Plating layer structure for plating multiple layers of nickel on steel surface
By forming semi-bright nickel plating layer, high sulfur nickel plating layer and bright nickel plating layer on the steel surface, and using rare earth electrolytic protective film, the problem of low corrosion resistance of bright nickel plating on the steel substrate is solved, and electrochemical protection and low The polluted coating structure meets the requirements of high corrosion resistance and low pollution.
Patent Information
- Application Number
- CN202420437103.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2034-03-07
AI Technical Summary
Directly plating bright nickel on steel substrates has low corrosion resistance and is prone to corrosion, and the traditional chromate electrolytic protection process has high pollution problems.
A multi-layer nickel-plated coating structure is adopted for steel surfaces, including semi-bright nickel-plated layer, high-sulfur nickel-plated layer and bright nickel-plated layer from the inside to the outside, and a rare earth electrolytic protective film is implemented on the bright nickel-plated layer to form an electrochemical Protective coating structure.
Improve the corrosion resistance of nickel plating layer, overcome the defect that direct bright nickel plating does not have electrochemical protection, and avoids the high pollution problem of chromate electrolytic protection, and meets the corrosion resistance of GB/T 9797–2022 standards. Required and demonstrate good bonding and corrosion resistance.
Smart Images

Figure CN221988692U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of metal surface treatment, and in particular relates to a plating structure of multiple layers of nickel on the surface of steel. Background Art
[0002] Nickel plating is a protective decorative coating widely used in daily hardware products, household appliances, clocks, instruments, automobiles, motorcycles, bicycles and other manufacturing industries. The electrode potential of nickel is more positive than that of steel. The nickel plating is a cathodic coating for the steel substrate and has no electrochemical protective effect on the steel substrate. The nickel plating contains a certain number of pores. Only when the coating thickness exceeds 25μm is it basically pore-free. [1] Therefore, the conventional process for preparing a nickel-plated layer on the surface of steel generally includes a cyanide pre-plated copper layer, an acid copper plating layer, and a bright nickel-plated layer.
[0003] Under the strict control of the use of cyanide, the industry is seeking other process methods to replace cyanide copper plating. However, the divalent copper cyanide-free copper plating process studied for many years is still far behind cyanide copper plating, and the bonding strength of direct cyanide-free copper plating on substrates such as steel needs to be studied and improved. [2] .
[0004] At present, some electroplating companies use the method of directly plating bright nickel on steel substrates to avoid the use of cyanide copper plating process, but the corrosion resistance of the prepared nickel plating layer often cannot meet the requirements of GB / T 9797-2022 "Metallic Covering Nickel + Chromium and Copper + Nickel + Chromium Electroplating Layer". The nickel plating layer formed by direct plating of bright nickel on the steel substrate can easily be corroded by the corrosive medium through the pores of the plating layer. First, red rust appears in the pores, and then the corrosive medium diffuses laterally on the surface of the steel substrate to corrode the entire substrate surface, causing the nickel plating layer to fall off.
[0005] The nickel-plated layer itself is easy to discolor. In the past, the chromate electrolysis process was usually used to prepare an electrolytic protective film on the bright nickel-plated layer, but the use of chromate has a high pollution problem.
[0006] References: [1] Zhang Yuncheng, Hu Runan, Xiang Rong, Electroplating Handbook [M], Beijing, National Defense Industry Press, 1997, 308-309. [2] Qin Zuzu, Li Jiansan, Xu Jinlai, Research progress of cyanide-free copper plating process at home and abroad [J], Electroplating and Finishing, 2015, 34(3): 149-152. Summary of the invention
[0007] In order to solve the problem of low corrosion resistance of bright nickel directly plated on a steel substrate, the utility model provides a multi-layer nickel plating structure on the surface of steel. In order to achieve the above purpose, the utility model adopts the following technical solutions:
[0008] A multi-layer nickel plating structure on the surface of steel comprises a steel substrate, and a semi-bright nickel plating layer, a high-sulfur nickel plating layer, a bright nickel plating layer, and a rare earth electrolytic protective film sequentially prepared from inside to outside on the steel substrate.
[0009] Preferably, the thickness of the semi-bright nickel plating layer is 6 to 18 μm.
[0010] Preferably, the thickness of the high-sulfur nickel plating layer is 2 to 4 μm.
[0011] Preferably, the thickness of the bright nickel plating layer is 3-9 μm.
[0012] The sulfur content of semi-bright nickel plating is about 0.005%, the sulfur content of bright nickel plating is about 0.03%, and the sulfur content of high-sulfur nickel plating is 0.1% to 0.2%. As the sulfur content increases, the electrode potential of these three coatings becomes negative in turn, and the potential difference is large. Compared with the semi-bright nickel plating, the high-sulfur nickel plating and the bright nickel plating are anodic coatings. This coating structure has an electrochemical protection effect and can effectively prevent the corrosive medium from corroding the substrate. The electrode potential of the high-sulfur nickel plating is more negative than that of the bright nickel plating. When this coating structure is corroded, the corrosive medium first corrodes the high-sulfur nickel plating and forms lateral corrosion along the high-sulfur nickel plating. However, under the protection of the bright nickel surface layer, the corrosion rate is relatively slow.
[0013] Compared with the prior art, the utility model has the following beneficial effects:
[0014] 1. The multi-layer nickel plating structure of the steel surface disclosed in the utility model adopts a semi-bright nickel + high-sulfur nickel + bright nickel plating structure. This plating structure has an electrochemical protective effect, which overcomes the technical defect that bright nickel directly plated on the steel substrate does not have an electrochemical protective effect;
[0015] 2. The multi-layer nickel plating structure on the steel surface disclosed by the utility model implements rare earth electrolytic protection on the bright nickel plating layer, thus overcoming the high pollution problem of the traditional method using chromate electrolytic protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:
[0017] Figure 1 It is a schematic diagram of the coating structure of Example 1 and Example 2 of the utility model. DETAILED DESCRIPTION
[0018] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The schematic embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0019] A multi-layer nickel plating structure on the surface of steel comprises a steel substrate, and a semi-bright nickel plating layer, a high-sulfur nickel plating layer, a bright nickel plating layer, and a rare earth electrolytic protective film sequentially prepared from inside to outside on the steel substrate.
[0020] According to the current pre-treatment process, the steel workpiece substrate is degreased, derusted and activated, and then a semi-bright nickel plating layer, a high-sulfur nickel plating layer, a bright nickel plating layer, and a rare earth electrolytic protective film are prepared in sequence.
[0021] The semi-bright nickel plating layer is prepared by adopting the current semi-bright nickel plating process.
[0022] Preferably, the thickness of the semi-bright nickel plating layer is 6 to 18 μm.
[0023] Preferably, the semi-bright nickel plating layer is prepared by using the NINFEA SM-700 semi-bright nickel plating process of Chaobang Chemical:
[0024] Nickel sulfate hexahydrate 240-300g / L, nickel chloride hexahydrate 40-50g / L, boric acid 40-50g / L, NINFEASM-700A auxiliary agent 2-5mL / L, NINFEA SM-700B main light agent 0.3-0.8mL / L, NINFEA SM-700C stabilizer 0.3-0.8mL / L, NINFEA NI-27 wetting agent 1-3mL / L, plating solution pH 3.8-4.4, plating tank temperature 50℃-65℃, cathode current density 3-5A / dm 2 , the cathode moves 6 to 8 m / min.
[0025] The high-sulfur nickel coating is prepared by the current high-sulfur nickel plating process:
[0026] Preferably, the thickness of the high-sulfur nickel plating layer is 2 to 4 μm.
[0027] Preferably, the high-sulfur nickel plating layer is prepared by using the NH-2 high-sulfur nickel plating process of Chaobang Chemical:
[0028] Nickel sulfate hexahydrate 280-360g / L, nickel chloride hexahydrate 80-120g / L, boric acid 35-45g / L, NH-2 high-sulfur nickel main brightener 2-5mL / L, Ni-051 wetting agent 0.5-1L / L, plating solution pH 2-3, plating tank temperature 48℃-52℃, cathode current density 2-5A / dm 2 , the cathode moves 4 to 6 m / min.
[0029] The bright nickel plating layer is prepared by adopting the current bright nickel plating process.
[0030] Preferably, the thickness of the bright nickel plating layer is 3 to 9 μm.
[0031] Preferably, the bright nickel plating layer is prepared by using the NINFEA 8003 bright nickel plating process of Chaobang Chemical:
[0032] Nickel sulfate hexahydrate 240-320g / L, nickel chloride hexahydrate 45-70g / L, boric acid 40-50g / L, NINFEASC-260 light nickel softener 15-40mL / L, NINFEA AS-250 light nickel auxiliary 3-7mL / L, NINFEA 8003 light nickel main brightener 0.4-0.8mL / L, NINFEA NI-35 light nickel wetting agent 0.5-1.5mL / L, plating solution pH 4.2-4.8, plating tank temperature 55℃-65℃, cathode current density 3-6A / dm 2 , uniform air stirring.
[0033] The rare earth electrolytic protection film is prepared by using the rare earth electrolytic protection process developed by Chaobang Chemical.
[0034] Preferably, the rare earth electrolysis protection process is:
[0035] Cerium acetate 1-5g / L, HEDP complexing agent 5-30g / L, sodium molybdate 5-10g / L, anhydrous sodium carbonate 100-150g / L, bath pH 11.5-12.5 (pH adjusted with sodium hydroxide solution), cathode current density 0.5-1.5A / dm 2 , operate at room temperature, use the plated part as cathode and the titanium plate as anode, and electrolyze for 60 to 120 seconds. Example
[0036] like Figure 1 As shown, a multi-layer nickel plating structure on the surface of steel includes a steel substrate 1, and a semi-bright nickel plating layer 2, a high-sulfur nickel plating layer 3, a bright nickel plating layer 4, and a rare earth electrolytic protective film 5 prepared in sequence from the inside to the outside on the steel substrate 1.
[0037] 1. Pre-treatment:
[0038] The steel substrate 1 is subjected to "alkaline chemical degreasing → water washing → acid washing → water washing → alkaline cathode electrolytic degreasing → water washing → alkaline anodic electrolytic degreasing → water washing → activation → water washing".
[0039] 2. Semi-bright nickel plating:
[0040] A semi-bright nickel plating layer 2 is prepared on a pre-treated steel substrate 1 by using NINFEA SM-700 semi-bright nickel plating process produced by SuperBang Chemical, and the plating thickness is 12 μm.
[0041] Nickel sulfate hexahydrate 260g / L, nickel chloride hexahydrate 42g / L, boric acid 42g / L, NINFEA SM-700A auxiliary agent 3.5mL / L, NINFEA SM-700B main light agent 0.5mL / L, NINFEA SM-700C stabilizer 0.5mL / L, NINFEA NI-27 wetting agent 2mL / L, plating solution pH 4.1, plating tank temperature 58℃, cathode current density 4A / dm 2 , cathode moves 6m / min.
[0042] 3. High sulfur nickel plating:
[0043] A high-sulfur nickel coating 3 is prepared on the semi-bright nickel coating 2 of the steel part by using the NH-2 high-sulfur nickel coating process of Chaobang Chemical, and the thickness of the coating is 3 μm.
[0044] Nickel sulfate hexahydrate 300g / L, nickel chloride hexahydrate 90g / L, boric acid 38g / L, NH-2 high sulfur nickel main brightener 4mL / L, Ni-051 wetting agent 0.8L / L, plating solution pH 2.5, plating tank temperature 50℃, cathode current density 4A / dm 2 , cathode moves 5m / min.
[0045] 4. Bright nickel plating:
[0046] A bright nickel plating layer 4 is prepared on the high-sulfur nickel plating layer 3 of the steel part by using the NINFEA 8003 bright nickel plating process of Chaobang Chemical, and the plating thickness is 6 μm.
[0047] Nickel sulfate hexahydrate 260g / L, nickel chloride hexahydrate 45g / L, boric acid 42g / L, NINFEA SC-260 nickel softener 25mL / L, NINFEA AS-250 nickel auxiliary 5mL / L, NINFEA 8003 nickel main brightener 0.6mL / L, NINFEA NI-35 nickel wetting agent 0.8mL / L, plating solution pH 4.5, plating tank temperature 58℃, cathode current density 4A / dm 2 , uniform air stirring.
[0048] 5. Rare earth electrolysis protection:
[0049] A rare earth electrolytic protection film 5 is prepared on the bright nickel plating 4 of the steel part by using the rare earth electrolytic protection process of Chaobang Chemical.
[0050] Cerium acetate 3g / L, HEDP complexing agent 20g / L, sodium molybdate 10g / L, anhydrous sodium carbonate 120g / L, bath pH 12 (pH adjusted with sodium hydroxide solution), cathode current density 1A / dm 2 , operated at room temperature, using the plated piece as cathode and the titanium plate as anode, and electrolyzing for 100s.
[0051] 6. Drying:
[0052] After rare earth electrolytic protection, the steel parts are subjected to “water washing → pure water washing → drying”. Example
[0053] like Figure 1 As shown, a multi-layer nickel plating structure on the surface of steel includes a steel substrate 1, and a semi-bright nickel plating layer 2, a high-sulfur nickel plating layer 3, a bright nickel plating layer 4, and a rare earth electrolytic protective film 5 prepared in sequence from the inside to the outside on the steel substrate 1.
[0054] 1. Pre-treatment:
[0055] The steel substrate 1 is subjected to "alkaline chemical degreasing → water washing → acid washing → water washing → alkaline cathode electrolytic degreasing → water washing → alkaline anodic electrolytic degreasing → water washing → activation → water washing".
[0056] 2. Semi-bright nickel plating:
[0057] A semi-bright nickel plating layer 2 is prepared on a pre-treated steel substrate 1 by using the NINFEA SM-700 semi-bright nickel plating process of Chaobang Chemical, and the plating thickness is 12 μm.
[0058] Nickel sulfate hexahydrate 280g / L, nickel chloride hexahydrate 48g / L, boric acid 48g / L, NINFEA SM-700A auxiliary agent 3.5mL / L, NINFEA SM-700B main light agent 0.5mL / L, NINFEA SM-700C stabilizer 0.5mL / L, NINFEA NI-27 wetting agent 2mL / L, plating solution pH 4.1, plating tank temperature 58℃, cathode current density 4A / dm 2 , cathode moves 6m / min.
[0059] 3. High sulfur nickel plating:
[0060] A high-sulfur nickel coating 3 is prepared on the semi-bright nickel coating 2 of the steel part by using the NH-2 high-sulfur nickel coating process of Chaobang Chemical, and the thickness of the coating is 3 μm.
[0061] Nickel sulfate hexahydrate 340g / L, nickel chloride hexahydrate 110g / L, boric acid 43g / L, NH-2 high sulfur nickel main brightener 4mL / L, Ni-051 wetting agent 0.8L / L, plating solution pH 2.5, plating tank temperature 50℃, cathode current density 4A / dm 2 , cathode moves 5m / min.
[0062] 4. Bright nickel plating:
[0063] A bright nickel plating layer 4 is prepared on the high-sulfur nickel plating layer 3 of the steel part by using the NINFEA 8003 bright nickel plating process of Chaobang Chemical, and the plating thickness is 6 μm.
[0064] Nickel sulfate hexahydrate 300g / L, nickel chloride hexahydrate 60g / L, boric acid 48g / L, NINFEA SC-260 nickel softener 25mL / L, NINFEA AS-250 nickel auxiliary 5mL / L, NINFEA 8003 nickel main brightener 0.6mL / L, NINFEA NI-35 nickel wetting agent 0.8mL / L, plating solution pH 4.5, plating tank temperature 58℃, cathode current density 4A / dm 2 , uniform air stirring.
[0065] 5. Rare earth electrolysis protection:
[0066] A rare earth electrolytic protection film 5 is prepared on the bright nickel plating 4 of the steel part by using the rare earth electrolytic protection process of Chaobang Chemical.
[0067] Cerium acetate 5g / L, HEDP complexing agent 30g / L, sodium molybdate 5g / L, anhydrous sodium carbonate 150g / L, bath pH 12 (pH adjusted with sodium hydroxide solution), cathode current density 1A / dm 2 , operated at room temperature, using the plated piece as cathode and the titanium plate as anode, and electrolyzing for 100s.
[0068] 6. Drying:
[0069] After rare earth electrolysis, the plated parts are “washed with water → washed with pure water → dried”.
[0070] Test Example 1:
[0071] According to the acetic acid salt spray test of GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", the steel parts prepared in Example 1 and Example 2 had no red rust on the surface of the multi-layer nickel-plated samples after 72 hours, which exceeded the requirements of GB / T 9797-2022 "Metal coating nickel + chromium and copper + nickel + chromium electroplating layer" standard.
[0072] Test Example 2:
[0073] In this test example, the multi-layer nickel-plated steel samples prepared in Example 1 and Example 2 were tested for the bonding strength of the coating by a thermal shock method according to GB / T 5270-2005 "Review of test methods for adhesion strength of electrodeposited and chemically deposited metal coatings on metal substrates". The plated parts were placed in a heating furnace and heated to 300°C for 30 minutes. After being taken out, they were suddenly cooled in water at room temperature. The coating did not bubble or fall off, and the coating structure had good bonding strength.
[0074] The technical solutions provided by the embodiments of the present utility model are described in detail above. The principles and implementation methods of the embodiments of the present utility model are described in detail using specific examples herein. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present utility model. It should be pointed out that for those skilled in the art, according to the embodiments of the present utility model, there will be changes in the specific implementation methods and application scopes, which should all fall within the protection scope of the present utility model.
Claims
1. A multi-layer nickel coating structure on a steel surface, characterized in that: The invention comprises a steel substrate, and a semi-bright nickel plating layer, a high-sulfur nickel plating layer, a bright nickel plating layer, and a rare earth electrolytic protective film which are sequentially prepared from the inside to the outside on the steel substrate.
2. The multi-layer nickel plating structure on the steel surface as claimed in claim 1, characterized in that: The thickness of the semi-bright nickel plating layer is 6-18 μm.
3. The multi-layer nickel plating structure on the steel surface as claimed in claim 1, characterized in that: The thickness of the high-sulfur nickel plating layer is 2-4 μm.
4. The multi-layer nickel plating structure on the steel surface as claimed in claim 1, characterized in that: The thickness of the bright nickel plating layer is 3-9 μm.