with a density ≥7.0 g / cm³. 3 The blank.
6. The method for recovering niobium ingot chips based on molten salt purification according to claim 4, characterized in that, The vacuum sintering is performed at a vacuum degree <5×10⁻⁶. -2 Two segments are performed under Pa; The first stage of sintering is carried out at a temperature of 550-650℃ for 1-3 hours; the second stage of sintering is carried out at 1500-1700℃ for 40-90 minutes, during which an intermittent pulse current is applied, with a pulse conduction time of 10-30ms and an interval time of 60-100ms.
7. The method for recovering niobium ingot chips based on molten salt purification according to claim 1, characterized in that, During the process of immersing niobium ingot chips in molten salt, the generated gas is collected and condensed for recovery.
8. The method for recovering niobium ingot chips based on molten salt purification according to claim 1, characterized in that, The process of obtaining clean niobium chips involves purging the niobium ingot chips after molten salt treatment with a non-oxidizing gas to remove the molten salt and other impurities adhering to their surface.
9. The method for recovering niobium ingot chips based on molten salt purification according to claim 1, characterized in that, The molten salt electrolysis process will also be used to remove dissolved metal impurities from the niobium ingot chips, and the molten salt will be regenerated and used for the next batch of niobium ingot chips.
10. The method for recovering niobium ingot chips based on molten salt purification according to claim 9, characterized in that, The electrolytic treatment is carried out at a temperature of 350-450℃ and a voltage of 2.2-2.8V.
Citation Information
Patent Citations
Niobium ingot chip recovery method
CN121046659A