Device for manufacturing negative electrode capable of improving rapid charging performance of negative electrode
By using a magnet plate device in the negative electrode manufacturing process, constant and periodic magnetic fields are formed using unit magnets in different directions, the problem of insufficient orientation of the negative electrode active material is solved, and the charging and discharging efficiency of the battery is significantly improved and the electrode is prevented from peeling off.
Patent Information
- Application Number
- CN202323594002.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-20
- Filing Date
- 2023-12-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2033-12-28
AI Technical Summary
The prior art is difficult to ensure the full vertical orientation of the negative electrode active material in a short time, resulting in a degradation of battery performance and electrode stripping, which affects the charging and discharge efficiency of the battery.
Using a device including upper and lower magnet plates, unit magnets in different directions are arranged on the magnet plates to form a constant perpendicular magnetic force and periodically changing magnetic field to improve the vertical orientation of the negative electrode active material during the coating and drying of the negative electrode mixture. Spend.
The electrode stripping phenomenon is effectively suppressed, the charging performance and charging and discharging efficiency of the battery are improved, and the high orientation of the negative electrode active material is ensured.
Smart Images

Figure CN222126584U_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0022121, filed on February 20, 2023, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] The technology and implementation methods disclosed in this patent document generally relate to a negative electrode, a method and an apparatus for manufacturing the negative electrode. Background Art
[0004] An electrode is an electrical conductor that is used to make contact with non-metallic parts of a circuit, such as an electrolyte. Electrodes are an important part of a battery and can be made of a variety of materials, depending on the type of battery. Utility Model Content
[0005] Technical issues to be solved
[0006] As described above, the purpose of the present invention is to provide a negative electrode that can improve battery performance by ensuring a sufficient vertical orientation degree of a negative electrode active material in a short time, and a negative electrode manufacturing device and method that can manufacture the negative electrode.
[0007] The utility model aims to provide a method for manufacturing a negative electrode using the device for manufacturing a negative electrode as described above.
[0008] The utility model aims to provide a negative electrode which comprises a negative electrode active material oriented in a direction perpendicular to a negative electrode current collector and reduces, minimizes or prevents the peeling between the negative electrode current collector and the negative electrode mixture layer.
[0009] As another specific embodiment of the utility model, when the orientation degree of the negative electrode is increased, the curl of the electrode is aggravated, so that during the charge and discharge process, the graphite repeatedly shrinks and expands, resulting in a peeling phenomenon in which the negative electrode current collector and the negative electrode mixture layer cannot maintain the adhesive force and separate. The utility model can be implemented in some embodiments to provide a negative electrode that can suppress the occurrence of such peeling.
[0010] Technical Solution
[0011] The utility model relates to a device for manufacturing a negative pole, the device comprising a pair of magnet plates, an upper magnet plate and a lower magnet plate, arranged above and below a plane (for example, an XY plane) in which the negative pole travels along a first direction (for example, an X-axis direction), wherein a first vertical unit magnet and a second vertical unit magnet and a first horizontal unit magnet and a second horizontal unit magnet with different directions of magnetic force lines are arranged in the magnet plate, and the directions of the magnetic force lines of the unit magnets are changed by 90 degrees each time along a second direction (for example, a Y-axis direction), magnets with opposite polarities of the upper magnet plate and the lower magnet plate face each other, and the magnetic force of the upper magnet plate and the lower magnet plate is constant in the X-axis direction, and the magnetic force changes in the Y-axis direction.
[0012] The length of the vertical unit magnet in the Y-axis direction (eg, LY1 ) and the length of the horizontal unit magnet in the Y-axis direction (eg, LY2 ) may be the same or different.
[0013] A ratio (eg, LY2 / LY1 ) of a length of the horizontal unit magnet in the Y-axis direction (eg, LY2 ) to a length of the vertical unit magnet in the Y-axis direction (eg, LY1 ) may be greater than 0.5 and less than 2.67.
[0014] The length of the vertical unit magnet in the X-axis direction (eg, LX1 ) and the length of the horizontal unit magnet in the X-axis direction (eg, LX2 ) may be the same as or different from each other.
[0015] The magnet plate may include two or more unit magnet columns, at least one unit magnet of the unit magnet columns is arranged parallel to the X-axis, and the unit magnet columns may have at least one unit magnet.
[0016] One unit magnet column may include two or more unit magnets having magnetic lines of force in the same direction.
[0017] One unit magnet column may include two or more unit magnets having the same cross-sectional shape.
[0018] Lengths in the X-axis direction of two or more unit magnets included in the unit magnet array may be the same as or different from each other.
[0019] The thickness of the vertical unit magnet and the thickness of the horizontal unit magnet may be the same as or different from each other.
[0020] Surfaces of the upper magnet plate and the lower magnet plate facing each other may be parallel planes.
[0021] The maximum value of the magnetic force in the Y-axis direction can be greater than 7000G.
[0022] In addition, the utility model provides a method for manufacturing a negative electrode, which includes the following steps: a coating step, coating a negative electrode mixture containing a negative electrode active material on at least one side of a negative electrode collector; and a magnetic field applying step, wherein the negative electrode collector coated with the negative electrode mixture is made to travel between an upper magnetic plate and a lower magnetic plate under the application of a magnetic field, wherein the magnetic field is applied by any of the above-mentioned devices for manufacturing a negative electrode.
[0023] The method of manufacturing a negative electrode may further include a drying step of drying the negative electrode mixture, and the drying step may be performed during the step of applying a magnetic field or after the step of applying a magnetic field.
[0024] The magnetic field may be applied in a direction perpendicular to the negative electrode current collector.
[0025] The magnetic force and the direction of the magnetic field lines in the X-axis direction of the magnetic field may be constant.
[0026] The magnetic field may repeat the increase and decrease of the magnetic force along the Y-axis direction.
[0027] The magnetic force of the magnetic field according to the position in the Y-axis direction may have a sine wave.
[0028] The magnetic field may be applied for more than 1 second.
[0029] The negative electrode mixture may have a viscosity of 150,000 cp or less (at 25° C., 0.1 s -1 Measured at a shear rate of 2.
[0030] The utility model provides a negative electrode, which comprises: a negative electrode collector, which has an XY plane; and a negative electrode mixture layer, which is formed on at least one side of the negative electrode collector and contains a negative electrode active material, wherein the orientation degree of the negative electrode active material in the X-axis direction and the orientation degree of the negative electrode active material in the Y-axis direction of the negative electrode mixture layer are different from each other, and the orientation degree of the negative electrode active material in the Y-axis direction periodically increases and decreases repeatedly.
[0031] The black and white value of the negative electrode may be 63.18 to 63.42.
[0032] The preferred orientation (PO) value of the negative electrode may be 0.29 to 0.37.
[0033] Beneficial Effects
[0034] According to the utility model, a negative electrode can be manufactured. In the process of manufacturing the negative electrode, magnetic plates are arranged above and below the running surface of the negative electrode. The magnetic plates have a magnet arrangement that applies a constant magnetic force to the running direction of the negative electrode and changes the magnetic force in the width direction of the negative electrode. This can inhibit the peeling of the battery cell and improve the charging performance of the battery cell.
[0035] In addition, according to the utility model, not only can a negative electrode be manufactured whose orientation degree changes at a constant period in the width direction relative to the traveling direction of the negative electrode, but also by optimizing the ratio of the vertical length and the horizontal length of the unit magnet, the peeling of the battery cell can be suppressed, and the charging performance of the battery cell can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is a diagram schematically showing a magnet module including a magnet plate for applying a magnetic field between an upper side and a lower side. Figure 1 An example of a magnet plate in which identical unit magnets are arranged in a row.
[01] Figure 2 Schematically shows a magnet plate including vertical unit magnets and horizontal unit magnets arranged according to some embodiments of the present invention. In some implementations, the direction of the magnetic field lines rotates 90 degrees each time in the counterclockwise direction.
[0037] Figure 3 It is schematically shown that Figure 2 A diagram showing changes in magnetic force and magnetic field line direction when a magnet plate of the magnet arrangement shown is placed only on one side.
[0038] Figure 4 (a) is a schematic diagram showing the Figure 2 The magnet arrangement shown is a diagram of a magnet module with magnet plates placed on each side of the negative pole travel plane and the magnetic force and magnetic field line direction of the generated magnetic field. Figure 4 (b) is a diagram schematically showing changes in magnetic force depending on the arrangement positions of the magnet plates.
[0039] Figure 5 The figure schematically shows one of the magnet plates arranged above and below the XY plane where the negative pole runs along the X-axis direction. The magnet plate forms a magnetic field in which the magnetic force periodically changes by arranging the vertical unit magnets and the horizontal unit magnets so that the direction of the magnetic force lines changes by 90 degrees in the clockwise direction along the Y-axis direction.
[0040] Figure 6The figure schematically shows one of the magnet plates arranged above and below the XY plane where the negative pole runs in the X-axis direction. The magnet plate forms a magnetic field in which the magnetic force in the X-axis direction periodically changes by arranging the vertical unit magnets and the horizontal unit magnets so that the direction of the magnetic force lines changes by 90 degrees each time in the X-axis direction.
[0041] Figure 7 It schematically shows some embodiments of the present invention. Figure 2 A diagram showing the relationship between the change in magnetic force according to the change in the vertical length of the vertical unit magnet and the horizontal unit magnet in a magnet plate of a unit magnet arrangement.
[0042] Figure 8 A secondary battery according to one embodiment is schematically shown. DETAILED DESCRIPTION
[0043] The section headings used in this document are for ease of understanding only and do not limit the scope of the implementation to the section in which they are described.
[0044] The negative electrode for a secondary battery is manufactured by coating a negative electrode mixture slurry including a negative electrode active material, a conductive material, a binder, and a solvent on a negative electrode collector, followed by drying and rolling.
[0045] In the process of manufacturing the negative electrode as described above, the negative electrode active material having an anisotropic structure is mainly oriented in a horizontal direction parallel to the negative electrode current collector, and the pores formed between the negative electrode active materials are also mostly oriented in the horizontal direction. As described above, the negative electrode active material and the pores are oriented in the horizontal direction, so that lithium ions move through the pores oriented in the horizontal direction during the charge or discharge process of the secondary battery.
[0046] In recent years, as the demand for secondary batteries has increased, there has been an increasing demand for higher performance and longer-term use of secondary batteries, and there has been a trend to achieve higher capacity by increasing the amount of negative electrode load.
[0047] As described above, with the high capacity of batteries, the demand for improving the fast charging performance of batteries is continuously increasing. However, as described above, when the pores in the negative electrode are oriented in the horizontal direction, the load of the negative electrode increases and the movement distance of lithium ions increases significantly, and this increase in movement distance leads to an increase in resistance during charging, thereby increasing the charging and discharging time.
[0048] In particular, when charging or discharging at a high rate (high C-rate), lithium salt is precipitated on the surface of the negative electrode (lithium plating), which reduces the battery capacity with repeated charge and discharge cycles and also causes problems of impairing battery safety.
[0049] Graphite used as negative electrode active material generally has a spherical shape with a certain degree of anisotropy. When the graphite is oriented in a direction perpendicular to the current collector, the diffusion of lithium ions into the negative electrode is improved, thereby reducing resistance and, in particular, improving rapid charging performance.
[0050] As a method for orienting graphite as a diamagnetic material, the following method can be used: before the negative electrode slurry coated on the negative electrode current collector is dried, a magnetic field in a direction perpendicular to the negative electrode current collector is applied by a permanent magnet. At this time, the greater the magnetic force of the magnetic field, the higher the degree of perpendicular orientation of the negative electrode active material and the pores can be ensured within the same magnetic field application time.
[0051] In general, permanent magnets are used to apply a magnetic field, and conventionally, a magnetic plate in which individual magnets are arranged in a row is used to apply a magnetic field. For example, Figure 1 FIG. 2 schematically shows a magnet plate with a common magnet arrangement used to apply a magnetic field. However, when using Figure 1 When the magnet module shown in the figure is applied with a magnet plate having permanent magnets arranged therein, a maximum magnetic force of about 4000 Gauss (G) can be provided.
[0052] However, in order to improve the productivity of the negative electrode, the process of coating the negative electrode mixture slurry on the negative electrode current collector and drying it is gradually carried out at a high speed. Therefore, in the process of manufacturing the negative electrode, the time for applying the magnetic field is limited to within a few seconds. Figure 1 In the case of the conventional magnet plate shown above, the magnetic force of the magnetic field is small, and therefore it is difficult to ensure a sufficient degree of orientation of the negative electrode in a short time.
[0053] Therefore, it is necessary to provide a negative electrode that can improve the orientation degree of the negative electrode by increasing the magnetic force.
[0054] In some implementations, to improve battery performance by shortening the movement path of lithium ions, the negative electrode may be formed by: applying a magnetic field using a permanent magnet; coating the negative electrode mixture slurry on the negative electrode current collector; and then moving it into the magnetic field.
[0055] For example, the magnetic field may be applied by using a neodymium (Nd) permanent magnet including an N pole and an S pole as a unit magnet.
[0056] In some implementations, in order to maximize the magnetic force of the magnetic field, the negative electrode may include a magnet plate in which unit magnets are arranged. In one embodiment, the direction of the N pole and the S pole of each unit magnet, that is, the direction of the magnetic field line, rotates 90 degrees each time in a clockwise or counterclockwise direction.
[0057] For example, the magnet plate may be Figure 2In some implementations, such as Figure 2 As shown, in order to change the direction of the magnetic lines of force in the counterclockwise direction, a vertical unit magnet (1) with the magnetic lines of force directed upward, a horizontal unit magnet (2) with the magnetic lines of force directed leftward, a vertical unit magnet (3) with the magnetic lines of force directed downward, and a horizontal unit magnet (4) with the magnetic lines of force directed rightward can be arranged in sequence to form a magnet plate.
[0058] In addition, through the above Figure 2 The magnetic plate with unit magnets arranged therein is shown in FIG. 1 , and the directions of the magnetic lines of force are formed vertically and horizontally, so that a magnetic field having a magnetic field as shown in FIG. Figure 3 The magnetic field and the direction of the magnetic field lines are shown. Figure 2 As shown, a magnet plate can be used in which the vertical unit magnets (1, 3) and the horizontal unit magnets (2, 4) are arranged so that the direction of the magnetic lines of force is rotated 90 degrees each time in the counterclockwise direction.
[0059] For example, by Figure 1 The magnet plate with ordinary arrangement shown can form a maximum magnetic force of 4000G, but by Figure 2 The direction of the magnetic force shown rotates the magnet plate 90 degrees each time. Figure 3 The magnitude of the magnetic force shown varies with a constant period, but a greater magnetic force equivalent to 8000G can be generated. Figure 1 The magnet plate with the unit magnet arrangement can also orient the negative electrode active material, but if the negative electrode is arranged in a Figure 2 If the magnet plates of the magnet arrangement shown move within the magnetic field region, the orientation of the negative electrode active material in the negative electrode mixture layer can be further improved by a higher magnetic force.
[0060] When using Figure 2 When the magnet plate with the magnet arrangement shown is Figure 3 As shown, there are horizontal magnetic lines of force. If the negative electrode is moved in a magnetic field region having horizontal magnetic lines of force as described above, the horizontal magnetic lines of force will have an adverse effect on the orientation of the negative electrode active material. Therefore, there may be certain limitations in improving the orientation of the negative electrode.
[0061] However, when a magnetic plate having the above-described arrangement of magnets is disposed on both sides of the upper and lower portions of the path along which the negative electrode moves, the magnetic lines of force in the horizontal direction described above can be removed, so that only the magnetic lines of force in the vertical direction exist, thereby further improving the orientation of the negative electrode active material. Figure 4 It is schematically shown in (a).
[0062] like Figure 4As shown in (a), a pair of upper magnet plates 14 and lower magnet plates 12, which are arranged with vertical unit magnets (1, 3) and horizontal unit magnets (2, 4) having magnetic force lines in the vertical or horizontal direction and rotated 90 degrees in the clockwise direction at a time, can be arranged on the upper and lower sides of the path of travel of the negative pole. At this time, the upper magnet plate 14 and the lower magnet plate 12 can be arranged so that magnets with opposite polarities face each other.
[0063] For example, Figure 4 As shown in (a), when a vertical unit magnet whose polarity of the surface facing the negative pole running surface is S pole (i.e., vertical unit magnet (1)) is provided in the unit magnets provided in the lower magnet plate 12, a vertical unit magnet whose polarity of the surface facing the negative pole running surface is N pole (i.e., vertical unit magnet (3)) can be provided in the upper magnet plate 14 on the surface opposite to the vertical unit magnet (1).
[0064] Likewise, if Figure 4 As shown in (a), for the horizontal unit magnet (2), vertical unit magnet (3) and horizontal unit magnet (4) arranged on the lower magnet plate 12, the horizontal unit magnet (4), vertical unit magnet (1) and horizontal unit magnet (2) can be respectively arranged on the relative upper magnet plate 14.
[0065] By Figure 4 A pair of upper magnet plates 14 and lower magnet plates 12 shown in (a) are arranged on the upper and lower sides of the negative pole traveling surface, the magnetic force outside the traveling surface, i.e., below the lower magnet plate 12 and above the upper magnet plate 14, is reduced, and the magnetic force between the traveling surface of the negative pole, i.e., the upper magnet plate 14 and the lower magnet plate 12, is increased, thereby improving the orientation of the negative pole.
[0066] In addition, if Figure 4 As schematically shown in (a) and (b) of FIG. 1 , the magnetic force changes periodically by repeatedly increasing and decreasing. In some implementations, Figure 4 In (a), the magnetic force between the upper magnet plate 14 and the lower magnet plate 12 is represented by the thickness of the solid line, the magnetic force repeatedly increases and decreases, and the change of the magnetic force according to the arrangement position of the magnet plate is shown in Figure 4 (b) of the paper.
[0067] In addition, from Figure 4 As shown in (a) and (b), the increase and decrease of the magnetic force are repeated periodically, but the magnetic lines of force in the horizontal direction are removed from the area between the upper magnet plate 14 and the lower magnet plate 12, and the magnetic lines of force in the vertical direction act. Therefore, the magnetic field applied according to the embodiment of the utility model is applied in a direction perpendicular to the negative electrode current collector.
[0068] In some embodiments of the utility model, as described above, a pair of magnet plates using vertical unit magnets and horizontal unit magnets arranged in the direction of the magnetic lines of force rotated 90 degrees each time in the clockwise or counterclockwise direction are arranged on the upper and lower sides of the negative electrode moving surface, and the negative electrode is moved under the state of applying a magnetic field, so that a negative electrode in which the negative electrode active material in the negative electrode mixture layer is oriented in a direction perpendicular to the negative electrode current collector can be manufactured.
[0069] In some embodiments of the present invention, when the direction of travel of the negative electrode is referred to as the X-axis direction, and the plane in which the negative electrode travels is referred to as the XY plane, a magnet plate formed by vertical unit magnets and horizontal unit magnets arranged along the Y-axis direction is arranged above and below the XY plane. In some implementations, the term "direction of travel" of the electrode can be used to indicate the direction in which the electrode extends.
[0070] In some implementations, the magnet plate may include a first vertical unit magnet and a second vertical unit magnet and a first horizontal unit magnet and a second horizontal unit magnet whose magnetic force lines are directed differently from each other. For example, the vertical unit magnet may include a first vertical unit magnet having upward magnetic force lines and a second vertical unit magnet having downward magnetic force lines, and the horizontal unit magnet may include a first horizontal unit magnet having leftward magnetic force lines and a second horizontal unit magnet having rightward magnetic force lines.
[0071] In some implementations, the first and second vertical unit magnets and the first and second horizontal unit magnets may be arranged so that the direction of the magnetic field lines changes by 90 degrees each time in a clockwise or counterclockwise direction along the Y-axis direction.
[0072] There is no particular limitation on the arrangement mode of the unit magnets. Figure 2 As shown, it may include an arrangement pattern (1-2-3-4) including a first vertical unit magnet-a first horizontal unit magnet-a second vertical unit magnet-a second horizontal unit magnet, and as Figure 5 As shown, an arrangement pattern (1-4-3-2) including a first vertical unit magnet-a second horizontal unit magnet-a second vertical unit magnet-a first horizontal unit magnet may be included.
[0073] The upper and lower magnet plates can be arranged so that magnets with opposite polarities face each other. By arranging a pair of magnet plates as described above above and below the negative pole running surface, the magnetic force in the X-axis direction of the negative pole running can be constant, and the magnetic force in the Y-axis direction can be varied.
[0074] The device for manufacturing the negative electrode according to the utility model may include: Figure 5 A magnet plate with a unit magnet arrangement shown. Figure 5It is an example of the magnet plate according to the present invention, and may be an upper magnet plate or a lower magnet plate.
[0075] Figure 5 The magnet plate shown in the figure applies a magnetic field in the X-axis direction which is the traveling direction of the negative pole through the same unit magnet, so that in the X-axis direction which is the traveling direction of the negative pole, the magnetic force and direction of the magnetic lines of force of the magnetic field can be constant without changing.
[0076] In some implementations, Figure 5 The magnet plate is arranged with a first vertical unit magnet 1, a second horizontal unit magnet 4, a second vertical unit magnet 3 and a first horizontal unit magnet 2, so that the direction of the magnetic lines of force changes 90 degrees each time in the clockwise direction along the Y-axis direction, and this pattern is repeated many times, so that the magnetic force can repeatedly increase and decrease in the Y-axis direction.
[0077] The increase and decrease of the magnetic force in the Y-axis direction may have a constant periodicity, for example, the magnetic force according to the position in the Y-axis direction may form a sine wave. In some implementations, the periodicity of the magnetic force may vary according to the length (LY) of the unit magnet in the Y-axis direction.
[0078] The magnet plates are respectively disposed on the upper and lower sides, and the unit magnets are arranged so that magnets having polarities in opposite directions face each other, so the direction of the magnetic lines of force does not change, which is the same as the previous description.
[0079] In a device for manufacturing a negative electrode based on one embodiment, as described above, by applying a magnetic force in the X-axis direction which is the direction of travel of the negative electrode and a constant magnetic field in which the direction of the magnetic lines of force does not change, the negative electrode active material can be oriented in a direction perpendicular to the negative electrode current collector, thereby improving the movement path of lithium ions.
[0080] In addition, the negative electrode active material is oriented by the action of the magnetic field as described above, so warping of the electrode may occur at locations with greater magnetic force such as the center of the vertical unit magnet, but the occurrence of the warping can be suppressed by the parts with smaller magnetic force, thereby suppressing the phenomenon of the negative electrode mixture layer being peeled off from the negative electrode collector during high-rate charging of the battery.
[0081] Figure 6Schematically illustrates an example of a device for manufacturing a negative pole as follows, wherein a magnetic plate having vertical unit magnets and horizontal unit magnets is provided. In one embodiment, the direction of the magnetic force lines changes by 90 degrees each time along the X-axis direction as the traveling direction of the negative pole, and the magnetic force and the direction of the magnetic force lines of the magnetic field in the Y-axis direction do not change. The magnet plate is provided at any one of the upper side and the lower side of the traveling surface of the negative pole, and the magnet plate in which the magnet is provided as the magnet plate and the magnets having opposite polarities to each other face each other is provided on the other side.
[0082] like Figure 6 As shown, when the magnetic force of the applied magnetic field changes periodically in the X-axis direction which is the direction of travel of the negative electrode, the negative electrode active material can be oriented in a direction perpendicular to the negative electrode current collector, thereby maximizing the degree of orientation. However, during the high-rate charging process of the battery cell, the negative electrode mixture layer may be peeled off from the negative electrode current collector.
[0083] Therefore, as described above, in some embodiments of the present invention, a magnet plate is formed by setting the unit magnet so that the magnetic field does not change in the direction of travel of the negative pole (for example, the X-axis direction) and the direction of the magnetic lines of force changes 90 degrees each time along the width direction of the direction of travel of the negative pole (the Y-axis direction), thereby obtaining a negative electrode that improves the orientation degree according to the orientation of the negative electrode active material while suppressing the peeling problem of the negative electrode.
[0084] In some embodiments of the present invention, a plurality of unit magnets may be arranged so that the direction of the magnetic field lines changes 90 degrees each time in a constant direction along the Y-axis direction, and may have a unit magnet column parallel to the X-axis in the X-axis direction as the traveling direction of the negative pole. The unit magnet column is one or more unit magnets of the same type arranged parallel to the X-axis, and may include more than two of the unit magnet columns.
[0085] For example, Figure 5 As shown, at least one first vertical unit magnet 1 is arranged in a first vertical unit magnet column, at least one first horizontal unit magnet 2 is arranged in a first horizontal unit magnet column, at least one second vertical unit magnet 3 is arranged in a second vertical unit magnet column, and at least one second horizontal unit magnet 4 is arranged in a second horizontal unit magnet column can be arranged in sequence parallel to the X-axis, and a magnet plate can be formed by repeating the arrangement pattern as described above.
[0086] The unit magnets of the same type may refer to unit magnets having magnetic lines of force in the same direction. Figure 5 Schematically illustrating an example in which one unit magnet column in the X-axis direction is formed by using one unit magnet, and the length (LX) of the unit magnet in the X-axis direction is the same as the length of the unit magnet column.
[0087] When one unit magnet column in the X-axis direction is formed by using two or more unit magnets of the same type, the unit magnets of the same type may be unit magnets having the same cross-sections in a direction perpendicular to the X-axis direction. Although not shown, for example, the length (LY) and thickness (D) in the Y-axis direction of the unit magnets forming one unit magnet column may be the same.
[0088] The lengths (LX) in the X-axis direction of two or more unit magnets forming a unit magnet column may be the same or different from each other. For example, a unit magnet column in the X-axis direction may be formed by combining two or more unit magnets of the same size, and may be formed by using two or more unit magnets having different lengths (LX) in the X-axis direction.
[0089] In addition, if Figure 5 As shown, in a plurality of unit magnet columns, the length of each unit magnet column can be the same as each other, and can also be different from each other, and a portion of the unit magnet columns can be the same as each other. In addition, the length (LX) in the X-axis direction of the unit magnets used to form different unit magnet columns can be the same as each other, and can also be different from each other.
[0090] As described above, the magnet plates based on some embodiments of the utility model are arranged so that the direction of the magnetic lines of force of each unit magnet is rotated 90° each time in a constant direction along the Y-axis direction, and a first magnet plate and a second magnet plate are respectively arranged above and below the XY plane where the negative pole extends, and the first magnet plate and the second magnet plate are arranged so that the unit magnets with opposite polarities face each other, so that the magnetic lines of force in the horizontal direction can be removed, and a magnetic field in which the magnetic force periodically changes along the Y-axis direction can be applied.
[0091] The unit magnets arranged so that the direction of the magnetic lines of force changes 90 degrees each time along the Y-axis direction are formed by alternately arranging the first vertical unit magnet 1 and the second vertical unit magnet 3 that form the magnetic lines of force in the up and down vertical directions and the first horizontal unit magnet 2 and the second horizontal unit magnet 4 that form the magnetic lines of force in the left and right horizontal directions.
[0092] In some implementations, such as Figure 7 As shown, the magnetic force provided by the first vertical unit magnet 1 and the second vertical unit magnet 3 is greater than the magnetic force provided by the first horizontal unit magnet 2 and the second horizontal unit magnet 4, the maximum magnetic force is at the center of the first vertical unit magnet 1 and the second vertical unit magnet 3, the minimum magnetic force is at the center of the first horizontal unit magnet 2 and the second horizontal unit magnet 4, and this magnetic force change has a constant period in the Y-axis direction.
[0093] The characteristic of periodic magnetic force variation as described above can change according to the length ratio of the unit magnets. In some implementations, the larger the area of the first vertical unit magnet 1 and the second vertical unit magnet 3 facing the negative pole running surface, the larger the area providing a magnetic field with a greater magnetic force, which can be more helpful in improving the orientation of the negative pole. In addition, the smaller the area of the first horizontal unit magnet 2 and the second horizontal unit magnet 4, the smaller the area providing a magnetic field with a smaller magnetic force, so that the proportion of the highly oriented area increases, thereby improving the high-speed charging performance, but at the same time, the tendency of the negative pole to peel off due to the volume expansion of the electrode during charging may increase.
[0094] In some embodiments of the present invention, by controlling the lengths of the horizontal unit magnets and the vertical unit magnets, the orientation of the negative pole can be improved, and the effect of preventing peeling can be improved. That is, the first vertical unit magnet 1 and the second vertical unit magnet 3 having a larger magnetic force can be more helpful in improving the orientation of the negative pole, and the first horizontal unit magnet 2 and the second horizontal unit magnet 4 can be helpful in preventing the peeling of the negative pole.
[0095] In some implementations, as a specific embodiment of the utility model, when the lengths of the first vertical unit magnet 1 and the second vertical unit magnet 3 in the Y-axis direction and the lengths of the first horizontal unit magnet 2 and the second horizontal unit magnet 4 in the Y-axis direction are appropriately controlled, the orientation degree of the negative pole can be improved and the effect of preventing peeling can be further improved.
[0096] Although not limited to this, when the length of the first vertical unit magnet 1 and the second vertical unit magnet 3 in the Y-axis direction is set to LY1, and the length of the first horizontal unit magnet 2 and the second horizontal unit magnet 4 in the Y-axis direction is set to LY2, the length ratio LY2 / LY1 of LY1 and LY2 can be adjusted to have a value greater than 0.5 and less than 2.67, thereby improving the orientation degree of the negative electrode and solving the peeling problem.
[0097] When LY2 / LY1 is less than 0.5, the magnetic force change period in the Y-axis direction becomes shorter, thereby forming an interface stress at the interface between the negative electrode mixture layer and the negative electrode current collector, and thus it is difficult to suppress the phenomenon of the electrode mixture layer peeling off from the negative electrode current collector. In addition, when LY2 / LY1 is more than 2.67, the area with the maximum magnetic force is reduced, so that the desired level of negative electrode orientation cannot be obtained, and thus the effect of improving the charge and discharge efficiency may be reduced.
[0098] The length LX1 of the first vertical unit magnet 1 and the second vertical unit magnet 3 in the X-axis direction and the length LX2 of the first horizontal unit magnet 2 and the second horizontal unit magnet 4 in the X-axis direction may be the same as or different from each other, without particular limitation.
[0099] In addition, the thickness D1 of the first vertical unit magnet 1 and the second vertical unit magnet 3 and the thickness D2 of the first horizontal unit magnet 2 and the second horizontal unit magnet 4 may be the same as each other, or may be different from each other, without particular limitation. However, the surfaces of the first magnet plate and the second magnet plate facing each other with reference to the XY plane where the negative pole travels may be planes parallel to each other.
[0100] As described above, a negative electrode current collector coated with a negative electrode mixture is allowed to travel in a negative electrode manufacturing device including a pair of magnet plates, wherein the pair of magnet plates have an arrangement of unit magnets based on the implementation scheme on both sides of the XY plane where the negative electrode travels, so that the negative electrode active material in the negative electrode mixture layer can be oriented, thereby shortening the movement path of lithium ions, and thus improving the fast charging performance.
[0101] The negative electrode can be manufactured by coating a negative electrode mixture containing a negative electrode active material on one or both sides of a negative electrode collector, and allowing the negative electrode collector coated with the negative electrode mixture to travel between a pair of magnetic plates as described above under a magnetic field.
[0102] Generally, the negative electrode having the negative electrode mixture layer formed on the negative electrode current collector can be manufactured by coating a negative electrode mixture in a slurry phase containing a negative electrode active material on at least one side of the negative electrode current collector, drying the mixture, and then rolling the mixture.
[0103] In some implementations, as described above, the negative electrode mixture slurry is applied to the negative electrode current collector and dried while the magnetic force is varied along the Y-axis direction (the Y-axis direction of the XY plane where the negative electrode travels along the X-axis direction) on both sides of the upper and lower sides of the XY plane, so that the negative electrode active material can be oriented in a direction perpendicular to the negative electrode current collector. In addition, a magnetic field may be applied during the drying process after the negative electrode mixture is applied to the negative electrode current collector to orient the negative electrode active material in the negative electrode mixture layer, and a magnetic field may be applied after the negative electrode mixture slurry is applied to the negative electrode current collector to orient the negative electrode active material in the negative electrode mixture layer and then dried.
[0104] The maximum magnetic force of the magnetic field based on some embodiments of the utility model can be 4000G or more, for example, 4500G or more, 5000G or more, 5500G or more, 6000G or more, 6500G or more, 7000G or more, and can be 8000G or more. In addition, the greater the maximum magnetic force, the more the orientation degree of the negative electrode active material in the negative electrode mixture layer can be improved, which is not particularly limited, but can be 12000G or less, for example, 10000G or less.
[0105] In addition, the magnetic field can be applied to the negative electrode mixture layer for more than 1 second, for example, for more than 1.5 seconds, more than 2 seconds, more than 3 seconds or more than 4 seconds, and can be applied for less than 30 seconds, for example, for less than 25 seconds, less than 20 seconds, less than 15 seconds or less than 10 seconds.
[0106] As another example, although not limited thereto, the negative electrode current collector coated with the negative electrode mixture slurry can be moved at a speed of 0.1-50 m / min, for example. The slower the moving speed of the negative electrode current collector, the longer the negative electrode mixture stays in the magnetic field, thereby improving the orientation of the negative electrode active material.
[0107] The viscosity of the negative electrode mixture in the slurry phase may affect the orientation of the negative electrode active material caused by the application of the magnetic field. For example, the lower the viscosity of the negative electrode mixture, the smaller the resistance to the flow of the negative electrode mixture even if the magnetic force and the magnetic field are applied for the same time, so it is easy to orient the negative electrode active material in a direction perpendicular to the negative electrode current collector.
[0108] As a specific embodiment, at 25°C and 0.1s -1 The viscosity of the negative electrode mixture slurry when measured at a shear rate of 300000 cp or less may be 300000 cp or less. The viscosity of the negative electrode mixture slurry may be, for example, 150000 cp or less, 130000 cp or less, 100000 cp or less, 75000 cp or less, 50000 cp or less, 35000 cp or less, 30000 cp or less, 27500 cp or less, or 25000 cp or less.
[0109] The lower limit of the viscosity of the negative electrode mixture slurry is not particularly limited, but may be 5000 cp or more (25° C., shear rate 0.1 s -1 ). When the viscosity of the negative electrode mixture slurry is too low, the negative electrode active material in the negative electrode mixture slurry may be easily precipitated.
[0110] The drying process is a process for removing the solvent contained in the negative electrode mixture. In some implementations, the drying method is not particularly limited, so a conventional drying method can be applied, for example, various drying methods such as natural drying, heating drying, reduced pressure drying and air drying can be used, and can be performed in several steps.
[0111] The drying process is not particularly limited, but may be performed, for example, at a temperature in the range of 60-180° C., and in some implementations, at a temperature in the range of 70-150° C. for 20-300 seconds, such as 40-240 seconds or 60-200 seconds.
[0112] After the drying process, a calendering process may be performed, and the thickness or density of the negative electrode mixture layer may be adjusted by the calendering process. The calendering process may be performed by conventional methods such as a roll pressing method and a flat pressing method, and the thickness of each single side of the negative electrode mixture layer may be manufactured to be 20 μm or more and 120 μm or less, for example, 40 μm or more and 100 μm or less or 60 μm or more and 80 μm or less.
[0113] The negative electrode obtained by the rolling process may have a negative electrode mixture layer with a density of 1.5 g / cm 3 For example, the density of the negative electrode mixture layer can be 1.5 g / cm 3 Above and 2.2g / cm 3 Below or 1.5g / cm 3 Above and 2.0g / cm 3 When the density of the negative electrode mixture layer satisfies the above range, the power, lifespan, and high-temperature storage characteristics when the battery is manufactured can be improved.
[0114] The negative electrode obtained based on some embodiments of the utility model is a negative electrode obtained by applying a constant magnetic force in the traveling direction of the negative electrode (e.g., the X-axis direction) and applying a periodically changing magnetic force in the width direction (e.g., the Y-axis direction) during the manufacturing process of the negative electrode. As for the obtained negative electrode, the negative electrode having an XY plane is alternately formed with intervals with a high vertical orientation degree and intervals with a low vertical orientation degree in different intervals in one direction, and has a constant vertical orientation degree in the other direction. Therefore, the following negative electrode can be obtained, in which the orientation degrees of the negative electrode active material in the negative electrode mixture layer of the negative electrode are different from each other in the X-axis direction and the Y-axis direction, the orientation degree of the negative electrode active material in any direction of the X-axis direction or the Y-axis direction is constant, and the orientation degree of the negative electrode active material in the other direction changes periodically.
[0115] The negative electrode thus obtained is not limited thereto, but the maximum value of the black and white degree of the negative electrode may be greater than 63, for example, may be 63.18 to 63.42.
[0116] In addition, the preferred orientation (PO) of the negative electrode according to the embodiment of the present invention has a minimum value of 0.37 or less, and in some implementations, may have a value of 0.29 to 0.37.
[0117] In some embodiments of the present invention, the negative electrode mixture layer can be formed by coating a negative electrode mixture slurry including a negative electrode active material, a conductive material, a binder and a solvent on a negative electrode current collector. In addition, the negative electrode mixture layer can further include additives such as a thickener as needed.
[0118] The negative electrode active material may be a carbon-based negative electrode active material. As long as the carbon-based negative electrode active material is generally used to manufacture the negative electrode of a secondary battery, it may also be applicable to some embodiments based on the present utility model. This carbon-based negative electrode active material is not particularly limited, but may be artificial graphite, natural graphite, or a mixture of artificial graphite and natural graphite, and may be artificial graphite. Artificial graphite can further improve the dispersibility of the slurry, and can improve the life and high temperature storage characteristics.
[0119] Compared with amorphous carbon-based active materials, the crystallographic properties of particles of crystalline carbon-based active materials such as artificial graphite or a mixture of artificial graphite and natural graphite are more developed. Therefore, when such crystalline carbon-based active materials are used as negative electrode active materials, the orientation characteristics of the carbon material in the negative electrode mixture layer with respect to the external magnetic field can be further improved, and the orientation of the pores can be improved.
[0120] The form of the artificial graphite or natural graphite can be amorphous, plate-like, flaky, spherical, fibrous or a combination thereof. In addition, when the artificial graphite and natural graphite are mixed, the mixing ratio can be 70:30 to 95:5 by weight.
[0121] The negative electrode active material can be used without particular limitation as long as it has a shape that can perform the function of inserting and extracting lithium ions, but in terms of improving the function of the negative electrode active material for the lithium secondary battery, the aspect ratio (aspect ratio) can generally be greater than 20. When a magnetic field is applied while using a negative electrode active material having an aspect ratio as described above, the (002) plane of the negative electrode active material particles can be oriented in a direction perpendicular to the plane of the negative electrode current collector.
[0122] In addition, the negative electrode active material may further include at least one of a silicon (Si)-based negative electrode active material, a tin (Sn)-based negative electrode active material, or a lithium vanadium oxide negative electrode active material in addition to the carbon-based negative electrode active material. When the negative electrode active material further includes these substances, these substances may be included in a range of 1-50 weight % relative to the total weight of the negative electrode active material.
[0123] The Si-based anode active material may be Si, Si-C composite, SiO x (0 < x < 2), Si-Q alloy. In the Si-Q alloy, Q may be an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof other than Si. In some implementations, it may be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0124] Generally, the Si-based anode active material known as the anode active material has the characteristic of large volume change. Therefore, generally, in addition to including a carbon-based anode active material such as graphite, a silicon-based anode active material may be further included. At this time, carbon nanotubes may be included as a conductive material in terms of preventing swelling caused by the volume expansion of the silicon-based anode active material.
[0125] The Sn-based anode active material may be Sn, SnO2, Sn-R alloy. In the Sn-R alloy, R is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof other than Sn and Si. In some implementations, it may be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof. In addition, at least one of them may be used in mixture with SiO2.
[0126] Relative to the total weight of the anode mixture layer, the content of the anode active material in the anode mixture layer may be 94-98% by weight.
[0127] The conductive material is used to impart conductivity to the electrode. The conductive material can be used without restriction as long as it is a conductive material commonly used in secondary batteries. For example, carbon-based substances such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanotubes, etc.; metal-based substances such as metal powders or metal fibers such as copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or conductive materials containing mixtures thereof can be used.
[0128] The content of the conductive material may be 0.1 to 3 wt % relative to the total weight of the negative electrode mixture layer.
[0129] The negative electrode mixture layer may include a binder. The binder serves to bind the negative electrode active material particles to each other and to bind the negative electrode active material to the negative electrode current collector. The binder may be a water-dispersible water-based binder, but is not limited thereto.
[0130] The water-based adhesive can include styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber, nitrile rubber, acrylic rubber, butyl rubber, ethylene-propylene copolymer, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol resin, acrylate-based resin or a combination thereof.
[0131] The content of the binder may be 1.5-3 wt % relative to the total weight of the negative electrode mixture layer.
[0132] In addition to the binder, the negative electrode mixture layer may further contain a thickener to impart viscosity. The thickener may be a water-soluble compound, and may include a cellulose-based compound, for example, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or their alkali metal salts, etc. may be mixed and used. The alkali metal may use Na, K, or Li. Relative to 100 parts by weight of the negative electrode active material, 0.1-3 parts by weight of the thickener may be used.
[0133] As the solvent, an aqueous solvent such as water can be used.
[0134] In some embodiments of the present invention, the negative electrode current collector may use at least one selected from copper foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper, a polymer substrate coated with a conductive metal, and a combination thereof. The thickness of the negative electrode current collector is not particularly limited, for example, it may be 5-30 μm.
[0135] In the negative electrode provided in a specific embodiment of the utility model, by orienting the negative electrode active material in the negative electrode mixture layer in a direction perpendicular to the negative electrode current collector, lithium ions can be easily diffused into the interior of the electrode, thereby improving the charge and discharge efficiency at high rates, thereby improving battery performance, such as improving fast charging performance.
[0136] A secondary battery may be manufactured using a negative electrode in which the negative electrode active material as described above is oriented in a direction perpendicular to the negative electrode current collector. Figure 8 An embodiment of a secondary battery is schematically shown in FIG. Figure 8 As shown, in some embodiments, the secondary battery 100 can be manufactured by the following steps: an electrode assembly 120 is manufactured by alternately stacking a positive electrode 121 and a negative electrode 122 as described above with a separator 123 as a boundary, and then inserted into a battery case 110 and sealed, and an electrolyte is injected.
[0137] The positive electrode is described in some implementations below. The positive electrode is not particularly limited, but the positive electrode is formed by coating a positive electrode mixture in a slurry phase on at least one side of a positive electrode current collector and drying and rolling to form a positive electrode mixture layer. As long as it is a positive electrode commonly used in a secondary battery, it can be applied to some embodiments based on the utility model.
[0138] The positive electrode mixture may include a positive electrode active material, a binder, and a solvent, and may include a conductive material and a thickener as needed.
[0139] The positive electrode active material may use a compound (lithiated intercalation compound) that can reversibly insert and remove lithium. In some implementations, the positive electrode active material may use one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof.
[0140] As a more specific example, the positive electrode active material can be represented by the general formula LiMO2, and a layered lithium transition metal compound (oxide) can be listed, wherein M can include at least one of transition metal elements such as Ni, Co, Mn, and can further include other metal elements or non-metal elements. As the composite oxide, for example, a monolithic lithium transition metal composite oxide containing one of the transition metal elements, a binary lithium transition metal composite oxide containing two of the transition metal elements, and an NCM or NCA-based ternary lithium transition metal composite oxide containing Ni, Co and Mn as transition metal elements as constituent elements can be listed. In some implementations, the composite oxide can be Li x Mn 1-y M y A2.Li x Mn 1-y My O 2-z X z , Li x Mn2O 4-z X z , Li x Mn 2-y M y M' z A4, Li x Co 1-y M y A2.Li x Co 1-y M y O 2-z X z , Li x Ni 1-y M y A2.Li x Ni 1-y M y O 2-z X z , Li x Ni 1-y Co y O 2-z X z , Li x Ni 1-y-z Co y M z A α , Li x Ni 1-y-z Co y M z O 2-α X α , Li x Ni 1-y-z Mn y M z A α , Li x Ni 1-y-z Mn y M z O 2-α X (in the formula, 0.9≤x≤1.1, 0≤y≤0.5, 0≤z≤0.5, 0≤α≤2, M and M' are the same or different from each other, and are selected from Mg, Al, Co, K, Na, Ca, Si, Ti, Sn, V, Ge, Ga, B, As, Zr, Mn, Cr, Fe, Sr, V and rare earth elements, A is selected from O, F, S and P, and X is selected from F, S and P), for example, Li (Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2 and other ternary lithium transition metal composite oxides.
[0141] In addition, the positive electrode active material can be a lithium transition metal compound (oxide) represented by the general formula Li2MO3, wherein M can include at least one of the transition metal elements containing Mn, Fe, and Co, and can further include other metal elements or non-metal elements, for example, Li2MnO3 and Li2PtO3 can be listed.
[0142] In addition, the positive electrode active material may be a solid solution of the LiMO2 and the Li2MO3, for example, may be a solid solution represented by 0.5LiNiMnCoO2-0.5Li2MnO3.
[0143] In addition, a substance having a coating on the surface of the positive electrode active material can also be used, and the compound and the compound having a coating can also be mixed and used. The coating can contain at least one coating element compound selected from oxides, hydroxides, oxyhydroxides, oxycarbonates and hydroxycarbonates of the coating element. The compound forming such a coating can be amorphous or crystalline. The coating element contained in the coating can use Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or a mixture thereof.
[0144] In the positive electrode, the content of the positive electrode active material may be 90-98% by weight relative to the solid weight of the positive electrode mixture.
[0145] The binder serves to bind the positive electrode active material particles to each other and to bind the positive electrode active material to the positive electrode current collector. The binder content may be 1.5-5% by weight relative to the solid weight of the positive electrode mixture. The binder may be, for example, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, cellulose diacetate, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, polyamide fiber, etc.
[0146] The positive electrode mixture slurry may contain a thickener in addition to the binder to impart viscosity. The thickener may be the same as that contained in the negative electrode mixture, and the content of the thickener may be 0.1-3 parts by weight relative to 100 parts by weight of the positive electrode active material.
[0147] The conductive material is used to impart conductivity to the positive electrode, and any conductive material commonly used in the positive electrode of a secondary battery can be used appropriately, and the conductive material used in the negative electrode mixture can be used. The content of the conductive material can be 0.1-5% by weight based on the solid weight of the positive electrode mixture.
[0148] The solvent can use an aqueous solvent such as water, and can also use a non-aqueous solvent. As a non-aqueous solvent, based on some embodiments of the utility model, any solvent commonly used to manufacture a positive electrode mixture of a secondary battery can be used, for example, N-methyl-2-pyrrolidone (NMP) can be cited, but it is not limited thereto.
[0149] The positive electrode current collector may be made of a metal with good conductivity, such as aluminum, nickel, titanium, stainless steel, etc., and may be in various forms such as sheet, foil, mesh, etc. The thickness of the positive electrode current collector is not particularly limited, and may be, for example, 5-30 μm.
[0150] As described above, the positive electrode having the positive electrode mixture layer formed on the positive electrode collector may be manufactured by coating the positive electrode mixture on at least one side of the positive electrode collector and performing drying and rolling.
[0151] The drying and rolling process can be performed by the same method as the method of manufacturing the negative electrode, and thus a detailed description is omitted.
[0152] The separator between the positive electrode and the negative electrode may be a porous sheet, a non-woven fabric, etc., and may be polyethylene, polypropylene, polyvinylidene fluoride or a multilayer film of two or more layers thereof, a two-layer mixed multilayer film of polyethylene / polypropylene, a three-layer mixed multilayer film of polyethylene / polypropylene / polyethylene, a three-layer mixed multilayer film of polypropylene / polyethylene / polypropylene, etc., and a porous heat-resistant layer may be provided on one or both sides of the porous sheet, non-woven fabric, etc. The separator is not particularly limited, but for example, a separator having a thickness of about 10-40 μm may be used.
[0153] The electrolyte may include a non-aqueous organic solvent and a lithium salt. The non-aqueous organic solvent acts as a medium in which ions participating in the electrochemical reaction of the battery can move. For example, carbonate-based solvents, ester-based solvents, ether-based solvents, ketone-based solvents, alcohol-based solvents or aprotic solvents may be used, and solvents commonly used in lithium-ion secondary batteries may be used. The organic solvent may be used alone or in combination of two or more. In some implementations, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, fluoroethylene carbonate (FEC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, cyclopentane sulfone, γ-butyrolactone, propylene sulfite and tetrahydrofuran may be listed.
[0154] The lithium salt is dissolved in an organic solvent and serves as a supply source of lithium ions in the battery, so that the lithium ion secondary battery can basically operate, and the lithium salt is a substance that promotes the movement of lithium ions between the positive electrode and the negative electrode. The lithium salt can be used without limitation as long as it is a lithium salt commonly used in an electrolyte for a lithium secondary battery. The lithium salt can be composed of Li + X - The anion of the lithium salt is not particularly limited, but can be exemplified by F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C- CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - wait.
[0155] In some implementations, the lithium salt may be selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are each independently an integer from 1 to 20), one or more of LiCl, LiI and LiB(C2O4)2 (lithium bis(oxalato)borate (LiBOB).
[0156] The concentration of the lithium salt is not particularly limited, but can be used in the range of 0.1 M to 2.0 M. In order to improve the battery life, the electrolyte may further contain vinylene carbonate or a vinyl carbonate-based compound as required.
[0157] In the negative electrode according to the embodiment of the utility model, the negative electrode active material in the negative electrode mixture layer is oriented in a direction perpendicular to the negative electrode current collector, so that lithium ions can easily diffuse into the electrode during the charge and discharge process of the secondary battery, so in some implementations, the resistance of the battery can be reduced and the charge and discharge efficiency at high rates can be improved, thereby improving the cycle life characteristics and fast charging performance. As another specific embodiment, the peeling between the negative electrode current collector and the negative electrode mixture layer during high rate charge and discharge can be prevented.
[0158] In another specific embodiment, a lithium secondary battery is provided in which each negative electrode and positive electrode as described above are alternately stacked with a separator as a boundary. The lithium secondary battery of the utility model can be manufactured by the following steps: an electrode assembly having a separator arranged between the positive electrode and the negative electrode according to some embodiments of the utility model is manufactured, and then the electrode assembly is contained in a battery case and an electrolyte is injected therein. The shape of the lithium secondary battery of the utility model is not particularly limited, but can be a soft-pack type battery, and can be a cylindrical or prismatic battery using a can, and can be a coin-type battery.
[0159] Example
[0160] The following examples are provided to illustrate the present invention in some implementations. The following examples are specific examples of the present invention and are not intended to limit the present invention.
[0161] Comparative Example 1
[0162] Artificial graphite, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were mixed at a mass ratio of 97.8:1.2:1.0 and dispersed in deionized distilled water to prepare a negative electrode mixture into a slurry phase.
[0163] The negative electrode mixture of the slurry phase was coated on a copper foil with a width of 150 mm using a slot die so that the load value (Loading Weight) was 12.5 mg / cm 2 .
[0164] The negative electrode mixture is dried by passing the copper foil coated with the negative electrode mixture through a drying device, thereby manufacturing a negative electrode.
[0165] Comparative Example 2
[0166] A vertical unit magnet having a horizontal length and a vertical length of 50 mm and a thickness (T) of 20 mm as a neodymium (Nd) magnet was prepared in accordance with Figure 1 The same arrangement as shown is used to make a lower magnet plate with a size of 250 mm × 250 mm.
[0167] Furthermore, the upper magnet plate is manufactured by the same method as that of the lower magnet plate.
[0168] In some implementations, the lower magnet plate and the upper magnet plate are arranged so that the polarities of the surfaces facing each other are opposite to each other, and the lower magnet plate and the upper magnet plate are separated by a gap of 40 mm, so as to produce Figure 1 The magnet module shown.
[0169] The magnet module is arranged just before the drying device, and is designed to perform the drying process immediately after the orientation of the negative electrode active material.
[0170] The negative electrode mixture was the same as that of Comparative Example 1 and coated on a copper foil by the same method, and then dried while passing the copper foil through the magnet module for magnetic orientation for 2 seconds under application of a magnetic field, thereby manufacturing a negative electrode.
[0171] Comparative Example 3
[0172] The first vertical unit magnet and the second vertical unit magnet, which are neodymium magnets, have a horizontal length and vertical length of 40 mm respectively, a thickness of 20 mm, and have magnetic lines of force directed upward and downward, and the first horizontal unit magnet and the second horizontal unit magnet, which have a horizontal length and vertical length of 40 mm respectively, a thickness of 20 mm, and have magnetic lines of force directed rightward and leftward, are used respectively.
[0173] like Figure 6 As shown, the first vertical unit magnet and the second vertical unit magnet and the first horizontal unit magnet and the second horizontal unit magnet are arranged so that the direction of the magnetic force lines is rotated 90 degrees each time along the X-axis direction extending along the negative pole.
[0174] Thus, a lower magnet plate having an overall size of 240 mm×240 mm was produced.
[0175] In some implementations, the upper magnet plate is manufactured by the same method as the lower magnet plate. At this time, the lower magnet plate and the upper magnet plate are arranged so that the polarities of the faces facing each other are opposite to each other.
[0176] The lower magnet plate and the upper magnet plate were spaced apart at an interval of 40 mm to produce a magnet module.
[0177] The magnet module is arranged just before the drying device, and is designed to perform the drying process immediately after the orientation of the negative electrode active material.
[0178] The negative electrode mixture was passed through a magnet module for 2 seconds for magnetic orientation by the same method as in Comparative Example 2 and then dried to manufacture a negative electrode.
[0179] Example 1
[0180] As neodymium magnets, a first vertical unit magnet with an upward magnetic field line and a second vertical unit magnet with a downward magnetic field line are used, and a length LY1 in the Y-axis direction and a length LX1 in the X-axis direction are 40 mm respectively, a thickness length D1 is 20 mm, and a first horizontal unit magnet with a leftward magnetic field line and a second horizontal unit magnet with a rightward magnetic field line are used.
[0181] In some implementations, such as Figure 5 As shown, the first vertical unit magnet 1, the second horizontal unit magnet 4, the second vertical unit magnet 3 and the first horizontal unit magnet 2 are arranged in order so that the direction of the magnetic lines of force are rotated 90 degrees each time along the Y-axis direction relative to the XY plane extending along the X-axis direction of the negative pole, and this arrangement pattern is repeated to produce a magnet plate with an overall size of 240mm×240mm.
[0182] The prepared magnet plate was used as a lower magnet plate.
[0183] In addition, the upper magnet plate is made by the same method as the lower magnet plate, and the lower magnet plate and the upper magnet plate are separated by a gap of 40 mm to make a magnet module. In some implementations, the lower magnet plate and the upper magnet plate are arranged so that the polarities of the faces facing each other are opposite to each other.
[0184] The magnet module is arranged just before the drying device, and is designed to perform the drying process immediately after the orientation of the negative electrode active material.
[0185] Artificial graphite, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) were mixed at a mass ratio of 97.8:1.2:1.0 and dispersed in deionized distilled water to prepare a negative electrode mixture into a slurry phase.
[0186] The prepared negative electrode mixture slurry was coated on a copper foil with a width of 150 mm using a slot die so that the load value (load weight) was 12.5 mg / cm 2 .
[0187] The copper foil was passed through the magnet module for 2 seconds under application of a magnetic field for magnetic orientation, and the negative electrode mixture was dried, thereby manufacturing negative electrodes, respectively.
[0188] Evaluation of physical properties
[0189] [Maximum magnetic force]
[0190] For each magnet module used in Comparative Example 2, Comparative Example 3 and Example 1, the maximum magnetic force was measured on the travel surface where the negative pole travels between the lower magnet plate and the upper magnet plate, and the results are shown in Table 1. In some implementations, the maximum magnetic force is measured at a constant interval of 1 cm in the X-axis direction for a vertical unit magnet column located in the center portion of the width direction (Y-axis direction) of the electrode.
[0191] [Black and white and POO]
[0192] For each negative electrode manufactured in Comparative Examples 1 to 3 and Example 1, a black and white degree measuring instrument was used to measure the black and white degree of the coated negative electrode at 10 points at intervals of 10 mm in the width direction of the negative electrode (Y-axis direction), and the preferred orientation (Preferred Orientation, PO) representing the orientation degree of the negative electrode active material was measured using XRD. The larger the black and white degree value, the better the vertical orientation degree of the negative electrode active material, and the smaller the PO value, the better the vertical orientation degree of the negative electrode active material.
[0193] Table 1 shows the maximum value of the degree of black and white and the minimum value of PO measured above.
[0194] [Evaluation of battery cell performance]
[0195] The negative electrodes manufactured in Comparative Examples 1 to 3 and Example 1 and the same positive electrode were used to make battery cells, and then charged in a constant current (CC) mode of 2.5C until the voltage reached 4.2V to obtain the charging capacity, and discharged in a constant current (CC) mode of 0.3C until the voltage reached 2.5V to obtain the discharge capacity.
[0196] The charge capacity measured as described above was divided by the discharge capacity to calculate the charge / discharge efficiency, and the results are shown in Table 1.
[0197] In addition, the battery cell was disassembled in a state where the voltage reached 4.2 V in a constant current (CC) mode at 2.5 C to confirm whether the negative electrode was peeled off. The results are shown in Table 1.
[0198] [Table 1]
[0199]
[0200] It can be seen from Table 1 that compared with Comparative Example 1, in Comparative Example 2, Comparative Example 3 and Example 1, in which the negative electrode active material is oriented by applying a magnetic field, there are high black and white values and low preferential orientation (PO) values, so it can be seen that the negative electrode active material is oriented in a direction perpendicular to the negative electrode current collector.
[0201] In addition, it can be seen from Table 1 that, compared with Comparative Example 2 using a magnet plate with a common magnet arrangement, in Comparative Example 3 and Example 1 using a magnet plate with a unit magnet arrangement in which the direction of the magnetic lines of force is changed by 90 degrees each time based on some embodiments of the present invention, a magnetic field with a significantly high magnetic force can be applied. Therefore, even if a magnetic field is applied for a short time, the orientation of the negative electrode active material can be further improved, and due to the high orientation of the negative electrode active material as described above, the charge and discharge efficiency of the negative electrode can be further improved.
[0202] In addition, the negative electrode was manufactured by the same method in Example 1 and Comparative Example 3, except that a magnet plate whose direction of magnetic force lines set as a unit magnet was changed by 90 degrees each time along the X-axis direction as the traveling direction of the negative electrode was used in Comparative Example 3, while a magnet plate whose direction of magnetic force lines set as a unit magnet was changed by 90 degrees each time along the Y-axis direction as the width direction of the traveling direction of the negative electrode was used in Example 1. For the maximum magnetic force provided in Example 1 and Comparative Example 3, Example 1 showed a value higher by about 50G, but the black and white degree and preferred orientation (PO) value of the obtained negative electrode were similar, and the charge and discharge efficiency of the battery cell using the obtained negative electrode also showed equivalent results.
[0203] In addition, the results of disassembling the battery and analyzing it can be confirmed that the negative electrode mixture layer is peeled off from the negative electrode current collector in the battery cell using the negative electrode of Comparative Example 3. This can be explained by the fact that when lithium ions are not easy to penetrate into the negative electrode during high-rate charging, lithium salts will precipitate on the surface of the negative electrode, thereby reducing the charging / discharging efficiency. As the vertical orientation of the negative electrode as a whole increases significantly, graphite expands in the direction horizontal to the current collector during charging, and the interfacial stress with the current collector increases, resulting in peeling.
[0204] In addition, the peeling of the negative electrode mixture layer was not observed in the negative electrode of Example 1, because the orientation degree of the negative electrode active material was improved by applying a magnetic field, and the negative electrode had the characteristic that the orientation degree of the negative electrode active material periodically changed in a constant direction by applying a magnetic field in which the magnetic force in the traveling direction of the negative electrode was constant and the magnetic force in the width direction of the negative electrode changed. Therefore, it can be interpreted that during the charge and discharge process, the volume expansion caused by the expansion of the negative electrode active material can be dispersed in the direction in which the orientation degree changes, thereby improving the charge / discharge efficiency while suppressing the peeling of the negative electrode.
[0205] Example 2 to Example 10
[0206] The magnet module is manufactured by the same method as in Example 1, except that as the magnet plate, a magnet plate with an overall size of 240 mm×240 mm is used, which is manufactured by using a plurality of vertical unit magnets having a length LY1 in the Y-axis direction, a length LX1 in the X-axis direction, and a thickness length D1 as shown in Table 2, and a horizontal unit magnet having a length LY2 in the Y-axis direction, a length LX2 in the X-axis direction, and a thickness length D2.
[0207] [Table 2]
[0208]
[0209] A negative electrode was manufactured by the same method as in Example 1 using the prepared magnet module.
[0210] The maximum magnetic force of the magnetic field applied during the manufacture of the negative electrode in each example, the maximum value of the black and white degree and the minimum value of the preferred orientation (PO) of the negative electrode manufactured in the above examples, as well as whether the electrode is peeled and the charge / discharge efficiency as the performance of the battery cell using the negative electrode manufactured in each example were evaluated by the same method as in Example 1, and the evaluation results are shown in Table 3.
[0211] [Table 3]
[0212]
[0213]
[0214] In addition, the negative electrodes obtained in Examples 3 to 6 and Examples 9 to 10 are obtained by applying a constant magnetic force in the traveling direction of the negative electrode and applying a periodically changing magnetic force in the width direction. It can be confirmed that intervals with a high degree of vertical orientation and intervals with a low degree of vertical orientation are alternately formed in different intervals in the width direction of the negative electrode. When the intervals with a low degree of vertical orientation exist periodically, they play a role in alleviating the expansion of graphite in a direction parallel to the current collector, thereby improving the exfoliation characteristics.
[0215] However, in Example 2, Example 7 and Example 8, a magnetic field is applied by arranging vertical unit magnets and horizontal unit magnets so that the direction of the magnetic lines of force is changed by 90 degrees each time in the horizontal direction (Y-axis direction) along the direction of travel of the negative pole. However, unlike other examples, electrode peeling phenomenon is shown to occur.
[0216] When comparing the embodiments 2, 7 and 8 with the embodiments 3 to 6 and 9 to 10, it can be seen that when the length ratio LY2 / LY1 in the Y-axis direction between the vertical unit magnet and the horizontal unit magnet is less than 0.5, the change period of the magnetic force in the width direction becomes shorter, so that the interface stress is formed between the negative electrode mixture layer and the current collector, and thus the peeling of the negative electrode mixture layer may occur. In addition, in the case of the embodiment 6 in which the length ratio LY2 / LY1 is 2.67, the charge and discharge efficiency is 98.2%, showing a relatively low value. It can be seen that this is due to the reduction in the magnitude of the maximum magnetic force, and thus it is shown that the desired level (99.0% or more) of charge / discharge efficiency characteristics cannot be obtained.
[0217] From the results of Examples 1 to 10 described above, it can be seen that when vertical unit magnets and horizontal unit magnets are used and the length ratio LY2 / LY1 between the vertical unit magnets and the horizontal unit magnets in the Y-axis direction is greater than 0.5 and less than 2.67, the battery charging and discharging efficiency can be improved and the electrode peeling can be more effectively suppressed.
[0218] The utility model can be implemented in various electrochemical devices having positive and negative electrodes, and the utility model can be implemented to manufacture these electrochemical devices, such as rechargeable secondary batteries widely used in battery-powered devices or systems, including, for example, digital cameras, mobile phones, laptops, hybrid vehicles, electric vehicles, uninterruptible power supplies, battery energy storage power stations, and other devices including battery energy storage for solar panels, wind turbines and other green technology generators. Specifically, the utility model can be implemented in some embodiments to provide improved electrochemical devices, such as batteries for various power sources and power supply devices, thereby alleviating climate change associated with the use of power sources and power supply devices. Lithium secondary batteries based on the utility model can be used to power electric vehicles (EVs) as an alternative to vehicles using fossil fuel-based engines, and to address various adverse effects such as air pollution and greenhouse gas emissions by providing battery-based energy storage systems (ESS) to store renewable energy such as solar and wind energy.
[0219] The utility model only describes limited examples of implementations of certain embodiments. The disclosed embodiments and other embodiments can be changed, improved and enhanced based on the disclosure of this patent document.
Claims
1. A device for manufacturing a negative electrode, characterized in that: The device for manufacturing the negative electrode includes a pair of magnet plates, wherein the pair of magnet plates includes an upper magnet plate and a lower magnet plate respectively arranged above and below a plane where the negative electrode moves along a first direction, wherein each of the pair of magnet plates comprises a first vertical unit magnet and a second vertical unit magnet and a first horizontal unit magnet and a second horizontal unit magnet having magnetic force lines in different directions, and the directions of the magnetic force lines of the first horizontal unit magnet, the first vertical unit magnet, the second horizontal unit magnet, and the second vertical unit magnet are sequentially changed by 90 degrees each time along the second direction, and The upper magnet plate and the lower magnet plate include magnets of opposite polarities facing each other.
2. The device for manufacturing a negative electrode according to claim 1, characterized in that: The lengths of the first and second vertical unit magnets in the second direction may be the same as or different from the lengths of the first and second horizontal unit magnets in the second direction.
3. The device for manufacturing a negative electrode according to claim 1, characterized in that A ratio of the length of the first and second horizontal unit magnets in the second direction to the length of the first and second vertical unit magnets in the second direction is greater than 0.5 and less than 2.
67.
4. The device for manufacturing a negative electrode according to claim 1, characterized in that: The lengths of the first vertical unit magnet and the second vertical unit magnet in the first direction and the lengths of the first horizontal unit magnet and the second horizontal unit magnet in the first direction may be the same as or different from each other.
5. The device for manufacturing a negative electrode according to claim 1, characterized in that: The magnet plate includes two or more unit magnet columns, at least one unit magnet of the unit magnet columns is arranged parallel to the first direction, and the unit magnet columns have at least one unit magnet.
6. The device for manufacturing a negative electrode according to claim 5, characterized in that: One of the unit magnet columns includes two or more unit magnets, and the unit magnets include magnetic lines of force having the same direction as each other.
7. The device for manufacturing a negative electrode according to claim 5, characterized in that: One of the unit magnet columns includes two or more unit magnets having the same cross-sectional shape as each other.
8. The device for manufacturing a negative electrode according to claim 6, characterized in that: The lengths of two or more unit magnets included in the unit magnet array in the first direction may be the same or different.
9. The device for manufacturing a negative electrode according to claim 1, characterized in that: The thicknesses of the first and second vertical unit magnets and the thicknesses of the first and second horizontal unit magnets may be the same as or different from each other.
10. The device for manufacturing a negative electrode according to claim 1, characterized in that: The surfaces of the upper magnet plate and the lower magnet plate facing each other are parallel planes.
Citation Information
Patent Citations
Terminal component and secondary battery and assembled battery each including the terminal component
KR1020230022121A