Composite membrane for alkaline electrolyzed water and alkaline water electrolyzer comprising same

By designing composite membrane structures with differentiated hydrophilic coating thickness and pore size, the problems of hydrogen and oxygen mixing and insufficient mechanical strength in existing composite membranes during water electrolysis are solved, resulting in lower resistance and higher electrolysis efficiency, reduced costs, and good commercialization potential.

CN221971698UActive Publication Date: 2024-11-08SHANGHAI ENERGY NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202322437086.1
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-09-08
Publication Date
2024-11-08
Estimated Expiration
2033-09-08

AI Technical Summary

Technical Problem

Existing composite membranes have problems in water electrolysis, such as mixing hydrogen and oxygen, difficulty in balancing ion transport capacity and airtightness, insufficient mechanical strength, and high resistance, resulting in high energy consumption and high cost, making it difficult to apply on a large scale.

Method used

A composite membrane structure was designed, including a base membrane and hydrophilic coatings on both sides. The thickness and pore size of the hydrophilic coatings were designed differently. The composite membrane was prepared by combining hydrophilic inorganic particles and polymer resin through a phase inversion method, forming a three- or four-layer composite membrane, thereby optimizing electrolytic performance and mechanical strength.

Benefits of technology

It achieves lower sheet resistance, higher mechanical strength and conductivity, reduces raw material costs, and improves electrolysis efficiency and stability, showing good commercial prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221971698U_ABST
    Figure CN221971698U_ABST
Patent Text Reader

Abstract

The utility model provides a composite membrane for alkaline electrolyzed water and an alkaline water electrolyzer comprising the composite membrane, the composite membrane comprises a base membrane, a plurality of electrode plates and a plurality of electrode plates, the base membrane is of a porous structure; the first hydrophilic coating is formed on one side of the base film; the second hydrophilic coating is formed on the other side, opposite to the first hydrophilic coating, of the base film; wherein the thickness of the first hydrophilic coating is greater than that of the second hydrophilic coating. The composite film provided by the utility model has low surface resistance and high mechanical strength, and the raw material cost can be optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field related to hydrogen production by water electrolysis, and in particular to a composite membrane and a preparation method thereof. Background Art

[0002] The process of water electrolysis for hydrogen production is simple, fully automated, and environmentally friendly. At present, the technology for water electrolysis for hydrogen production is mature at home and abroad, and the equipment has been integrated and serialized. The more representative water electrolysis devices include: solid polymer electrolyte water electrolyzer, solid oxide water electrolyzer and alkaline water electrolyzer.

[0003] The solid polymer electrolyte (SPE) water electrolyzer has a simple structure and uses water as the electrolyte, so it has high efficiency, high safety, stable performance and long life. However, due to the high cost of electrode materials and polymer films, it is still difficult to put into large-scale use.

[0004] Solid Oxide Electrolyzer Cells (SOEC) are composed of a DC power supply, a cathode, an anode and an oxide electrolyte. During electrolysis, electrons enter the cathode from the external circuit and react with water molecules at the cathode to generate H2 and O 2- , hydrogen is collected at the cathode, O 2- The electrons migrate to the anode through the oxide electrolyte, and then they lose electrons to generate O2. Since the solid oxide water electrolyzer electrolyzes water at a high temperature of 600-1000°C, the electrolysis efficiency is very high. However, the high temperature has high requirements for the electrolyzer materials, so the material cost is expensive and it cannot be put into large-scale use in the short term.

[0005] Alkaline water electrolyzer hydrogen production is the most mature water electrolysis hydrogen production device at present. It is widely used in industry because of its simple operation and high efficiency. Alkaline water electrolyzer is mainly composed of electrodes and composite membranes. The electrolyzer is divided into an anode chamber and a cathode chamber, which are separated by a composite membrane. The electrolyzer is filled with electrolyte with good conductivity. Usually 30% to 40% KOH or NaOH solution is used as the electrolyte. During the electrolysis process, the anode produces oxygen and the cathode produces hydrogen. The composite membrane is used to prevent the mixing of hydrogen and oxygen and allow the hydroxide ions in the solution to pass through, ensuring that the electrolysis process continues.

[0006] Traditional diaphragms are made of asbestos. Asbestos has a fibrous structure and is a fiber bundle composed of a mixture of various silicates. It has the characteristics of chemical corrosion resistance, high temperature resistance, high tensile strength, and strong hydrophilicity. However, the swelling property of asbestos, on the one hand, reduces the overall tensile strength of the diaphragm, making the diaphragm easily damaged by the impact of electrolyte and gas. On the other hand, the distribution of electrolyte ions inside the diaphragm after swelling will affect the distribution of current density, increase the resistance of the diaphragm, and increase the energy consumption of electrolysis.

[0007] Polyphenylene Sulfide (PPS) diaphragm is expected to become a new type of diaphragm to replace the traditional asbestos diaphragm. Polyphenylene sulfide has the characteristics of good mechanical properties, resistance to high temperature and high concentration alkali corrosion, and excellent electrical properties. Polyphenylene sulfide diaphragms can be used in alkaline water electrolyzers, but due to the poor hydrophilicity of polyphenylene sulfide, the electrolyte cannot fully enter the pores of the diaphragm. During the electrolysis process, tiny bubbles will gather on the surface of the diaphragm. These phenomena will increase the resistance of the diaphragm and lead to increased energy consumption. The poor solubility of polyphenylene sulfide also limits the method of preparing diaphragms from polyphenylene sulfide. Some scholars melt-spin polyphenylene sulfide resin and then weave it to obtain a polyphenylene sulfide braided diaphragm. This method can well overcome the poor solubility of polyphenylene sulfide. Improve the hydrophilicity of polyphenylene sulfide diaphragms.

[0008] Polysulfone (PSF) is a polymer compound with phenylene sulfone as a structural unit. It is a thermoplastic resin with the advantages of strong oxidation resistance, strong acid and alkali corrosion resistance, good solubility, and simple and convenient production. Various existing membrane-making processes are suitable for the preparation of polysulfone diaphragms. However, polysulfone diaphragms have poor hydrophilicity. During the water electrolysis process, tiny bubbles of hydrogen and oxygen tend to gather on the surface of the diaphragm, affecting the flow of the electrolyte and reducing the current efficiency. The poor hydrophilicity of polysulfone diaphragms greatly reduces the performance of the diaphragms. Therefore, if the hydrophilicity of polysulfone diaphragms can be enhanced through effective means, polysulfone diaphragms will have more superior application prospects in the field of water electrolysis diaphragms.

[0009] Phase inversion is the most widely used film making method in the field of film making. The main purpose of the phase inversion film making process is to form a polymer-rich phase and a polymer-poor phase, and to separate the polymer-rich phase and the polymer-poor phase under a specific environment, and the polymer-rich phase solidifies into a film. According to the different phase separation process methods, it is divided into thermal induced precipitation phase separation method, solvent evaporation precipitation phase separation method, gas phase precipitation phase separation method and immersion precipitation phase separation method. Among them, the immersion precipitation phase separation method is the most widely used and relatively mature film making method in the field of film making. In the immersion precipitation phase inversion film making process, the polymer solution is first placed on a specific mold by coating or casting, and then the mold is placed in a non-solvent. In the process of mutual exchange of the solvent and non-solvent of the polymer solution, a polymer-rich phase is gradually formed, and finally solidified into a film. During the operation, by controlling the influencing factors at different stages such as polymer concentration, pre-evaporation time, non-solvent (also known as coagulation bath) temperature, etc., membrane materials with different structures and properties can be obtained.

[0010] The main structure of the current composite membrane is a three-layer structure. The two hydrophilic layers have the same thickness and the same average pore size. This composite membrane with uniform pores on both sides is prone to mixing of hydrogen and oxygen in alkaline water electrolysis applications. Its ion transmission capacity and air tightness cannot be taken into account, which increases the resistance of the composite membrane.

[0011] In addition, since the composite membrane must withstand the impact of electrolyte and generated gas for a long time, it requires high mechanical strength, and the composite membrane must be able to maintain chemical stability under electrolysis temperature and alkaline conditions. Generally, in order to effectively separate the gas generated by the anode and cathode while conducting ions, the thickness of the composite membrane is relatively thick, usually above 500μm. However, as the coating thickness increases, the surface resistance will also increase, and since the main component of the coating is inorganic material, the increase in thickness will also reduce the mechanical strength of the composite membrane. Utility Model Content

[0012] The utility model aims to provide a composite membrane, characterized in that it comprises: a base membrane, which is a porous structure; a first hydrophilic coating, which is formed on one side of the base membrane; and a second hydrophilic coating, which is formed on the other side of the base membrane relative to the first hydrophilic coating; wherein the thickness of the first hydrophilic coating is greater than the thickness of the second hydrophilic coating.

[0013] Preferably, the average pore size of the first hydrophilic coating is less than or equal to the average pore size of the second hydrophilic coating.

[0014] Preferably, the thickness of the composite film is less than 500 μm; and / or the thickness of the base film is 150 to 200 μm; and / or the thickness of the first hydrophilic coating is 100 to 180 μm; and / or the thickness of the second hydrophilic coating is 20 to 110 μm.

[0015] Preferably, the porous structure of the base membrane is filled with hydrophilic inorganic particles with a particle size of 120 nm to 500 nm and / or a particle size of 40 nm to 100 nm.

[0016] Preferably, the first hydrophilic coating comprises an upper hydrophilic coating and a lower hydrophilic coating, wherein the lower hydrophilic coating is located between the base film and the upper hydrophilic coating, wherein the thickness of the upper hydrophilic coating is greater than that of the lower hydrophilic coating.

[0017] Preferably, the average pore size of the second hydrophilic layer is equal to the average pore size of the lower hydrophilic coating layer, and / or the average pore size of the second hydrophilic layer is greater than or equal to the average pore size of the upper hydrophilic coating layer.

[0018] Preferably, the thickness of the composite membrane is less than 500 μm; and / or the thickness of the base membrane is 120 to 230 μm; and / or the thickness of the first hydrophilic coating is 100 to 160 μm; and / or the thickness of the second hydrophilic coating is 20 to 100 μm; and / or the thickness of the upper hydrophilic coating is 60 to 100 μm; and / or the thickness of the lower hydrophilic coating is 20 to 100 μm.

[0019] Preferably, the first hydrophilic coating layer and the second hydrophilic coating layer include hydrophilic inorganic particles with a particle size of 120 nm to 500 nm and / or a particle size of 40 nm to 100 nm.

[0020] The utility model further proposes an alkaline water electrolysis cell, characterized in that it comprises: a cathode, an anode, and the composite membrane described above, wherein the first hydrophilic coating is connected to the cathode, and the second hydrophilic coating is connected to the anode. The utility model further proposes an alkaline water electrolysis cell, characterized in that it comprises: a cathode, an anode, and the composite membrane described above, wherein the upper hydrophilic coating is connected to the cathode, and the second hydrophilic coating is connected to the anode.

[0021] The composite membrane proposed by the utility model is composed of two hydrophilic coatings coated on both sides of the base membrane, and the two hydrophilic coatings and the base membrane form a three-layer structure. By reducing the thickness of the anode hydrophilic coating and maintaining or increasing the thickness of the cathode coating, it has lower surface resistance, higher conductivity, and higher mechanical strength than the existing diaphragm, and can effectively save the coating slurry, and can reduce the cost of raw materials while ensuring the power density of the composite membrane.

[0022] The utility model further proposes another composite film, wherein one side of the base film has a hydrophilic coating, and the other side of the base film has two hydrophilic coatings. During the initial coating, a three-layer sandwich structure of the hydrophilic coating, the base film, and the hydrophilic coating is formed, and the two hydrophilic coatings fix the base film in the middle, and then another hydrophilic coating is coated on the outside of one of the hydrophilic coatings for a second time to increase the gas barrier property of the composite film.

[0023] The composite membrane proposed by the utility model has different average pore sizes of the hydrophilic layers on both sides of the base membrane. When water electrolysis is performed, placing the hydrophilic coating with a small pore structure of the composite membrane close to the cathode side can effectively improve the electrolysis performance of the composite membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a structural schematic diagram showing the longitudinal section structure of a composite membrane of the present invention.

[0025] Figure 2 It is a structural schematic diagram showing the longitudinal section structure of another form of the composite membrane of the utility model.

[0026] Figure 3 It is a schematic diagram showing the structure of an alkaline water electrolysis cell. DETAILED DESCRIPTION

[0027] The following is a detailed description of the specific implementation of the present invention in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0028] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0029] Please refer to Figure 1 , presents a composite membrane 10 according to an embodiment of the present invention in a longitudinal cross-section. The composite membrane 10 comprises a base membrane 1, a first hydrophilic coating 2, and a second hydrophilic coating 3. The first hydrophilic coating 2 is formed on one side of the base membrane 1, and the second hydrophilic coating 3 is formed on the other side of the base membrane 1 relative to the first hydrophilic coating 2. The base membrane 1, the first hydrophilic coating 2, and the second hydrophilic coating 3 form a sandwich structure, and the thickness of the first hydrophilic coating 2 is greater than the thickness of the second hydrophilic coating 3.

[0030] The base film 1 is located between the first hydrophilic coating 2 and the second hydrophilic coating 3 and is a porous structure. In a preferred embodiment, the base film 1 is a porous structure with a mesh size of 60 and / or a wire diameter of 110 μm. In another preferred embodiment, the base film 1 is polyphenylene sulfide (PPS), which has good mechanical properties, high temperature and high concentration alkali corrosion resistance, and excellent electrical properties. The first hydrophilic coating 2 and the second hydrophilic coating 3 are composed of a hydrophilic material and a binder and are hydrophilic coatings. Preferably, the average pore size of the first hydrophilic coating 2 is less than or equal to the average pore size of the second hydrophilic coating 3.

[0031] When the composite membrane 10 is placed in an alkaline water electrolysis cell, the first hydrophilic coating 2 faces the cathode, and the second hydrophilic coating 3 faces the anode.

[0032] In a preferred embodiment, the thickness of the composite film 10 is less than 500 μm, and in a preferred embodiment, the thickness of the composite film 10 is less than or equal to 400 μm. Preferably, the thickness of the base film 1 is 150 to 200 μm, the thickness of the first hydrophilic coating 2 is 100 to 180 μm, and the thickness of the second hydrophilic coating 3 is 20 to 110 μm. In a preferred embodiment, the thickness of the first hydrophilic coating 2 is 110 to 150 μm, and the thickness of the second hydrophilic coating 3 is 40 to 80 μm.

[0033] The first hydrophilic coating 2 and the second hydrophilic coating 3 include a plurality of hydrophilic inorganic particles, and the pores of the base membrane 1 are also filled with a plurality of hydrophilic inorganic particles. Preferably, the hydrophilic inorganic particles can be zirconium oxide with a particle size of 120 to 500 nm or a particle size of 40 to 100 nm. The hydrophilic inorganic particles can increase the hydrophilicity, improve the interface effect between porous materials and improve the ion transmission capacity. Preferably, the particle size of zirconium oxide is not less than 1 / 20 of the pore size of the base membrane 1 to avoid the zirconium dioxide from falling off during terminal application, so that the composite membrane 10 has better electrochemical properties while ensuring its stability in long-term use.

[0034] In a preferred embodiment, a pore-forming agent may be added to the slurry when forming the first hydrophilic coating 2 and the second hydrophilic coating 3. The pore-forming agent is polyvinyl pyrrolidone (PVP) with a weight average molecular weight of 400,000 to 650,000. In another preferred embodiment, the PVP content does not exceed 10% of the mass of the inorganic particles.

[0035] In a preferred embodiment, please refer to Figure 2 The first hydrophilic coating 2 can be divided into an upper hydrophilic coating 21 and a lower hydrophilic coating 22, and the lower hydrophilic coating 22 is located between the base film 1 and the upper hydrophilic coating 21. The thickness of the upper hydrophilic coating 21 is greater than or equal to the thickness of the lower hydrophilic coating 22. The average pore size of the upper hydrophilic coating 21 is less than or equal to the average pore size of the lower hydrophilic coating 22, and / or the average pore size of the lower hydrophilic coating 22 is equal to the average pore size of the second hydrophilic coating 3.

[0036] Preferably, the thickness of the composite film 10 is less than 500 μm. In a preferred embodiment, the thickness of the composite film 10 is less than or equal to 400 μm. Preferably, the thickness of the base film 1 is 120 to 230 μm, the thickness of the first hydrophilic coating 2 is 100 to 160 μm, and the thickness of the second hydrophilic coating 3 is 20 to 100 μm. In a preferred embodiment, the thickness of the first hydrophilic coating 2 is 110 to 150 μm, and the thickness of the second hydrophilic coating 3 is 40 to 60 μm. Preferably, the surface resistance of the composite film is less than 0.5 Ω*cm 2 , the mechanical strength is greater than 25MPa. In a preferred embodiment, the composite film surface resistance is less than or equal to 0.3Ω*cm 2 , mechanical strength is greater than or equal to 28Mpa.

[0037] When preparing the slurry, the polymer resin used is polysulfone, preferably, the polymer resin is polyethersulfone with a molecular weight of 30,000 to 50,000. When preparing the slurry, preferably, the solvent used is N-ethyl-2-pyrrolidone (NEP) with a purity of 99%.

[0038] The following is an example of a method for preparing a composite membrane according to an embodiment of the present invention.

[0039] First, prepare the slurry. In a dry room with a humidity of 10% or less, first dissolve the polysulfone resin in the solvent and stir at a constant speed for 5 to 10 hours until the solution becomes uniform and transparent, then add PVP and stir for 0.5 to 1 hour until the PVP is completely dissolved, and finally slowly pour a certain amount of zirconium oxide into the above solution and stir for 2 to 8 hours to make the solution form a milky white and uniform casting slurry to obtain the slurry.

[0040] Next, the slurry is degassed by stirring the slurry at 1,000 to 2,000 rpm for 10 to 20 minutes.

[0041] The completed slurry is coated on one side of the base film 1 to form a first hydrophilic coating 2. Preferably, the wet film thickness of the first hydrophilic coating 2 is 500 to 750 μm.

[0042] The other side of the base film 1 relative to the first hydrophilic coating 2 is placed in the slurry, and the base film is pressed with external force to fill the slurry into the pores of the base film 1 to form the second hydrophilic coating 3. Preferably, the thickness of the second hydrophilic coating 3 is 50 to 250 μm.

[0043] Next, the composite film 10 coated with the first hydrophilic coating 2 and the second hydrophilic coating 3 is placed in the air for 15 seconds to 2 minutes for pre-evaporation.

[0044] Next, the composite membrane 10 is subjected to a coprecipitation process. The composite membrane 10 is placed in non-solvent phase water, ethanol or water and solvent for 20 to 40 minutes for phase conversion. After the exchange of solvent and non-solvent is completed, the composite membrane 10 is placed in non-solvent phase water for 30 to 60 minutes. Finally, the composite membrane 10 is naturally air-dried or maintained at a certain humidity for standby use. Since the surface tension of ethanol is smaller than that of water, the coprecipitation process is slower, so the pore size formed on the first hydrophilic coating 2 and the second hydrophilic coating 3 will be more uniform. Because the process of coprecipitation using ethanol takes a long time, after the pore size is uniform, the composite membrane 10 needs to be placed in water again to speed up the solvent exchange so that more PVP and solvent are exchanged.

[0045] In another state, when preparing the slurry, the polysulfone resin is first dissolved in the solvent and stirred at a uniform speed for 5 to 10 hours until the solution becomes uniform and transparent, and then the above solution is divided into two parts, and different masses of PVP are added respectively, and stirred for 0.5 to 1 hour respectively until the PVP is completely dissolved. Finally, a certain mass of zirconium oxide is slowly poured into the above two solutions, and stirred for 2 to 8 hours respectively, so that the solution forms a milky white and uniform casting slurry, and a first hydrophilic coating slurry and a second hydrophilic coating slurry containing different masses of PVP are obtained.

[0046] The completed first hydrophilic coating slurry is coated on the base film 1 by slit extrusion, so that the first hydrophilic coating slurry completely covers the base film 1, forming a lower hydrophilic coating 22 and a second hydrophilic layer 3. Preferably, the wet film thickness of the lower hydrophilic coating 22 and the second hydrophilic layer 3 is 500 to 800 μm. In another state, the slit extrusion can be repeated when coating the lower hydrophilic coating 22 and the second hydrophilic layer 3 until the wet film thickness is uniform.

[0047] The second hydrophilic coating slurry is coated on the lower hydrophilic coating 22 by slot extrusion to form an upper hydrophilic coating 21, so that the upper hydrophilic coating 21 and the lower hydrophilic coating 22 together form the first hydrophilic coating 2. Preferably, the wet film thickness of the upper hydrophilic coating 21 is 40 to 200 μm.

[0048] Finally, after the same pre-evaporation and co-precipitation processes, the composite membrane is naturally air-dried or maintained at a certain humidity for standby use.

[0049] Please refer to Figure 3 The composite membrane 10 described above can be installed in an alkaline water electrolyzer. The alkaline water electrolyzer includes a cathode 30 and an anode 31, and the outer sides of the cathode 30 and the anode 31 also have a gasket 32, a polar plate 33 and an end plate 34. The cathode 30 in the electrolyzer is connected to the upper hydrophilic coating 21 in the first hydrophilic coating 2, and the anode 31 is connected to the second hydrophilic coating 3.

[0050] The following examples are used to illustrate the method for preparing the composite film with a three-layer structure in the present invention.

[0051] Embodiment 1:

[0052] 1. Slurry preparation. Slurry preparation was performed in a drying room with a humidity of no more than 5%. First, 5 g of polysulfone was added to 28 g of solvent, and after fully dissolved, 1 g of PVP with a weight average molecular weight of 50,000 was added and stirred for 30 minutes, and finally 20 g of zirconium dioxide with a primary particle size of 150 nm was added and stirred at 750 rpm for 4 hours.

[0053] 2. Degassing the slurry: Stir at 2,000 rpm to degas the slurry for 15 minutes and then let it stand for use.

[0054] 3. Applying the first hydrophilic coating: Apply the slurry on the base film to obtain a wet film with a thickness of 700 μm.

[0055] 4. Apply the second hydrophilic coating layer: Place a base film with a mesh size of 60 and / or a wire diameter of 110 μm in the slurry, press the base film in with external force, and apply the slurry on the base film to obtain a second hydrophilic coating layer with a thickness of 100 μm.

[0056] 5. Perform a pre-evaporation process and let the composite film stand for 1 minute.

[0057] 6. Carry out the coprecipitation process, prepare a solution with a ratio of 1:1 between water and solvent as a coagulation bath, and put the composite membrane with double-sided wet film into the coagulation bath for 20 minutes. After exchanging with the solvent, put the composite membrane into water for 30 minutes. Finally, let the composite membrane dry naturally and then conduct performance test.

[0058] Embodiment 2:

[0059] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 5%. First, add 5g of polysulfone to 28g of solvent and fully dissolve it, and divide the solution containing polysulfone into two parts. Add 0.5g of PVP with a molecular weight of 50,000 to the first solution, stir for 30 minutes, then add 10g of zirconium dioxide with a primary particle size of 150nm, and stir at 750rpm for 4 hours to obtain the first hydrophilic coating slurry. Add 0.5g of PVP with a molecular weight of 50,0000 to the other solution, stir for 30 minutes, then add 10g of zirconium dioxide, and stir at 750rpm for 4 hours to obtain the second hydrophilic coating slurry.

[0060] 2. Degassing the slurry: Stir at 2,000 rpm to degas the slurry for 15 minutes and then let it stand for use.

[0061] 3. Apply the first hydrophilic coating, apply the slurry on the base film to obtain a wet film with a thickness of 700 μm.

[0062] 4. Apply the second hydrophilic coating, place a base film with a mesh size of 60 and / or a wire diameter of 110 μm in the slurry, press the base film with external force, and apply the slurry on the base film to obtain a second hydrophilic coating with a thickness of 100 μm.

[0063] 5. Perform a pre-evaporation process and let the composite film stand for 1 minute.

[0064] Sixth, the coprecipitation process is carried out, and a solution with a ratio of 1:1 between water and solvent is prepared as a coagulation bath, and the composite membrane coated with wet film on both sides is placed in the coagulation bath for 20 minutes. After exchanging with the solvent, the composite membrane is placed in water for 30 minutes. Finally, the composite membrane is naturally air-dried and then the performance is tested.

[0065] Embodiment 3:

[0066] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 5%. First, add 5g of polysulfone to 28g of solvent and fully dissolve it, and divide the solution containing polysulfone into two parts. Add 0.75g of PVP with a molecular weight of 50,000 to the first solution, stir for 30 minutes, then add 10g of zirconium oxide with a primary particle size of 150nm, and stir at 750rpm for 4 hours to obtain the first hydrophilic coating slurry. Add 0.75g of PVP with a molecular weight of 50,0000 to the other solution, stir for 30 minutes, then add 10g of zirconium dioxide, and stir at 750rpm for 4 hours to obtain the second hydrophilic coating slurry.

[0067] 2. Degassing the slurry: Stir at 2,000 rpm to degas the slurry for 15 minutes and then let it stand for use.

[0068] 3. Applying the first hydrophilic coating: Apply the slurry on the base film to obtain a wet film with a thickness of 700 μm.

[0069] 4. Apply the second hydrophilic coating layer: Place a base film with a mesh size of 60 and / or a wire diameter of 110 μm in the slurry, press the base film in with external force, and apply the slurry on the base film to obtain a second hydrophilic coating layer with a thickness of 100 μm.

[0070] 5. Perform a pre-evaporation process and let the composite film stand for 1 minute.

[0071] 6. Carry out the coprecipitation process. Prepare a solution with a water-solvent ratio of 1:1 as a coagulation bath, and place the composite membrane with double-sided wet film in the coagulation bath for 20 minutes. After exchanging with the solvent, place the composite membrane in water for 30 minutes. Finally, let the composite membrane air dry naturally and then conduct performance test.

[0072] Comparative Example 1:

[0073] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 5%. First, add 5g of polysulfone to 28g of solvent and fully dissolve it, and divide the solution containing polysulfone into two parts. Add 0.75g of PVP with a molecular weight of 50,000 to the first solution, stir for 30 minutes, then add 10g of zirconium dioxide, and stir at 750rpm for 4 hours to obtain the first hydrophilic coating slurry. Add 0.75g of PVP with a molecular weight of 500,000 to the other solution, stir for 30 minutes, then add 10g of zirconium dioxide, and stir at 750rpm for 4 hours to obtain the second hydrophilic coating slurry.

[0074] 2. Degas the slurry by stirring at 2,000 rpm for 15 minutes and then letting it stand for use.

[0075] 3. Apply the first hydrophilic coating, apply the slurry on the base film to obtain a wet film with a thickness of 500 μm.

[0076] 4. Apply the second hydrophilic coating, place a base film with a mesh size of 60 and / or a wire diameter of 110 μm in the slurry, press the base film with external force, and apply the slurry on the base film to obtain a second hydrophilic coating with a thickness of 300 μm.

[0077] 5. Perform a pre-evaporation process and let the composite film stand for 1 minute.

[0078] Sixth, the coprecipitation process is carried out, and a solution with a ratio of 1:1 between water and solvent is prepared as a coagulation bath, and the composite membrane coated with wet film on both sides is placed in the coagulation bath for 20 minutes. After exchanging with the solvent, the composite membrane is placed in water for 30 minutes. Finally, the composite membrane is naturally air-dried and then the performance is tested.

[0079] Comparative Example 2:

[0080] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 5%. First, add 5g of polysulfone to 28g of solvent and fully dissolve it, and divide the solution containing polysulfone into two parts. Add 0.75g of PVP with a molecular weight of 500,000 to the first solution, stir for 30 minutes, then add 10g of zirconium dioxide, stir at 750rpm for 4 hours to obtain the first hydrophilic coating slurry. Add 0.75g of PVP with a molecular weight of 50,000 to the other solution, stir for 30 minutes, then add 10g of zirconium dioxide, stir at 750rpm for 4 hours to obtain the second hydrophilic coating slurry.

[0081] 2. Degassing the slurry: Stir at 2,000 rpm to degas the slurry for 15 minutes and then let it stand for use.

[0082] 3. Apply the first hydrophilic coating, apply the slurry on the base film to obtain a wet film with a thickness of 700 μm.

[0083] 4. Apply the second hydrophilic coating, place a base film with a mesh size of 60 and / or a wire diameter of 110 μm in the slurry, press the base film with external force, and apply the slurry on the base film to obtain a second hydrophilic coating with a thickness of 100 μm.

[0084] 5. Perform a pre-evaporation process and let the composite film stand for 1 minute.

[0085] Sixth, the coprecipitation process is carried out, and a solution with a ratio of 1:1 between water and solvent is prepared as a coagulation bath, and the composite membrane coated with wet film on both sides is placed in the coagulation bath for 20 minutes. After exchanging with the solvent, the composite membrane is placed in water for 30 minutes. Finally, the composite membrane is naturally air-dried and then the performance is tested.

[0086] Comparative Example 3:

[0087] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 5%. First, add 5g of polysulfone to 28g of solvent and fully dissolve it, and divide the solution containing polysulfone into two parts. Add 2g of PVP with a molecular weight of 50,000 to the first solution, stir for 30 minutes, then add 10g of zirconium dioxide, and stir at 750rpm for 4 hours to obtain the first hydrophilic coating slurry. Add 2g of PVP with a molecular weight of 500,000 to the other solution, stir for 30 minutes, then add 10g of zirconium dioxide, and stir at 750rpm for 4 hours to obtain the second hydrophilic coating slurry.

[0088] 2. Degassing the slurry: Stir at 2,000 rpm to degas the slurry for 15 minutes and then let it stand for use.

[0089] 3. Applying the first hydrophilic coating: Apply the slurry on the base film to obtain a wet film with a thickness of 700 μm.

[0090] 4. Apply the second hydrophilic coating layer: Place a base film with a mesh size of 60 and / or a wire diameter of 110 μm in the slurry, press the base film in with external force, and apply the slurry on the base film to obtain a second hydrophilic coating layer with a thickness of 100 μm.

[0091] 5. Perform a pre-evaporation process and let the composite film stand for 1 minute.

[0092] 6. Carry out the coprecipitation process. A solution with a water-solvent ratio of 1:1 is used as a coagulation bath, and the composite membrane coated with a wet film on both sides is placed in the coagulation bath for 20 minutes. After exchanging with the solvent, the composite membrane is placed in water for 30 minutes. Finally, the composite membrane is naturally air-dried and then the performance is tested.

[0093] The composite membrane test method is described as follows:

[0094] a. Ionic conductivity:

[0095] Take a composite membrane of a certain thickness of 2.5x2.5cm (the test area is a circle with a diameter of 2cm), soak it in ethanol for 2 hours, and vibrate it with ultrasound for 5 minutes, then soak it in 3M potassium hydroxide solvent for 24 hours, and then move it to a stainless steel test chamber for testing. Use an electrochemical workstation to obtain the impedance spectrum of the composite membrane, take the intersection of the high-frequency part of the spectrum line and the real axis as the impedance value, and convert it into ionic conductivity.

[0096] b. Mechanical properties:

[0097] At a constant temperature of 25°C, the composite film was cut into sample strips of 1x6 cm, placed in an experimental fixture and clamped vertically, stretched at a speed of 50 mm / min until it broke, and the tensile strength was read.

[0098] c. Alkaline electrolyzed water test:

[0099] Active area 15cm 2 The LSCF single stack is used as the electrolyzer, and the composite membrane is placed in the electrolyzer. 30% KOH is used as the electrolyte, and the DC power supply is used at 80°C, with the cell voltage ranging from 1.5 to 2.0V. The voltammetric curve of the composite membrane is tested at a step size of 0.05V, and the power of the system at 1.8V is calculated.

[0100] In order to clearly compare the characteristics of all the above examples, all test results are summarized in Table 1. The competitive diaphragm used is Zirfon UTP500 from AGFA, Belgium.

[0101] Table 1

[0102]

[0103] Please refer to Table 1. According to the comparison between Examples 1 and 2, when the thickness of the first hydrophilic coating connected to the cathode is greater than the thickness of the second hydrophilic coating connected to the anode, increasing the pore size of the second hydrophilic coating will increase the ionic conductivity and the power at 1.8V, while the tensile strength will decrease. According to the comparison between Examples 2 and 3, increasing the content of PVP in the first hydrophilic coating slurry and the second hydrophilic coating slurry will increase the ionic conductivity and the power at 1.8V, while the tensile strength will decrease.

[0104] According to the comparison between Example 2 and Comparative Example 1, when the thickness of the second hydrophilic coating connected to the anode is greater than the thickness of the first hydrophilic coating connected to the cathode, although the ionic conductivity is improved, the tensile strength and the power at 1.8V are both reduced. According to the comparison between Example 1 and Comparative Example 2, increasing the pore size of the first hydrophilic coating can improve the ionic conductivity, but the tensile strength and the power at 1.8V are both reduced. According to the comparison between Example 3 and Comparative Example 3, when the PVP content of the first hydrophilic coating slurry and the second hydrophilic coating slurry is increased from 0.75g to 2g, the ionic conductivity is increased from 157mS / cm to 169mS / cm, but the tensile strength is reduced from 29.1Mpa to 20.5Mpa, and the power at 1.8V is reduced from 0.96W / cm 2 Down to 0.75W / cm 2 .

[0105] According to the comparison between Examples 1 to 3 and the composite membranes of competing products, it can be seen that the composite membrane proposed by the present invention is thinner in thickness, and is superior to the composite membranes of competing products in terms of ionic conductivity, tensile strength, and power at 1.8V, and has good commercial prospects.

[0106] The following examples are used to illustrate the method for preparing the composite membrane with a four-layer structure in the present invention.

[0107] Embodiment 4:

[0108] 1. Slurry preparation. The slurry is prepared in a drying room with a humidity not higher than 10%. First, add 4.9g of polysulfone resin to 25g of solvent and stir at a uniform speed for 8 hours until the solution is uniform and transparent. Divide the above solution into two parts, add 1g of PVP and 0.5g of PVP respectively, stir for 0.5 hours respectively until the PVP is completely dissolved, and finally slowly pour 19.6g of zirconium oxide (large-particle zirconium oxide and small-particle zirconium oxide are mixed in a 1:1 ratio) into the above two solutions respectively, and stir for 4 hours respectively, so that the solution forms a milky white and uniform casting slurry, and obtains the first hydrophilic coating slurry and the second hydrophilic coating slurry dissolved with different PVP masses.

[0109] 2. Degas the slurry. Stir at 2,000 rpm, centrifuge the slurry to degas for 15 minutes, and then let it stand for use.

[0110] 3. Apply the second hydrophilic coating 3 and the lower hydrophilic coating 22, and apply the completed first hydrophilic coating slurry on the base film 1 by slit extrusion, so that the first hydrophilic coating slurry completely covers the base film 1, and obtain the lower hydrophilic coating 22 and the second hydrophilic layer 3 with a wet film thickness of 700 μm.

[0111] Fourth, coating the upper hydrophilic coating 21, coating the second hydrophilic coating slurry on the lower hydrophilic coating 22 by slit extrusion method, to form the upper hydrophilic coating 21 with a wet film thickness of 100 μm.

[0112] 5. Perform pre-evaporation and place the composite film in the air for 15 seconds.

[0113] Sixth, co-precipitation is performed, the composite membrane 10 is placed in non-solvent phase water, ethanol or water and solvent for 20 minutes for phase conversion, after the solvent and non-solvent exchange is completed, the composite membrane 10 is placed in non-solvent phase water for 30 minutes. Finally, the membrane is naturally air-dried or kept at a certain humidity for standby use.

[0114] Embodiment 5:

[0115] 1. Slurry preparation. The slurry is prepared in a drying room with a humidity not higher than 10%. First, add 4.9g of polysulfone resin to 25g of solvent and stir at a uniform speed for 8 hours until the solution is uniform and transparent. Divide the above solution into two parts, add 1g of PVP and 0.5g of PVP respectively, stir for 0.5 hours respectively until the PVP is completely dissolved, and finally slowly pour 19.6g of zirconium oxide (large-particle zirconium oxide and small-particle zirconium oxide are mixed in a 1:1 ratio) into the above two solutions respectively, and stir for 4 hours respectively, so that the solution forms a milky white and uniform casting slurry, and obtains the first hydrophilic coating slurry and the second hydrophilic coating slurry dissolved with different PVP masses.

[0116] 2. Degas the slurry. Stir at 2,000 rpm, centrifuge the slurry to degas for 15 minutes, and then let it stand for use.

[0117] 3. Apply the second hydrophilic coating 3 and the lower hydrophilic coating 22, and apply the completed second hydrophilic coating slurry on the base film 1 by slit extrusion, so that the second hydrophilic coating slurry completely covers the base film 1, and obtain the lower hydrophilic coating 22 and the second hydrophilic layer 3 with a wet film thickness of 700 μm.

[0118] Fourth, coating the upper hydrophilic coating 21, coating the first hydrophilic coating slurry on the lower hydrophilic coating 22 by slit extrusion method, to form the upper hydrophilic coating 21 with a wet film thickness of 100 μm.

[0119] 5. Perform pre-evaporation and place the composite film in the air for 15 seconds.

[0120] Sixth, co-precipitation is performed, the composite membrane 10 is placed in non-solvent phase water, ethanol or water and solvent for 20 minutes for phase conversion, after the solvent and non-solvent exchange is completed, the composite membrane 10 is placed in non-solvent phase water for 30 minutes. Finally, the membrane is naturally air-dried or kept at a certain humidity for standby use.

[0121] Comparative Example 4:

[0122] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 10%. First, add 4.9g of polysulfone resin to 25g of solvent and stir at a uniform speed for 8 hours until the solution is uniform and transparent. Add 1g of PVP and stir for 0.5 hours until the PVP is completely dissolved. Finally, slowly pour 19.6g of zirconium oxide (large-particle zirconium oxide and small-particle zirconium oxide are mixed in a 1:1 ratio) into the above solution and stir for 4 hours to form a milky white and uniform casting slurry.

[0123] 2. Degas the slurry. Stir at 2,000 rpm, centrifuge the slurry to degas for 15 minutes, and then let it stand for use.

[0124] 3. Apply the first hydrophilic coating 2 and the second hydrophilic coating 3, and apply the completed slurry on the base film 1 by slit extrusion so that the slurry completely covers the base film 1, thereby obtaining the first hydrophilic coating 2 and the second hydrophilic coating 3 with a wet film thickness of 800 μm.

[0125] 4. Perform pre-evaporation and place the composite film in the air for 15 seconds.

[0126] Fifth, coprecipitation is performed, the composite membrane 10 is placed in non-solvent phase water, ethanol or water and solvent for 20 minutes for phase conversion, after the solvent and non-solvent exchange is completed, the composite membrane 10 is placed in non-solvent phase water for 30 minutes. Finally, the membrane is naturally air-dried or kept at a certain humidity for standby use.

[0127] Comparative Example 5:

[0128] The preparation method and steps are the same as those of Example 4, except that when conducting the water electrolysis performance test, the first hydrophilic coating 2 of the composite membrane 10 is placed close to the anode and the second hydrophilic coating 3 is placed close to the cathode.

[0129] Comparative Example 6:

[0130] 1. Slurry preparation. Slurry preparation is carried out in a drying room with a humidity not higher than 10%. First, add 4.9g of polysulfone resin to 25g of solvent and stir at a uniform speed for 8 hours until the solution is uniform and transparent. Add 1g of PVP and stir for 0.5 hours until the PVP is completely dissolved. Finally, slowly pour 19.6g of zirconium oxide (large-particle zirconium oxide and small-particle zirconium oxide are mixed in a 1:1 ratio) into the above solution and stir for 4 hours to form a milky white and uniform casting slurry.

[0131] 2. Degas the slurry. Stir at 2,000 rpm, centrifuge the slurry to degas for 15 minutes, and then let it stand for use.

[0132] 3. Applying the lower hydrophilic coating layer 22 and the second hydrophilic coating layer 3, applying the completed slurry on the base film 1 by slit extrusion, so that the slurry completely covers the base film 1, forming the lower hydrophilic coating layer 22 and the second hydrophilic coating layer 3.

[0133] Fourth, coating the upper hydrophilic coating 21 , coating the slurry on the lower hydrophilic coating 22 by slit extrusion to form the upper hydrophilic coating 21 .

[0134] 5. Perform pre-evaporation and place the composite film in the air for 15 seconds.

[0135] Sixth, co-precipitation is performed, the composite membrane 10 is placed in non-solvent phase water, ethanol or water and solvent for 20 minutes for phase conversion, after the solvent and non-solvent exchange is completed, the composite membrane 10 is placed in non-solvent phase water for 30 minutes. Finally, the membrane is naturally air-dried or kept at a certain humidity for standby use.

[0136] In order to clearly compare the characteristics of all the above examples, all test results are summarized in Table 1, and the competitive diaphragm used is Zirfon.

[0137] Table 2

[0138]

[0139] Please refer to Table 2, wherein the rightmost column of Table 2 represents the current density measured at a voltage of 1.8 V. According to the comparison between Examples 4 and 5, when the pore size of the upper hydrophilic coating is larger than the pore size of the lower hydrophilic coating and the second hydrophilic coating, the conductivity and electrolytic performance decrease, while the tensile strength increases.

[0140] According to the comparison between Example 4 and Comparative Examples 4 and 6, when the first hydrophilic coating 2 and the second hydrophilic coating 3 have the same pore size, the conductivity is high, and the tensile strength and electrolytic performance are reduced. According to the comparison between Example 4 and Comparative Example 5, if the directions of the first hydrophilic coating 2 and the second hydrophilic coating 3 of the composite membrane 10 are reversed during electrolysis, the conductivity and electrolytic performance will both decrease.

[0141] According to the comparison between Examples 4 and 5 and competing membranes, the composite membrane proposed by the present invention is thinner in thickness, and is superior to competing membranes in electrical conductivity, tensile strength and electrolytic performance, and has good commercial prospects.

[0142] The above contents involving common knowledge are not described in detail, and those skilled in the art can understand them.

[0143] The above descriptions are only some specific embodiments of the utility model and are not intended to limit the utility model. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the utility model shall be included in the protection scope of the utility model. The technical scope of this utility model is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A composite membrane for alkaline water electrolysis, It is characterized in that Include: A basement membrane having a porous structure; A first hydrophilic coating layer formed on one side of the base film; as well as a second hydrophilic coating layer formed on the other side of the base film relative to the first hydrophilic coating layer; Wherein, the thickness of the first hydrophilic coating is greater than the thickness of the second hydrophilic coating; Wherein, when the composite membrane is placed in an alkaline water electrolysis cell, the first hydrophilic coating faces the cathode, and the second hydrophilic coating faces the anode.

2. The composite membrane for alkaline water electrolysis according to claim 1, It is characterized in that The average pore size of the first hydrophilic coating is smaller than or equal to the average pore size of the second hydrophilic coating.

3. The composite membrane for alkaline water electrolysis according to claim 1, It is characterized in that The thickness of the composite film is less than 500 μm; and / or The thickness of the base film is 150 to 200 μm; and / or The thickness of the first hydrophilic coating is 100 to 180 μm; and / or The thickness of the second hydrophilic coating layer is 20 to 110 μm.

4. The composite membrane for alkaline water electrolysis according to claim 1, It is characterized in that The porous structure of the base film is filled with hydrophilic inorganic particles with a particle size of 120nm to 500nm and / or a particle size of 40nm to 100nm.

5. The composite membrane for alkaline water electrolysis according to claim 1, It is characterized in that The first hydrophilic coating layer includes an upper hydrophilic coating layer and a lower hydrophilic coating layer, wherein the lower hydrophilic coating layer is located between the base film and the upper hydrophilic coating layer, wherein the thickness of the upper hydrophilic coating layer is greater than or equal to that of the lower hydrophilic coating layer.

6. The composite membrane for alkaline water electrolysis according to claim 5, It is characterized in that The average pore size of the second hydrophilic coating is equal to the average pore size of the lower hydrophilic coating, and the average pore size of the second hydrophilic coating is greater than or equal to the average pore size of the upper hydrophilic coating.

7. The composite membrane for alkaline water electrolysis according to claim 5, It is characterized in that The thickness of the composite film is less than 500 μm; and / or The thickness of the base film is 120 to 230 μm; and / or The thickness of the first hydrophilic coating is 100 to 160 μm; and / or The thickness of the second hydrophilic coating is 20 to 100 μm; and / or The thickness of the upper hydrophilic coating is 60 to 100 μm; and / or The thickness of the lower hydrophilic coating layer is 20 to 100 μm.

8. The composite membrane for alkaline water electrolysis according to claim 5, It is characterized in that The first hydrophilic coating layer and the second hydrophilic coating layer include hydrophilic inorganic particles with a particle size of 120 nm to 500 nm and / or a particle size of 40 nm to 100 nm.

9. An alkaline water electrolyzer, It is characterized in that Include: A cathode, an anode, and a composite membrane for alkaline water electrolysis according to any one of claims 1 to 4, wherein the first hydrophilic coating is connected to the cathode, and the second hydrophilic coating is connected to the anode.

10. An alkaline water electrolyzer, It is characterized in that Include: A cathode, an anode, and a composite membrane for alkaline water electrolysis according to any one of claims 5 to 8, wherein the upper hydrophilic coating is connected to the cathode, and the second hydrophilic coating is connected to the anode.