A method for upgrading and regenerating waste nickel-rich layered cathode materials

By using a ternary eutectic molten salt medium of LiOH·H2O-NaCl-KCl and an oxygen atmosphere sintering process, efficient regeneration of waste layered cathode materials has been achieved. This solves the problems of high environmental cost and insufficient performance in existing technologies, improves the stability and fast charging performance of the materials, and is suitable for high energy density power batteries and energy storage applications.

CN123120953APending Publication Date: 2026-11-17JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611445525.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for recycling waste layered cathode materials suffer from problems such as high environmental costs, low regeneration performance, waste of solid waste resources, poor process adaptability, insufficient high-voltage stability, and weak fast-charging capability, making it impossible to achieve high-voltage performance upgrades and industrial continuous mass production.

Method used

Using LiOH·H2O-NaCl-KCl ternary eutectic molten salt as the reaction medium and lithium replenishment source, combined with oxygen atmosphere segmented sintering, water washing desalination, and secondary calcination processes, Al3+ and Cu2+ are used to embed into the lattice sites, simultaneously completing the removal of organic impurities, lithium vacancy replenishment, lattice defect repair, and polycrystalline particle single crystal reconstruction, thus achieving Al/Cu dual lattice site synergistic doping.

Benefits of technology

It realizes the resource utilization of waste aluminum and copper current collectors, reduces recycling costs, improves the thermal stability and cycle reversibility of materials, has higher discharge specific capacity and ultra-high rate fast charging performance, is compatible with a variety of waste cathode materials, and is suitable for high energy density power batteries and energy storage applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120953A_ABST
    Figure CN123120953A_ABST
Patent Text Reader

Abstract

This application provides a method for upgrading and regenerating waste nickel-rich layered cathode materials, comprising: (1) dismantling, grinding, sieving, and cleaning the waste nickel-rich layered cathode materials to obtain waste cathode powder; (2) collecting scraps from waste aluminum current collectors, crushing, grinding, and sieving them to obtain Al-doped powder; collecting scraps from waste copper current collectors, etching with alkaline solution, washing, drying, and grinding them to obtain Cu(OH)2-doped powder; (3) mixing the waste cathode powder, Al-doped powder, Cu(OH)2-doped powder, and ternary eutectic molten salt evenly to obtain composite precursor powder; (4) placing the composite precursor powder in an oxygen atmosphere for segmented heating and sintering, cooling, and then washing with water to remove salt and performing secondary calcination to obtain high-voltage single-crystal layered cathode materials. The method provided in this application can utilize dismantled current collector waste on-site, is broadly adaptable to various types of waste cathodes, and integrates lattice repair and high-voltage performance upgrade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of battery regeneration technology, and relates to a method for regenerating cathode materials, and more particularly to an upgraded regeneration method for waste nickel-rich layered cathode materials. Background Technology

[0002] Currently, the global new energy vehicle industry and electrochemical energy storage industry are experiencing explosive growth, and various countries have successively introduced policies for the management of power battery recycling to promote the full life cycle management of lithium batteries. Since its large-scale commercial use, lithium-ion power batteries have undergone an 8-10 year service life, and the first batch of vehicle power batteries and energy storage batteries have entered the large-scale retirement and scrapping window period, with the annual retirement volume increasing to the millions of tons.

[0003] Retired lithium-ion batteries contain large amounts of valuable metals such as nickel, cobalt, manganese, lithium, copper, and aluminum. If disposed of through indiscriminate dumping, landfilling, or crude dismantling, organic solvents, fluorides, and heavy metal ions from the battery's electrolyte will seep into the soil and groundwater, causing persistent ecological pollution. Simultaneously, the loss of these valuable metals exacerbates dependence on imports for key minerals like lithium, nickel, and cobalt, hindering the security of China's new energy industry supply chain and the achievement of dual-carbon goals. Therefore, efficient, green, low-cost, and high-value-added recycling technologies for the cathode materials of retired lithium-ion batteries have become an essential industry need and a hot research topic.

[0004] Existing recycling routes for waste layered cathode materials are mainly divided into three categories: pyrometallurgy, hydrometallurgy, and direct recycling, all of which have significant shortcomings. Pyrometallurgy relies on high-temperature smelting to enrich metals. While it boasts strong material compatibility, it suffers from significant energy consumption, carbon emissions, and flue gas pollution. The smelting process completely destroys the original layered crystal structure, producing only coarse metal material to be returned to upstream metallurgical processes. This results in a long recycling chain, low product added value, and does not align with low-carbon development principles. Hydrometallurgy prepares cathodes through strong acid and alkali leaching, extraction precipitation, and then sintering. While the metal recovery rate is acceptable, the process is lengthy, consumes large amounts of acid and alkali reagents, generates substantial amounts of wastewater and hazardous sludge, and incurs high costs for waste treatment. Furthermore, the leaching process easily introduces impurities and depletes metal, leading to poor batch stability of recycled materials and making it unsuitable for the low-margin, large-scale production scenarios of the recycling industry.

[0005] Conventional direct regeneration processes, centered on lithium replenishment and repair of the original crystal framework, offer advantages such as short processes, low carbon footprint, and low energy consumption, making them a mainstream research and development direction in the industry. However, existing technologies face several technical bottlenecks. First, they can only restore the initial performance of spent cathode materials, failing to achieve quality improvement and upgrades. This makes them unsuitable for the 4.6V high voltage and ultra-fast charging requirements of next-generation batteries. Under high voltage conditions, materials are prone to cell deformation, microcracks, irreversible phase transitions, and lattice oxygen precipitation, resulting in rapid cycle degradation and a high risk of thermal runaway. Second, the aluminum and copper current collector scraps generated from battery dismantling can only be sold off at low prices or landfilled, failing to be converted into modified raw materials on-site. This leads to resource waste and increased processing costs, preventing the formation of a closed-loop industrial chain. Third, the ability to repair microscopic defects is insufficient. After cycling, waste batteries have nearly 40% lithium loss, a large number of lattice vacancies, Li / Ni antisite defects, and thick layers of rock salt impurities. Conventional lithium replenishment simply adds lithium elements and cannot repair lattice collapse. The material remains a polycrystalline particle with concentrated grain boundary stress, resulting in inherent deficiencies in fast charging and long-cycle performance. Fourth, the material has poor adaptability. It can only process a single type of regular electrode sheet and cannot be compatible with NCM multi-element systems and mixed waste of lithium cobalt oxide. The sorting cost for broken black powder and water vapor-eroded failed batteries is high, which limits industrial promotion.

[0006] To improve the high-voltage stability of layered cathodes, existing research mainly employs methods such as single-element doping, coating modification, and single-crystal preparation, but these methods have significant technical limitations. Modification relies on purchasing high-purity aluminum and copper salts, which significantly increases regeneration costs; doping, repair, single-crystal formation, and coating are carried out in steps, which are cumbersome, time-consuming, and energy-intensive; single-element doping can only improve the properties of a single crystal lattice and cannot simultaneously suppress high-voltage strain accumulation and lattice oxygen evolution; single-crystal preparation is only suitable for liquid-phase synthesis with virgin raw materials and cannot directly reconstruct single-crystal particles in situ on waste cathodes.

[0007] It is evident that existing technologies generally suffer from multiple problems, such as high environmental costs, low regeneration performance, waste of solid waste resources, poor process adaptability, insufficient high-voltage stability, and weak fast-charging capability. The market urgently needs a closed-loop regeneration process that can utilize dismantled current collector waste on-site, be broadly compatible with various types of waste cathodes, and integrate lattice repair and high-voltage performance upgrades to fill the gaps in the existing technology system and support the development of waste lithium battery recycling towards high added value, high performance, and low-carbon circularity. Summary of the Invention

[0008] To address the shortcomings of existing technologies, the purpose of this application is to provide an upgraded regeneration method for waste nickel-rich layered cathode materials. This method utilizes dismantled current collector waste on-site, is broadly adaptable to various types of waste cathodes, and integrates lattice repair to achieve high-voltage performance upgrades in a closed-loop regeneration process, thus filling a gap in the existing technology system.

[0009] To achieve this objective, the present application adopts the following technical solution:

[0010] In a first aspect, this application provides a method for upgrading and regenerating waste nickel-rich layered cathode materials, comprising the following steps:

[0011] (1) Disassemble, grind, sieve and clean the waste nickel-rich layered cathode material to obtain waste cathode powder;

[0012] (2) Collect scraps of waste aluminum current collectors, crush, grind and sieve to obtain Al doped powder; collect scraps of waste copper current collectors, etch with alkaline solution, wash, dry and grind to obtain Cu(OH)2 doped powder;

[0013] (3) Prepare a ternary eutectic molten salt of LiOH·H2O-NaCl-KCl as a reaction medium and lithium replenishment source. Mix the waste cathode powder, Al doped powder, Cu(OH)2 doped powder and ternary eutectic molten salt evenly to obtain composite precursor powder.

[0014] (4) The composite precursor powder is placed in an oxygen atmosphere for segmented heating and sintering. After cooling, it is washed with water to remove salt and then calcined again to obtain a high-voltage single-crystal layered cathode material.

[0015] Steps (1) and (2) are not in any particular order.

[0016] This application transforms scraps and fragments from waste aluminum and copper current collectors into doping raw materials, eliminating the need to purchase high-purity doping reagents, thus realizing the resource utilization of solid waste, reducing recycling costs, and building a green circular industrial chain for waste batteries. It uses LiOH·H2O-NaCl-KCl ternary eutectic molten salt as the reaction medium and lithium replenishment source, combined with oxygen atmosphere segmented sintering, water washing and desalting, and secondary roasting integrated processes to simultaneously complete the removal of organic impurities, lithium vacancy replenishment, lattice defect repair, polycrystalline particle single crystal reconstruction, and Al / Cu dual lattice site synergistic doping. This eliminates the step-by-step modification process, shortens the production cycle, reduces energy consumption, and is suitable for industrial continuous mass production.

[0017] Among them, the molten salt liquid phase forms a solid-liquid reaction interface, which promotes the rapid diffusion and replenishment of lithium ions. Al 3+ Cu 2+ The two lattice sites of the transition metal layer and lithium layer are respectively embedded to fill lattice vacancies and suppress Li / Ni antisite defects. At the same time, it induces polycrystalline secondary particles to complete the morphology reconstruction of single-crystal primary particles, reduces the number of grain boundaries, and alleviates stress concentration during charging and discharging. The Al and Cu dual sites synergistically modify and strengthen metal-oxygen bonding, expand interlayer spacing, and anchor lattice oxygen, suppressing cell strain accumulation, irreversible precipitation of lattice oxygen, particle microcracks and irreversible rock salt / spinel phase transformation under the 2.6~4.6V ultra-high voltage window, reducing the risk of cell gas generation, cracking and thermal runaway, thereby improving the thermal stability and cycle reversibility of the material.

[0018] In addition, the recycled monocrystalline cathode has a higher discharge specific capacity, excellent long-cycle capacity retention rate and ultra-high-rate fast charging performance, which is significantly better than traditional directly recycled polycrystalline materials. It can meet the stringent application requirements of high-energy-density power batteries, energy storage, high-end power tools and other applications. The above process is compatible with a variety of waste cathode materials, does not require strict sorting, reduces the front-end material sorting cost, and has environmental, economic and engineering practical value.

[0019] And / or, the waste nickel-rich layered cathode material in step (1) includes at least one of NCM523, NCM622, NCM83 or LiCoO2.

[0020] And / or, the failure types of the waste nickel-rich layered cathode material in step (1) include at least one of the following: electrode breakage and black powder, dismantled waste cylindrical battery cathode, or water vapor erosion failure and scrapped cathode.

[0021] And / or, the cleaning agent used in step (1) includes a mixed solution of N-methylpyrrolidone and anhydrous ethanol.

[0022] And / or, after the cleaning described in step (1), the product is dried and sieved.

[0023] And / or, the drying temperature is 55~65℃ and the time is 10~14h.

[0024] And / or, the particle size of the Al-doped powder in step (2) is 10~30 mesh.

[0025] And / or, the alkaline solution used in step (2) for alkaline etching includes a sodium hydroxide solution with a concentration of 1~3 mol / L.

[0026] And / or, the immersion time for alkaline etching in step (2) is 30~60 min.

[0027] And / or, the detergent used in step (2) is deionized water, and the washing endpoint is when the washing liquid is neutral.

[0028] And / or, the molar ratio of LiOH·H2O, NaCl, and KCl in the ternary eutectic molten salt described in step (3) is (1~3):(0.5~1.5):(0.5~1.5).

[0029] And / or, based on the total molar amount of waste cathode powder, the mixing amount of the Al doped powder is 2.5 mol% to 3.5 mol%.

[0030] And / or, based on the total molar amount of waste cathode powder, the mixing amount of the Cu(OH)2 doped powder is 0.8mol%~1.2mol%.

[0031] And / or, the oxygen purity of the oxygen atmosphere in step (4) is ≥99%.

[0032] And / or, the segmented heating sintering in step (4) is a two-stage heating sintering, including a first stage heating sintering and a second stage heating sintering.

[0033] And / or, the heating rates of the first stage of heating sintering and the second stage of heating sintering are 4~6℃ / min, respectively.

[0034] And / or, the target temperature for the first stage of heating and sintering is 480~520℃, and the holding time is 2.5~3.5h.

[0035] And / or, the target temperature for the second stage of heating and sintering is 830~870℃, and the holding time is 7~9h.

[0036] And / or, the water washing and desalination in step (4) includes sequentially performing deionized water soaking, stirring, centrifugation, and drying.

[0037] And / or, the solid-liquid ratio of the deionized water soaking is 1g:(8~12)mL.

[0038] And / or, the endpoint of the water washing desalination is that no free alkaline ions and chloride ions remain in the washing solution.

[0039] And / or, the secondary calcination in step (4) is carried out in an oxygen atmosphere with an oxygen purity ≥99%.

[0040] And / or, the temperature of the secondary roasting in step (4) is 700~740℃.

[0041] And / or, the secondary roasting time in step (4) is 4.5~5.5h.

[0042] Secondly, this application provides a high-voltage single-crystal layered cathode material prepared by the upgrading and regeneration method described in the first aspect, wherein the high-voltage single-crystal layered cathode material has an operating voltage of 2.6~4.6V.

[0043] Compared with the prior art, this application has the following advantages:

[0044] (1) This application converts the scraps of waste aluminum and copper current collectors into doped raw materials, eliminating the need to purchase high-purity doping reagents, realizing the resource utilization of solid waste, reducing recycling costs, and building a green circular industrial chain for waste batteries; using LiOH·H2O-NaCl-KCl ternary eutectic molten salt as the reaction medium and lithium replenishment source, combined with oxygen atmosphere segmented sintering, water washing desalination, and secondary roasting integrated process, simultaneously completes the removal of organic impurities, lithium vacancy replenishment, lattice defect repair, polycrystalline particle single crystal reconstruction, and Al / Cu dual lattice site synergistic doping, eliminating the step-by-step modification process, shortening the production cycle, reducing energy consumption, and adapting to industrial continuous mass production.

[0045] (2) The molten salt liquid phase forms a solid-liquid reaction interface, which promotes the rapid diffusion and replenishment of lithium ions. Al 3+ Cu 2+ The two lattice sites of the transition metal layer and lithium layer are respectively embedded to fill lattice vacancies and suppress Li / Ni antisite defects. At the same time, it induces polycrystalline secondary particles to complete the morphology reconstruction of single-crystal primary particles, reduces the number of grain boundaries, and alleviates stress concentration during charging and discharging. The Al and Cu dual sites synergistically modify and strengthen metal-oxygen bonding, expand interlayer spacing, and anchor lattice oxygen, suppressing cell strain accumulation, irreversible precipitation of lattice oxygen, particle microcracks and irreversible rock salt / spinel phase transformation under the 2.6~4.6V ultra-high voltage window, reducing the risk of cell gas generation, cracking and thermal runaway, thereby improving the thermal stability and cycle reversibility of the material.

[0046] (3) Regenerated single-crystal cathode has higher discharge specific capacity, excellent long cycle capacity retention rate and ultra-high rate fast charging performance, which is significantly better than traditional direct regenerated polycrystalline materials. It can meet the stringent application requirements of high energy density power batteries, energy storage, high-end power tools, etc. The above process is compatible with a variety of waste cathode materials, without strict sorting, reducing the front-end material sorting cost, and has environmental value, economic value and engineering practical value. Attached Figure Description

[0047] Figure 1 These are scanning electron microscope images of the single-crystal NCM material provided in Example 2.

[0048] Figure 2 This is a scanning electron microscope image of the polycrystalline NCM material provided in Comparative Example 1. Detailed Implementation

[0049] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0050] One embodiment of this application provides a method for upgrading and regenerating waste nickel-rich layered cathode materials, including the following steps:

[0051] (1) Disassemble, grind, sieve and clean the waste nickel-rich layered cathode material to obtain waste cathode powder;

[0052] (2) Collect scraps of waste aluminum current collectors, crush, grind and sieve to obtain Al doped powder; collect scraps of waste copper current collectors, etch with alkaline solution, wash, dry and grind to obtain Cu(OH)2 doped powder;

[0053] (3) Prepare a ternary eutectic molten salt of LiOH·H2O-NaCl-KCl as a reaction medium and lithium replenishment source. Mix the waste cathode powder, Al doped powder, Cu(OH)2 doped powder and ternary eutectic molten salt evenly to obtain composite precursor powder.

[0054] (4) The composite precursor powder is placed in an oxygen atmosphere for segmented heating and sintering. After cooling, it is washed with water to remove salt and then calcined again to obtain a high-voltage single-crystal layered cathode material.

[0055] Steps (1) and (2) are not in any particular order.

[0056] This application transforms scraps and fragments from waste aluminum and copper current collectors into doping raw materials, eliminating the need to purchase high-purity doping reagents, thus realizing the resource utilization of solid waste, reducing recycling costs, and building a green circular industrial chain for waste batteries. It uses LiOH·H2O-NaCl-KCl ternary eutectic molten salt as the reaction medium and lithium replenishment source, combined with oxygen atmosphere segmented sintering, water washing and desalting, and secondary roasting integrated processes to simultaneously complete the removal of organic impurities, lithium vacancy replenishment, lattice defect repair, polycrystalline particle single crystal reconstruction, and Al / Cu dual lattice site synergistic doping. This eliminates the step-by-step modification process, shortens the production cycle, reduces energy consumption, and is suitable for industrial continuous mass production.

[0057] Among them, the molten salt liquid phase forms a solid-liquid reaction interface, which promotes the rapid diffusion and replenishment of lithium ions. Al 3+ Cu 2+ The two lattice sites of the transition metal layer and lithium layer are respectively embedded to fill lattice vacancies and suppress Li / Ni antisite defects. At the same time, it induces polycrystalline secondary particles to complete the morphology reconstruction of single-crystal primary particles, reduces the number of grain boundaries, and alleviates stress concentration during charging and discharging. The Al and Cu dual sites synergistically modify and strengthen metal-oxygen bonding, expand interlayer spacing, and anchor lattice oxygen, suppressing cell strain accumulation, irreversible precipitation of lattice oxygen, particle microcracks and irreversible rock salt / spinel phase transformation under the 2.6~4.6V ultra-high voltage window, reducing the risk of cell gas generation, cracking and thermal runaway, thereby improving the thermal stability and cycle reversibility of the material.

[0058] In addition, the recycled monocrystalline cathode has a higher discharge specific capacity, excellent long-cycle capacity retention rate and ultra-high-rate fast charging performance, which is significantly better than traditional directly recycled polycrystalline materials. It can meet the stringent application requirements of high-energy-density power batteries, energy storage, high-end power tools and other applications. The above process is compatible with a variety of waste cathode materials, does not require strict sorting, reduces the front-end material sorting cost, and has environmental, economic and engineering practical value.

[0059] In some embodiments, the waste nickel-rich layered cathode material in step (1) includes NCM523 (LiNi) 0.5 Co 0.2 Mn 0.3 O2), NCM622 (LiNi) 0.6 Co 0.2 Mn 0.2 O2), NCM83 (LiNi) 0.83 Co 0.12 Mn 0.05 At least one of O2 or LiCoO2.

[0060] In some embodiments, the failure type of the waste nickel-rich layered cathode material in step (1) includes at least one of the following: electrode breakage and black powder, dismantled waste cylindrical battery cathode, or cathode that has failed due to water vapor erosion.

[0061] In some embodiments, the cleaning agent used in step (1) includes a mixed solution of N-methylpyrrolidone (NMP) and anhydrous ethanol, which can effectively remove impurities such as residual electrolyte, PVDF binder, and conductive agent from the powder surface.

[0062] In some embodiments, the cleaning in step (1) is followed by drying and sieving to remove large particle agglomerates.

[0063] In some embodiments, the drying temperature is 55~65°C, for example, 55°C, 57°C, 59°C, 61°C, 63°C or 65°C, and the time is 10~14h, for example, 10h, 11h, 12h, 13h or 14h, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0064] In some embodiments, the particle size of the Al-doped powder in step (2) is 10 to 30 mesh, for example, it can be 10 mesh, 12 mesh, 14 mesh, 16 mesh, 18 mesh, 20 mesh, 22 mesh, 24 mesh, 26 mesh, 28 mesh or 30 mesh, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0065] In some embodiments, the alkaline solution used in step (2) for alkaline etching includes a sodium hydroxide solution with a concentration of 1 to 3 mol / L, for example, it can be 1 mol / L, 1.4 mol / L, 1.8 mol / L, 2 mol / L, 2.4 mol / L, 2.8 mol / L or 3 mol / L, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0066] This application uses alkaline etching to remove scraps and debris from waste copper current collectors. This process removes impurities such as residual electrode powder, organic binders, and electrolyte residues adhering to the surface of the copper current collector, preventing these impurities from being introduced into the subsequent regeneration system and contaminating the final cathode material. Furthermore, etching the original oxide layer on the copper surface fully exposes the copper substrate, facilitating subsequent grinding to obtain an active copper-based precursor. This ensures that Cu elements can be uniformly embedded in the lattice for doping during subsequent sintering. Simultaneously, it regulates the microscopic activity of the copper surface, allowing copper to gradually transform into Cu(OH)2 precursors in the alkaline solution, resulting in Cu(OH)2 powder that can be used for lattice doping, replacing purchased high-purity copper salts.

[0067] In some embodiments, the immersion time for alkaline etching in step (2) is 30 to 60 minutes, for example, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0068] In some embodiments, the detergent used in step (2) is deionized water, and the washing endpoint is when the washing liquid is neutral.

[0069] This application uses deionized water to wash the material after alkaline etching until it is neutral, which can thoroughly remove the alkaline residue on the surface of the material, avoid excessive alkali from being carried into the molten salt sintering system, prevent the imbalance of lithium salt ratio in the system and the formation of impurity phases in the material lattice due to excessive local alkalinity, and at the same time remove soluble by-products generated during the etching process, reduce the residue of soluble impurities in the finished product, and avoid the problems of aggravated side reactions and cell gas generation during high-voltage cycling.

[0070] In some embodiments, the molar ratio of LiOH·H2O, NaCl, and KCl in the ternary eutectic molten salt of step (3) is (1~3):(0.5~1.5):(0.5~1.5), for example, it can be 1:1:0.5, 1.5:0.5:1.5, 2:1:1, 2.5:1.5:1 or 3:1:1, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0071] In the aforementioned ternary eutectic molten salt, LiOH·H2O serves as the primary lithium source, generating a large amount of free Li in the molten state. +This process rapidly fills the vacancies in the lithium and transition metal layers formed by long-term recycling of waste cathodes, repairing lithium absences and Li / Ni antisite defects. Simultaneously, it provides an alkaline melting environment, oxidizing and decomposing organic residues such as PVDF and conductive carbon black within the powder during sintering, and participating in lattice reconstruction to provide lithium for the single-crystal growth of polycrystalline particles. NaCl and KCl, as composite fluxes, synergistically lower the overall eutectic melting point of the molten salt, enabling the system to form a stable liquid phase at lower temperatures. Compared to single lithium salts, this significantly reduces the melting initiation temperature and high-temperature energy consumption. Furthermore, the molten chloride salt forms a continuous liquid phase that coats the cathode particles, constructing a large-area solid-liquid reaction interface, accelerating ion diffusion, and promoting uniform Al / Cu doping. At the same time, NaCl and KCl are chemically stable and do not react with the layered cathode matrix in high-temperature environments. They can be completely removed by water washing after sintering, avoiding impurity residue contamination of the finished product.

[0072] Furthermore, this application limits the molar ratio of the components in the ternary eutectic molten salt to a reasonable range, balancing lithium replenishment effect and doping uniformity. If the lithium salt ratio is too low, the lithium supply will be insufficient and defect repair will be incomplete; if the lithium salt ratio is too high, the molten salt viscosity will be high, the liquid phase wetting will be poor, and the single crystallization and doping uniformity will decrease.

[0073] In some embodiments, the mixing amount of Al-doped powder is 2.5 mol% to 3.5 mol%, based on the total molar amount of waste cathode powder. For example, it can be 2.5 mol%, 2.7 mol%, 2.9 mol%, 3.1 mol%, 3.3 mol%, or 3.5 mol%, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0074] In some embodiments, based on the total molar amount of waste cathode powder, the mixing amount of Cu(OH)2 doped powder is 0.8 mol% to 1.2 mol%, for example, it can be 0.8 mol%, 0.85 mol%, 0.9 mol%, 0.95 mol%, 1.0 mol%, 1.05 mol%, 1.1 mol%, 1.15 mol% or 1.2 mol%, but it is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0075] In some embodiments, the mixing amount of the ternary eutectic molten salt can be adaptively adjusted according to the lithium deficiency ratio of the waste cathode powder, and no specific limitation is made here.

[0076] In some embodiments, the oxygen purity of the oxygen atmosphere in step (4) is ≥99%, for example, it can be 99%, 99.5%, 99.9%, 99.95% or 99.99%, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0077] In some embodiments, the segmented heating sintering in step (4) is a two-stage heating sintering, including a first-stage heating sintering and a second-stage heating sintering.

[0078] The first stage of heating and sintering achieves material dehydration, molten salt eutectic melting, carbon impurity oxidation and removal, and preliminary lithium replenishment. The second stage of heating and sintering promotes the formation of a liquid phase coating layer by the molten salt, constructs a solid-liquid wetting reaction interface, and drives the Li-Li... + Rapid diffusion replenishes lithium, repairs lattice vacancies and structural collapse, induces preferential growth of polycrystalline grains to achieve monocrystalline formation, and simultaneously embeds Al and Cu elements in situ into dual lattice doping sites.

[0079] In some embodiments, the heating rates of the first stage of heating sintering and the second stage of heating sintering are 4~6℃ / min, for example, 4℃ / min, 4.4℃ / min, 4.8℃ / min, 5℃ / min, 5.2℃ / min, 5.6℃ / min or 6℃ / min, but are not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0080] In some embodiments, the target temperature for the first stage of heating and sintering is 480~520℃, for example, 480℃, 488℃, 496℃, 504℃, 512℃ or 520℃, and the holding time is 2.5~3.5h, for example, 2.5h, 2.7h, 2.9h, 3.1h, 3.3h or 3.5h, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0081] In some embodiments, the target temperature for the second stage of heating and sintering is 830~870℃, for example, it can be 830℃, 840℃, 845℃, 850℃, 855℃, 860℃ or 870℃, and the holding time is 7~9h, for example, it can be 7h, 7.4h, 7.8h, 8.2h, 8.6h or 9h, but it is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0082] In some embodiments, the water washing and desalination in step (4) includes sequentially soaking in deionized water, stirring, centrifuging, and drying.

[0083] In some embodiments, the solid-liquid ratio of the deionized water soaking is 1g:(8~12)mL, for example, it can be 1g:8mL, 1g:9mL, 1g:10mL, 1g:11mL or 1g:12mL, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0084] In some embodiments, the endpoint of the water washing desalination is that no free alkaline ions and chloride ions remain in the washing solution.

[0085] In some embodiments, the secondary calcination in step (4) is carried out in an oxygen atmosphere with an oxygen purity ≥99%, such as 99%, 99.5%, 99.9%, 99.95% or 99.99%, but not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0086] In some embodiments, the temperature of the secondary calcination in step (4) is 700~740℃, for example, it can be 700℃, 708℃, 716℃, 724℃, 732℃ or 740℃, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0087] In some embodiments, the secondary roasting time in step (4) is 4.5 to 5.5 hours, for example, 4.5 hours, 4.7 hours, 4.9 hours, 5.0 hours, 5.1 hours, 5.3 hours or 5.5 hours, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0088] This application involves a second calcination process after water washing and desalination, which can fully remove the internal water of crystallization of the material, further regulate the lattice order, and strengthen the bonding of doped elements.

[0089] One embodiment of this application also provides a high-voltage single-crystal layered cathode material prepared by the upgraded regeneration method described in any of the above embodiments. The operating voltage of the high-voltage single-crystal layered cathode material is 2.6~4.6V, for example, it can be 2.6V, 3.0V, 3.4V, 3.8V, 4.2V or 4.6V, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0090] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0091] Example 1

[0092] This embodiment provides a method for upgrading and regenerating waste nickel-rich layered cathode materials, specifically including the following steps:

[0093] (1) Selecting LiNi power units for mass-produced retired electric vehicles 0.83 Co 0.12 Mn 0.05Waste O2 positive electrode sheets were mechanically peeled, crushed, and passed through a 100-mesh standard sieve to obtain coarse positive electrode powder. A cleaning solution of NMP and anhydrous ethanol in a 1:1 volume ratio was used, with a solid-liquid ratio of 1g:8mL, and the mixture was magnetically stirred at room temperature for 2 hours. After settling, the upper waste liquid was discarded, and the cleaning was repeated 3 times to thoroughly remove residual electrolyte, PVDF binder, conductive carbon black, and other impurities. The cleaned filter cake was placed in a 60℃ forced-air oven for constant temperature drying for 12 hours, cooled, and then passed through a 200-mesh sieve to obtain high-purity waste NCM83 positive electrode powder.

[0094] (2) Collect scraps of waste aluminum current collectors from the power battery dismantling production line, grind them by jaw crusher and planetary ball mill, and pass them through a 20-mesh standard sieve to directly obtain Al-doped powder; collect scraps of waste copper current collectors, remove the residual powder attached to the surface, soak them in a 2mol / L NaOH solution at room temperature for 40 minutes to dissolve the surface oxide layer and organic coating, wash them repeatedly with deionized water until the pH of the filtrate is 7, dry them at 60℃ and grind them to obtain pure Cu(OH)2 doped powder.

[0095] (3) Prepare ternary eutectic molten salt by weighing according to the molar ratio of LiOH·H2O:NaCl:KCl=2:1:1; based on the total molar amount of waste NCM83 cathode powder, add 3mol% Al doped powder and 1mol% Cu(OH)2 doped powder, and mix them with the ternary eutectic molten salt and waste cathode powder in a three-dimensional high-speed mixer for 30 minutes to obtain composite precursor powder.

[0096] (4) Spread the composite precursor powder evenly on the alumina crucible, place it in the tube furnace, and continuously introduce 99.99% high-purity oxygen; set the heating rate to 5℃ / min, heat to 500℃ in the first stage and keep it at a constant temperature for 3h; then heat to 850℃ at 5℃ / min and keep it at a constant temperature for 8h. After sintering, let the furnace cool down naturally to room temperature.

[0097] (5) The sintered crude product was washed and centrifuged repeatedly with deionized water at a solid-liquid ratio of 1g:10mL until the washing liquid was free of free alkaline ions and chloride ions. After washing, the material was dried at 60°C and then transferred to a muffle furnace for a second calcination at 720°C under an oxygen atmosphere for 5 hours. After natural cooling, it was passed through a 200-mesh sieve to finally obtain Al / Cu double-doped single crystal NCM83 high-voltage layered cathode material.

[0098] Testing showed that the cathode material obtained in this embodiment had a first-cycle discharge capacity of 215.6 mAh / g at 0.1C within a voltage window of 2.6~4.6V, and a capacity retention rate of 93.3% after 100 cycles at 1C. The discharge capacities at 5C, 10C, and 15C were 164 mAh / g, 134 mAh / g, and 87 mAh / g, respectively. When assembled into a 1.2Ah soft-pack full battery, the capacity retention rate after 200 cycles at 2.6~4.55V was 91.1%, and the battery cell could stably drive the continuous operation of a household robotic vacuum cleaner.

[0099] Example 2

[0100] This embodiment provides an upgrade and regeneration method for waste nickel-rich layered cathode materials. The method uses industrially recycled mixed waste cathode materials, including 30% NCM523, 30% NCM622 and 40% broken black material of failed NCM83 by mass. The above three types of materials are directly mixed as regeneration raw materials without sorting. The specific upgrade and regeneration method is the same as that in Embodiment 1, so it will not be described in detail here.

[0101] The results show that the upgraded regeneration method provided in this embodiment has strong adaptability to mixed and complex waste cathode materials. After regeneration, all materials are transformed into single-crystal structures with a particle size of approximately 2μm and uniform morphology (e.g., Figure 1 The lattice defects and lithium-nickel antisite defects are significantly repaired, and Al and Cu elements are uniformly distributed in the particles. The electrochemical performance is close to that of single NCM83 recycled material. The capacity retention rate after 100 cycles at 4.6V high voltage and 1C is still above 92.5%, and the 15C rate capacity is stable at above 83mAh / g. This proves that the method can directly process mixed and mixed waste cathodes industrially without prior sorting and classification.

[0102] Example 3

[0103] This embodiment provides an upgrade and regeneration method for waste nickel-rich layered cathode materials. The method uses NCM83 cathodes that have failed due to moisture corrosion during storage and cathode sheets of 18650 waste cylindrical batteries disassembled manually in the laboratory as regeneration materials. The specific upgrade and regeneration method is the same as in Embodiment 1, so it will not be described in detail here.

[0104] The results show that after upgrading and regeneration, both types of special failed waste cathodes can completely repair the problems caused by water vapor erosion, such as lattice collapse, severe lithium loss, and surface impurity phase enrichment. Both achieve polycrystalline to monocrystalline morphology transformation and uniform Al / Cu dual-site doping. The high-voltage cycle stability and rate performance are not significantly different from those of normally retired waste cathodes, proving that this method can be adapted to waste cathodes with various extreme failure modes and has a wide range of applicable scenarios.

[0105] Comparative Example 1

[0106] This comparative example provides a method for regenerating waste nickel-rich layered cathode materials. The method uses retired NCM83 waste cathode powder from the same source as in Example 1, supplemented only with an equal amount of LiOH lithium source, without adding NaCl-KCl molten salt system, without introducing waste aluminum / copper current collector dopants, and without using two-stage gradient sintering and secondary roasting; it only uses conventional solid-phase high-temperature sintering at 850℃ for one-time holding in an oxygen atmosphere for 8 hours as a traditional direct regeneration sample.

[0107] Upon observation, the microstructure of the regenerated sample obtained in this comparative example still maintains a polycrystalline secondary particle agglomeration state of about 10 μm, with disordered grain boundaries, a large number of lattice distortions and lithium-nickel antisite defects, and a rock salt phase degradation layer of about 8 nm thick on the surface, without the formation of monocrystalline morphology (such as...). Figure 2 ).

[0108] Testing revealed that the regenerated sample obtained in this comparative example exhibited a first-cycle discharge capacity of only 142.3 mAh / g at 0.1C within a voltage window of 2.6–4.6V, and a capacity retention rate of only 70.2% after 100 cycles at 1C. During high-voltage cycling, significant lattice oxygen precipitation occurred, resulting in severe cell bulging and gas generation. Capacity rapidly declined at rates above 5C, with a discharge capacity of only 19.6 mAh / g at 15C, almost completely losing its fast-charging capability. After cycling, severe particle cracking and pulverization occurred, failing to meet the requirements for high-voltage power batteries and long-cycle energy storage applications, and showing a significant performance gap compared to the cathode material obtained in Example 1.

[0109] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for upgrading and recycling waste and old nickel-rich layered cathode material, characterized in that, The upgrade and regeneration method includes the following steps: (1) Disassemble, grind, sieve and clean the waste nickel-rich layered cathode material to obtain waste cathode powder; (2) Collect scraps of waste aluminum current collectors, crush, grind and sieve to obtain Al doped powder; collect scraps of waste copper current collectors, etch with alkaline solution, wash, dry and grind to obtain Cu(OH)2 doped powder; (3) Prepare a ternary eutectic molten salt of LiOH·H2O-NaCl-KCl as a reaction medium and lithium replenishment source. Mix the waste cathode powder, Al doped powder, Cu(OH)2 doped powder and ternary eutectic molten salt evenly to obtain composite precursor powder. (4) The composite precursor powder is placed in an oxygen atmosphere for segmented heating and sintering. After cooling, it is washed with water to remove salt and then calcined again to obtain a high-voltage single-crystal layered cathode material. Steps (1) and (2) are not in any particular order.

2. The upgrading and regeneration method of the waste and old nickel-rich layered cathode material according to claim 1, characterized in that, The waste nickel-rich layered cathode material mentioned in step (1) includes at least one of NCM523, NCM622, NCM83 or LiCoO2; And / or, the failure types of the waste nickel-rich layered cathode material in step (1) include at least one of the following: electrode breakage and black powder, dismantled waste cylindrical battery cathode, or water vapor erosion failure and scrapped cathode.

3. The upgrading and regeneration method of the waste and old nickel-rich layered cathode material according to claim 1 or 2, characterized in that, The cleaning agent used in step (1) includes a mixed solution of N-methylpyrrolidone and anhydrous ethanol; And / or, after the cleaning described in step (1), the product is dried and sieved; The drying temperature is 55~65℃ and the drying time is 10~14h.

4. The upgrading and regeneration method of the waste and old nickel-rich layered cathode material according to claim 1 or 2, characterized in that, The particle size of the Al-doped powder in step (2) is 10~30 mesh; And / or, the alkaline solution used in step (2) for alkaline etching includes a sodium hydroxide solution with a concentration of 1~3 mol / L; And / or, the immersion time for alkaline etching in step (2) is 30~60 min; And / or, the detergent used in step (2) is deionized water, and the washing endpoint is when the washing liquid is neutral.

5. The method according to claim 1 or 2, wherein the spent nickel-rich layered cathode material is upgraded and regenerated. The molar ratio of LiOH·H2O, NaCl, and KCl in the ternary eutectic molten salt described in step (3) is (1~3):(0.5~1.5):(0.5~1.5); And / or, based on the total molar amount of waste cathode powder, the mixing amount of the Al-doped powder is 2.5 mol% to 3.5 mol%; And / or, based on the total molar amount of waste cathode powder, the mixing amount of the Cu(OH)2 doped powder is 0.8mol%~1.2mol%.

6. The upgrading and regenerating method of the waste and old nickel-rich layered cathode material according to claim 1 or 2, characterized in that, The oxygen purity of the oxygen atmosphere in step (4) is ≥99%; And / or, the segmented heating sintering in step (4) is a two-stage heating sintering, including a first stage heating sintering and a second stage heating sintering.

7. The upgrading and regenerating method of the waste and old nickel-rich layered cathode material according to claim 6, characterized in that, The heating rates for the first and second stages of heating sintering are 4~6℃ / min, respectively. And / or, the target temperature for the first stage of heating and sintering is 480~520℃, and the holding time is 2.5~3.5h; And / or, the target temperature for the second stage of heating and sintering is 830~870℃, and the holding time is 7~9h.

8. The method according to claim 1 or 2, wherein the spent nickel-rich layered cathode material is upgraded and regenerated. Step (4) of water washing and desalination includes soaking in deionized water, stirring, centrifugation, and drying in sequence; The solid-liquid ratio of the deionized water soaking is 1g:(8~12)mL; And / or, the endpoint of the water washing desalination is that no free alkaline ions and chloride ions remain in the washing solution.

9. The method according to claim 1 or 2, wherein the spent nickel-rich layered cathode material is upgraded and regenerated. The secondary calcination in step (4) is carried out in an oxygen atmosphere, wherein the oxygen purity of the oxygen atmosphere is ≥99%; And / or, the temperature of the secondary calcination in step (4) is 700~740℃; And / or, the secondary roasting time in step (4) is 4.5~5.5h.

10. A high-voltage single-crystal layered cathode material prepared by the upcycling method according to any one of claims 1 to 9, characterized in that, The operating voltage of the high-voltage single-crystal layered cathode material is 2.6~4.6V.