Tempering low-emissivity coated glass

By forming a multi-layer structure on the coated glass and adding rare earth elements and ultraviolet absorbers, the problems of permeability, reflectivity and stability of coated glass in radiation resistance are solved, and high-performance low-radiation and corrosion resistance are achieved. Meet the high quality and comfort needs of modern buildings.

CN222007639UActive Publication Date: 2024-11-15HUAIAN XINHONGXING ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323669478.7
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-31
Publication Date
2024-11-15
Estimated Expiration
2033-12-31

AI Technical Summary

Technical Problem

Existing coated glasses have problems with radiation resistance, reflectivity and coating stability, and cannot effectively block or absorb specific radiation, resulting in radiation penetration, glare and coating aging.

Method used

Adopt multi-layer structural design, including glass substrate, tin oxide film layer, graphene transparent conductive layer, silver layer, chromium nitride film, alumina passivation layer, calcium fluoride anti-reflective layer, tin oxide nanowire layer and optical super Material coating, high-performance coated glass is formed through vacuum coating, chemical vapor deposition and other technologies, and rare earth elements and ultraviolet absorbers are added to the tempering treatment.

Benefits of technology

It achieves high-performance low-radiation, corrosion-resistant and environmentally friendly coated glass, improves optical and thermal performance, and meets the high-quality, high energy-saving and high comfort needs of modern buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222007639U_ABST
    Figure CN222007639U_ABST
Patent Text Reader

Abstract

The utility model discloses temperable low-emissivity coated glass which comprises a glass substrate, a tin oxide thin film layer is arranged on one side of the glass substrate, a graphene transparent conducting layer is arranged on one side of the tin oxide thin film layer, a silver layer is arranged on one side of the graphene transparent conducting layer, a chromium nitride thin film is arranged on one side of the silver layer, and the chromium nitride thin film is arranged on the other side of the silver layer. An aluminum oxide passivation layer is arranged on one side of the chromium nitride film, and a calcium fluoride anti-reflection layer is arranged on one side of the aluminum oxide passivation layer. According to the temperable low-radiation coated glass, all functional layers can be sequentially formed on the surface of the glass through the technical means of vacuum coating, chemical vapor deposition, physical vapor deposition and the like, so that the temperable low-radiation coated glass with the high performance of being temperable, low in radiation, corrosion-resistant and the like is manufactured, and the glass not only has good optical performance, thermal performance and environment-friendly performance, but also has the advantages of being simple in manufacturing process and low in cost. And the requirements of modern buildings on high quality, high energy conservation and high comfort can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of coated glass, in particular to a tempered low-radiation coated glass. Background Art

[0002] Coated glass is a product that has one or more layers of metal, alloy or metal compound thin films coated on the surface of the glass. This coating can change the optical properties of the glass to meet specific needs. There are many types of coated glass, including heat reflective glass, low-emissivity glass (L0w-E glass) and conductive film glass. These different types of coated glass have their own unique characteristics and application areas.

[0003] Coated glass may have some disadvantages in terms of radiation resistance, mainly including the following aspects:

[0004] 1. Radiation transmittance: Some types of coated glass may not be able to effectively block or absorb certain types of radiation, such as ultraviolet, infrared or electromagnetic radiation, which may cause radiation to directly penetrate the glass, causing potential impacts on the indoor environment and human health.

[0005] 2. Radiation reflectivity: The surface coating of coated glass may reflect some radiation instead of completely absorbing or transmitting it. This reflection may cause glare or interference of radiation on the glass surface, affecting sight and visual comfort.

[0006] 3. Coating stability: The coating of some coated glass may change or be damaged due to the long-term influence of radiation. Long-term exposure to strong radiation environment may cause aging, discoloration or peeling of the coating, thereby reducing its radiation resistance. Utility Model Content

[0007] The purpose of the utility model is to provide a tempered low-emissivity coated glass to solve the problems raised in the above background technology.

[0008] To achieve the above-mentioned purpose, the utility model provides the following technical solutions: a tempered low-emissivity coated glass, comprising a glass substrate, a tin oxide thin film layer is provided on one side of the glass substrate, a graphene transparent conductive layer is provided on one side of the tin oxide thin film layer, a silver layer is provided on one side of the graphene transparent conductive layer, a chromium nitride thin film is provided on one side of the silver layer, an aluminum oxide passivation layer is provided on one side of the chromium nitride thin film, a calcium fluoride anti-reflection layer is provided on one side of the aluminum oxide passivation layer, a tin oxide nanowire layer is provided on one side of the calcium fluoride anti-reflection layer, an optical metamaterial coating is provided on one side of the tin oxide nanowire layer, and an anti-fingerprint coating is provided on one side of the optical metamaterial coating.

[0009] Compared with the prior art, the beneficial effects of the utility model are:

[0010] The tempered low-emissivity coated glass can form various functional layers on the glass surface in sequence through vacuum coating, chemical vapor deposition, physical vapor deposition and other technical means, thereby producing high-performance coated glass with temperability, low radiation, corrosion resistance, etc. This glass not only has good optical properties, thermal properties and environmental protection properties, but also can meet the needs of modern buildings for high quality, high energy saving and high comfort. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a schematic diagram of the structure of the utility model.

[0012] In the figure: 1. Glass substrate; 2. Tin oxide thin film layer; 3. Graphene transparent conductive layer; 4. Silver layer; 5. Chromium nitride thin film; 6. Aluminum oxide passivation layer; 7. Calcium fluoride anti-reflection layer; 8. Tin oxide nanowire layer; 9. Optical metamaterial coating; 10. Anti-fingerprint coating. DETAILED DESCRIPTION

[0013] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments in the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.

[0014] See also Figure 1 The utility model provides a technical solution: a tempered low-emissivity coated glass, comprising a glass substrate 1, a tin oxide thin film layer 2 is arranged on one side of the glass substrate 1, a graphene transparent conductive layer 3 is arranged on one side of the tin oxide thin film layer 2, a silver layer 4 is arranged on one side of the graphene transparent conductive layer 3, a chromium nitride thin film 5 is arranged on one side of the silver layer 4, an aluminum oxide passivation layer 6 is arranged on one side of the chromium nitride thin film 5, a calcium fluoride anti-reflection layer 7 is arranged on one side of the aluminum oxide passivation layer 6, a tin oxide nanowire layer 8 is arranged on one side of the calcium fluoride anti-reflection layer 7, an optical metamaterial coating 9 is arranged on one side of the tin oxide nanowire layer 8, and an anti-fingerprint coating 10 is arranged on one side of the optical metamaterial coating 9.

[0015] The glass substrate 1 is made of float glass, and the graphene transparent conductive layer 3 has a thickness of 5-10 nanometers.

[0016] The thickness of the tin oxide film layer 2 is 10-50 nanometers.

[0017] The thickness of the silver layer 4 is 10-30 nanometers.

[0018] The thickness of the chromium nitride film 5 is 5-20 nanometers.

[0019] The thickness of the aluminum oxide passivation layer 6 is 2-10 nanometers.

[0020] The thickness of the calcium fluoride anti-reflection layer 7 is 50-200 nanometers, and the thickness of the anti-fingerprint coating 10 and the optical metamaterial coating 9 are both 0.1-1 micrometers.

[0021] Manufacturing steps:

[0022] Manufacturing steps:

[0023] Glass substrate preparation:

[0024] Choose high-quality float glass or ultra-clear glass as substrate to ensure high transmittance and excellent physical properties.

[0025] Clean, dry and pre-treat the glass to ensure that the surface is free of impurities and moisture.

[0026] Deposition of metal oxide thin films:

[0027] Using vacuum coating technology, a layer of metal oxide film (such as tin oxide) is deposited on the surface of the glass substrate as a transparent conductive layer to improve the light transmittance and conductivity of the glass.

[0028] Thickness requirement: about 10-50 nanometers.

[0029] Depositing the graphene layer:

[0030] Depositing a layer of graphene on top of a metal oxide film using methods such as chemical vapor deposition or transfer printing can improve the glass's electrical conductivity and give it greater mechanical strength.

[0031] Thickness requirement: The thickness of a single layer of graphene is about 0.335 nanometers. The number of layers can be increased as needed, but it is usually kept at the nanometer level.

[0032] Depositing the silver layer:

[0033] A layer of silver is deposited on the graphene layer. As a key material for low-radiation performance, the silver layer can effectively reflect thermal radiation and reduce the temperature difference between indoors and outdoors.

[0034] Methods such as physical vapor deposition or chemical vapor deposition can be used.

[0035] Thickness requirement: about 10-30 nanometers.

[0036] Deposition of metal nitride thin films:

[0037] A metal nitride film (such as chromium nitride) is deposited on the silver layer as a protective layer to prevent the silver layer from oxidation and corrosion.

[0038] Thickness requirement: about 5-20 nanometers.

[0039] Deposition of oxide passivation layer:

[0040] An oxide passivation layer (such as aluminum oxide) is deposited on the metal nitride film to further enhance the stability and durability of the protective layer.

[0041] Thickness requirement: about 2-10 nanometers.

[0042] Adding rare earth elements:

[0043] During the coating process, rare earth elements (such as cerium and lanthanum) are added to the glass by ion implantation or co-deposition to improve the corrosion resistance and mechanical strength of the glass.

[0044] Thickness requirement: adjusted according to the concentration of rare earth elements and the thickness of glass.

[0045] Apply silicone resin:

[0046] Silicone resin is applied between the layers of materials as a bonding agent to ensure close bonding between the layers of materials and prevent peeling and blistering.

[0047] Thickness requirement: about 1-5 microns.

[0048] Deposition of fluoride antireflection layer:

[0049] A layer of fluoride (such as calcium fluoride) is deposited on the glass surface as an anti-reflection layer to reduce reflection on the glass surface and increase light transmittance.

[0050] Thickness requirement: about 50-200 nanometers.

[0051] Add UV absorber:

[0052] Adding an appropriate amount of UV absorber (such as titanium dioxide or zinc oxide) to the glass can reduce the damage of UV rays to indoor objects and humans.

[0053] Thickness requirement: Adjust according to the concentration of UV absorber and the thickness of glass.

[0054] Tempered treatment:

[0055] The coated glass is tempered to improve its strength and safety through a process of heating and rapid cooling.

[0056] No additional materials are required.

[0057] Filling with rare gas:

[0058] The middle layer of tempered glass is filled with rare gas (such as argon) to improve the thermal insulation and sound insulation effects of the glass.

[0059] Thickness requirements: Adjust according to the thickness of the glass and the required thermal insulation performance.

[0060] Adding metal oxide nanowires:

[0061] By growing or depositing a layer of metal oxide nanowires (such as tin oxide nanowires) on the glass surface using a solution method, a vapor phase method or an electrochemical deposition method, the light transmittance, electrical conductivity and photocatalytic performance of the glass can be improved.

[0062] The diameter of nanowires is usually at the nanometer level, and the length can be adjusted as needed.

[0063] Thickness requirements: The diameter of the nanowire can vary from a few nanometers to hundreds of nanometers, and the length can vary from hundreds of nanometers to tens of micrometers. It depends on the preparation method and process conditions.

[0064] Anti-fingerprint coating:

[0065] A special anti-fingerprint coating is applied to the glass surface to make it difficult for fingerprints and stains to remain on the glass surface and easy to clean.

[0066] Thickness requirement: about 0.1-1 micron.

[0067] Adding antimicrobial agents:

[0068] An appropriate amount of antimicrobial agent (such as silver ions or copper ions) is added to the glass.

[0069] Thickness requirement: Adjust according to the concentration of antimicrobial agent and the thickness of glass.

[0070] Add color additives (optional):

[0071] Add appropriate amount of color additives to the glass as needed. The thickness requirement is adjusted according to the concentration of color additives and the thickness of the glass.

[0072] After completing the above steps, quality inspection, packaging and transportation are carried out to ensure that the quality and performance of the product meet the requirements.

[0073] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A temperable low-emissivity coated glass, comprising a glass substrate (1), characterized in that: A tin oxide thin film layer (2) is provided on one side of the glass substrate (1), a graphene transparent conductive layer (3) is provided on one side of the tin oxide thin film layer (2), a silver layer (4) is provided on one side of the graphene transparent conductive layer (3), a chromium nitride thin film (5) is provided on one side of the silver layer (4), an aluminum oxide passivation layer (6) is provided on one side of the chromium nitride thin film (5), a calcium fluoride anti-reflection layer (7) is provided on one side of the aluminum oxide passivation layer (6), a tin oxide nanowire layer (8) is provided on one side of the calcium fluoride anti-reflection layer (7), an optical metamaterial coating (9) is provided on one side of the tin oxide nanowire layer (8), and an anti-fingerprint coating (10) is provided on one side of the optical metamaterial coating (9).

2. The temperable low-emissivity coated glass according to claim 1, characterized in that: The glass substrate (1) is made of float glass, and the graphene transparent conductive layer (3) has a thickness of 5-10 nanometers.

3. The temperable low-emissivity coated glass according to claim 1, characterized in that: The thickness of the tin oxide thin film layer (2) is 10-50 nanometers.

4. The temperable low-emissivity coated glass according to claim 1, characterized in that: The thickness of the silver layer (4) is 10-30 nanometers.

5. The temperable low-emissivity coated glass according to claim 1, characterized in that: The thickness of the chromium nitride film (5) is 5-20 nanometers.

6. The temperable low-emissivity coated glass according to claim 1, characterized in that: The aluminum oxide passivation layer (6) has a thickness of 2-10 nanometers.

7. The temperable low-emissivity coated glass according to claim 1, characterized in that: The thickness of the calcium fluoride anti-reflection layer (7) is 50-200 nanometers, and the thickness of the anti-fingerprint coating (10) and the optical metamaterial coating (9) are both 0.1-1 micrometers.