Method for obtaining laminated curved glass
The process of partially dissolving the stack of thin layers with a first enamel layer and applying a second enamel layer addresses the issue of enamel degradation during bending, maintaining adhesion and aesthetic integrity in laminated glazing.
Patent Information
- Application Number
- FR2022008666
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Undesirable interactions occur during the bending process of laminated glazing when a sheet of glass coated with a stack of thin layers is also coated with an enamel layer, leading to degradation of the enamel's aesthetic appearance and adhesion, particularly when the stack contains nitride layers and the enamel contains bismuth, causing bubbles and reduced chemical resistance.
A process involving a first sheet of glass coated with a stack of thin layers, where a first layer of enamel is deposited, partially dissolves the stack during pre-firing, followed by the application of a second enamel layer, ensuring no sticking or transfer during bending, and subsequent lamination with an additional glass sheet.
The process prevents enamel degradation and maintains adhesion by dissolving the stack under the first enamel layer, ensuring a smooth bending process and preserving the enamel's optical and chemical properties.
Smart Images

Figure 00000017_0000 
Figure 00000017_0001 
Figure 00000017_0002
Abstract
Description
Title of the invention: Method for obtaining laminated curved glazing
[0001] The invention relates to the field of curved laminated glazing for motor vehicles, for example for roofs or windscreens, comprising a sheet of glass coated with a stack of thin layers and a layer of enamel.
[0002] Laminated glazing is glazing in which two sheets of glass are bonded together by means of a lamination interlayer. This interlayer helps to hold glass fragments together in the event of breakage, but also provides other functionalities, particularly in terms of burglary resistance or improved acoustic properties.
[0003] These glazings often include coatings of various types, intended to confer different properties.
[0004] Layers of enamel, generally black and opaque, are often deposited on part of the glazing, usually in the form of a peripheral band intended to conceal and protect against ultraviolet radiation the polymer seals used to fix and position the glazing on the body frame. Enamelled areas also conceal the fixing points of the interior rearview mirror and various connectors and sensors.
[0005] In laminated glazing, these enamel layers are generally arranged on face 2, the faces being traditionally numbered starting from the face intended to be positioned on the exterior of the vehicle. Face 2 is therefore a face in contact with the lamination interlayer. The aesthetic appearance of the enamel layer as seen from the outside of the vehicle is of particular importance to automotive manufacturers. The enamel is generally obtained by firing a composition comprising a glass frit and pigments at temperatures above 500°C. A glass frit consists of fine particles of low-melting-point glass, which, under the effect of a firing heat treatment, softens and adheres to the glass sheet. This forms a mineral layer, generally opaque, with high chemical and mechanical resistance, adhering perfectly to the glass while retaining the pigment particles.The baking stage is usually carried out simultaneously with the curving of the glass sheet.
[0006] In the context of manufacturing laminated glass, the two glass sheets of the glazing are often curved together, with the glass sheet intended to be positioned inside the vehicle generally placed on top of the other glass sheet, which bears the enamel. In other processes, each glass sheet is curved separately. In all cases, it is necessary for the enamel to have non-stick properties to prevent any sticking between the two sheets of glass or between the glass sheet and the bending tools during the bending process. To achieve this, bismuth-containing enamels are usually used; that is, enamels obtained from glass frits containing bismuth oxide, generally bismuth borosilicates.
[0007] Coatings, generally in the form of stacks of thin films, may also be present on one of the glass panes of laminated glazing. These may include electrically conductive layers, which can provide two types of functionality. On the one hand, when current is supplied, these electrically conductive layers can dissipate heat by the Joule effect. These are then heating layers, useful, for example, for defrosting or demisting. On the other hand, these layers exhibit solar control or low-emissivity properties due to their reflection of infrared radiation. These layers are therefore valued for improving thermal comfort or for the energy savings they provide by reducing consumption for heating or air conditioning.These stacks of layers are generally arranged on face 3 of the laminated glazing, therefore also in contact with the lamination interlayer.
[0008] However, in certain cases which will be detailed later, it may be advantageous to place the enamel layer and the stack of thin layers on the same sheet of glass, and therefore on the same face of the sheet of glass in question so that these coatings are protected inside the laminated glazing.
[0009] However, it has been observed that when a glass sheet coated with a stack of thin films is to be provided with a layer of enamel, undesirable interactions can occur during the curvature between the stack and the enamel, leading in particular to a degradation of the aesthetic appearance of the enamel. In particular, it has been observed, especially when the stack contained at least one nitride layer and the enamel contained bismuth, that bubbles form within the enamel, near the interface between the latter and the stack, causing a significant decrease in enamel adhesion, altering its optical appearance (in particular the color on the glass side, i.e., the side opposite the enamel) and reducing its chemical resistance, especially to acids.
[0010] Several solutions have been proposed to this problem.
[0011] It is possible to remove the thin-layer stack beforehand in the areas where the enamel layer is to be deposited, for example by means of abrasives, so that the enamel is deposited in direct contact with the glass sheet and to avoid any adhesion problems between the enamel layer and the thin-layer stack. However, mechanical abrasion generates visible scratches, including on the enamel layer.
[0012] Application WO 2014 / 133929, and before it application WO0029346, proposed the idea of using special glass frits for the enamel. These frits, during firing or pre-firing, dissolve the stack of thin layers and adhere directly to the glass. However, such enamels do not possess good non-stick properties, resulting in the two glass sheets sticking together during the bending process. Application WO 2022 / 074333 proposes, to avoid this sticking, depositing refractory particles based on oxides, carbides, or metals onto the enamel, with a size of at least 30 µm. However, on the one hand, the particle deposition step is difficult to implement on an industrial scale, and on the other hand, enamel transfer is sometimes observed when the glass sheets are bent separately by pressing.
[0013] Application WO 2019 / 106264 proposes modifying the thin-film stack by adding an oxide layer between the stack and the bismuth-containing enamel. However, such a modification is not always possible.
[0014] The invention aims to overcome these drawbacks.
[0015] To this end, the invention relates to a method for obtaining laminated curved glazing, in particular for windshields or roofs of motor vehicles, comprising the following successive steps: a. the supply of a first sheet of glass, coated on at least part of one of its faces with a stack of thin layers, b. a step of depositing, on a part of the surface of the stack of thin layers, a first layer of enamel, c. a pre-firing stage of the first glaze layer during which the stack of thin layers located beneath the first glaze layer is at least partially dissolved by said first glaze layer d. a step of depositing, at least on a part of the first enamel layer, a second enamel layer different from the first enamel layer, e. a step of curving the first sheet of glass, the stack of thin layers located under the first layer of enamel being totally dissolved by said first layer of enamel at least at the end of this step, then f. a step of laminating said first sheet of glass with an additional sheet of glass by means of a laminating interlayer, so that the enamel layers are turned towards said interlayer.
[0016] The invention also relates to a curved laminated glazing, particularly for windshields or motor vehicle roofs, obtained by the process of the invention, comprising a first sheet of glass coated, on part of one of its faces, with a stack of thin layers, and, on another part of the same face, with a first layer enamel itself coated on at least part of its surface with a second layer of enamel different from the first layer of enamel, said first sheet of glass being laminated with an additional sheet of glass by means of a lamination interlayer, said layers of enamel being turned towards said lamination interlayer.
[0017] Dissolving the thin-film stack with the first enamel layer prevents the aforementioned interactions. The constituent elements of the stack are dissolved in the enamel layer, which, at least after the bending step (step e), is in direct contact with the glass sheet. The application of a second enamel layer prevents any sticking or transfer, regardless of the bending process used.
[0018] In this text, the stack of thin layers and the layers of enamel are collectively referred to as "the coatings". Step a
[0019] The first sheet of glass can be flat or curved. The first sheet of glass is generally flat at the time of deposition of the stack of thin layers and then the enamel layer, and is subsequently curved during step e. The first sheet of glass is therefore curved in the curved laminated glazing according to the invention.
[0020] The glass of the first sheet of glass is typically a soda-lime silicate glass, but other glasses, for example borosilicates or aluminosilicates, can also be used. The first sheet of glass is preferably obtained by flotation, that is to say, by a process consisting of pouring molten glass onto a bath of molten tin.
[0021] The first sheet of glass may be clear or tinted, preferably tinted, for example green, gray, or blue. To achieve this, the chemical composition of the first sheet of glass advantageously comprises iron oxide, in a weight content ranging from 0.5 to 2%. It may also comprise other coloring agents, such as cobalt oxide, chromium oxide, nickel oxide, erbium oxide, or selenium.
[0022] The first sheet of glass preferably has a thickness in the range of 0.7 to 19 mm, in particular 1 to 10 mm, particularly 2 to 6 mm, or even 2 to 4 mm.
[0023] The lateral dimensions of the first glass pane (and the additional glass pane) are to be adapted according to those of the laminated glazing into which it is intended to be integrated. The first glass pane (and / or the additional glass pane) preferably has a surface area of at least 1 m².
[0024] The first sheet of glass is preferably coated with the stack of thin films over at least 70%, in particular over at least 90%, or even over the entire surface of the surface of the glass sheet face. Some areas may indeed be left uncoated, in particular to provide communication windows allowing the passage of waves.
[0025] The stack of thin layers is preferably in contact with the glass sheet. During its deposition, the first layer of enamel is preferably in contact with the stack of thin layers. It is then in direct contact with the glass after curving.
[0026] In this text, "contact" means physical contact. The expression "based on" preferably means that the layer in question comprises at least 50% by weight of the material considered, in particular 60%, or even 70%, 80%, or 90%. The layer may even essentially consist of this material. "Essentially consist" means that the layer may contain impurities without affecting its properties. The terms "oxide" or "nitride" do not necessarily mean that the oxides or nitrides are stoichiometric. They may, in fact, be substoichiometric, overstoichiometric, or stoichiometric.
[0027] The stack preferably comprises at least one nitride-based layer. The nitride is, in particular, a nitride of at least one element selected from aluminum, silicon, zirconium, and titanium. It may comprise a nitride of at least two or three of these elements, for example, a silicon-zirconium nitride, or a silicon-aluminum nitride. Preferably, the nitride-based layer is a silicon nitride-based layer, more particularly a layer consisting essentially of a silicon nitride. When the silicon nitride layer is deposited by sputtering, it generally contains aluminum, since it is common practice to dope silicon targets with aluminum to accelerate deposition rates.
[0028] The nitride-based layer preferably has a physical thickness in the range of 2 to 100 nm, in particular 5 to 80 nm.
[0029] Nitride-based layers are commonly used in many thin-film stacks because they possess advantageous blocking properties, in that they prevent the oxidation of other layers present in the stack, in particular functional layers which will be described below.
[0030] The stack preferably comprises at least one functional layer, in particular an electrically conductive functional layer. The functional layer is preferably sandwiched between two thin dielectric layers, at least one of which is a nitride-based layer. Other possible dielectric layers are, for example, oxide or oxynitride layers.
[0031] At least one electrically conductive functional layer is advantageously chosen among : - metallic layers, especially silver or niobium, or even gold, and - layers of a transparent conductive oxide, especially chosen from indium tin oxide, doped tin oxides (for example with fluorine or antimony) and doped zinc oxides (for example with aluminium or gallium).
[0032] These coatings are particularly valued for their low emissivity, which gives the glazing excellent thermal insulation properties. In glazing for land vehicles, particularly automobiles, railways, as well as aircraft and ships, low-emissivity glazing reflects some of the solar radiation outwards in hot weather, thus limiting the heating of the vehicle's interior and, where necessary, reducing air conditioning costs. Conversely, in cold weather, this glazing retains heat inside the passenger compartment, consequently reducing heating energy consumption. The same principle applies to glazing used in buildings.
[0033] According to a preferred embodiment, the thin-film stack comprises at least one silver layer, in particular one, two, three, or even four silver layers. The physical thickness of the silver layer, or where applicable the sum of the thicknesses of the silver layers, is preferably between 2 and 50 nm, in particular between 3 and 40 nm.
[0034] According to another preferred embodiment, the thin-film stack comprises at least one layer of indium tin oxide. Its physical thickness is preferably between 30 and 200 nm, in particular between 40 and 150 nm.
[0035] In order to protect the or each electroconductive thin film (whether metallic or based on a transparent conductive oxide) during the bending step, each of these layers is preferably sandwiched between at least two dielectric layers. The dielectric layers are preferably based on an oxide, nitride, and / or oxynitride of at least one element selected from silicon, aluminum, titanium, zinc, zirconium, and tin.
[0036] At least part of the thin film stack can be deposited by various known techniques, for example by chemical vapor deposition (CVD), or by cathodic sputtering, in particular assisted by a magnetic field (magnetron process).
[0037] Thin film stacking is preferably deposited by sputtering, particularly magnetically assisted sputtering. In this process, a plasma is created under high vacuum in the vicinity of a target containing the chemical elements to be deposited. The active species of the plasma, by bombarding the target, detach these elements, which are then deposited onto the glass sheet, forming the desired thin film. This process is called "reactive" when the film is made of a resulting material of a chemical reaction between the elements removed from the target and the gas contained in the plasma. The major advantage of this process lies in the possibility of depositing a very complex stack of layers on the same line by successively passing the glass sheet under different targets, generally in a single device.
[0038] The aforementioned stacks possess electrical conduction and infrared reflection properties useful for providing a heating function (defrosting, demisting) and / or a thermal insulation function.
[0039] When the stack of thin films is intended to provide a heating function, current supply points must be provided. These may, in particular, consist of silver paste strips screen-printed onto the stack of thin films at two opposite edges of the glass sheet. Layers of enamel
[0040] The following details apply equally to the first layer of enamel and to the second layer of enamel.
[0041] In this text, the term "enamel composition" refers to the liquid compositions used to deposit the wet enamel layers during steps b and d. The term "enamel layer" is used to describe the layer at each stage of the process, both the wet layer (before doming or even before pre-firing, if applicable before drying) and the final layer (after firing).
[0042] In steps b and d, the enamel layer is preferably deposited from an enamel composition comprising at least one pigment, at least one glass frit, and the refractory particles. Neither the enamel composition nor the enamel layer preferably comprises lead oxide.
[0043] The enamel composition (for both the first and second enamel layers) generally also includes an organic medium, intended to facilitate the application of the composition to the substrate and its temporary adhesion to the substrate, and which is removed during the pre-firing or firing of the enamel. The medium typically comprises solvents, thinners, oils, and / or resins.
[0044] The pigments preferably comprise one or more oxides selected from chromium, copper, iron, manganese, cobalt, and nickel oxides. For example, they may be copper and / or iron chromates. The pigments are preferably black for the first enamel layer, and advantageously also for the second enamel layer.
[0045] The first layer of enamel is preferably applied by screen printing. To do this, a screen printing screen, which has a mesh with some closed openings, is placed on the glass sheet. The enamel composition is then deposited onto the screen, and a squeegee is applied to force the enamel composition into The material passes through the screen in areas where the screen mesh is not closed, forming a layer of wet enamel. The first layer of enamel can also be applied using digital printing.
[0046] The deposition of the second layer of enamel is preferably carried out by screen printing, as described in the preceding paragraph, or by digital printing.
[0047] Digital printing (particularly inkjet printing) is preferably carried out using a print head whose movement (in particular its position and speed) is controlled by a computer, or using a series of fixed print heads past which the glass moves at a controlled speed. To achieve this, the print head(s) include nozzles through which drops of ink are projected locally onto the sheet of glass. This technique is sometimes called "drop on demand" (DOD).
[0048] The thickness of the first and / or second layer of wet enamel is preferably between 15 and 40 pm, in particular between 20 and 30 pm.
[0049] Step b and / or step d is preferably immediately followed by a drying step, intended to remove at least some of the solvent contained in the enamel composition. Such drying is typically carried out at a temperature between 120 and 180°C. Step b
[0050] The glass frit of the first enamel layer is capable of dissolving the underlying layer stack. Preferably, the glass frit is based on borosilicate, or borate, bismuth, and zinc. In order to make it more "aggressive" towards the layer stack, the bismuth and / or boron contents are preferably higher, and / or the silica content is preferably lower (and may even be zero), than those of glass frits usually used.
[0051] The stack is preferably coated by the first layer of enamel over 2 to 25%, in particular 3 to 20%, or even 5 to 15% of its surface. The first layer of enamel preferably includes a peripheral band, that is to say a band closed upon itself which, from each point on the periphery of the first sheet of glass, extends inwards from the first sheet of glass over a certain width, generally variable, typically between 1 and 20 cm. Step d
[0052] The second layer of enamel is deposited at least on part of the first layer of enamel. Preferably, it is deposited only on the entire surface of the first layer of enamel. In practice, perfect alignment between the two layers of enamel can easily be achieved by digital printing, but is more difficult to achieve with screen printing. It is therefore possible that an area of the first The first layer of enamel may not be coated with the second layer of enamel, or conversely, an area of the second layer of enamel may be deposited directly onto the first sheet of glass, typically over a width of 0.1 to 1 mm. Alternatively, the second layer of enamel may be in direct contact with the first sheet of glass over a wider area, and in this case, a transition zone, for example based on a gradient of dots, may be advantageously created.
[0053] The second enamel layer is different from the first enamel layer. Typically, the chemical composition of the glass frit used for the second enamel layer is different from that used for the first enamel layer.
[0054] The second enamel layer is preferably deposited from an enamel composition comprising a glass frit based on bismuth borosilicate, or even on bismuth and zinc borosilicate. The second enamel layer therefore preferably comprises a vitreous or glass-crystalline binder based on bismuth borosilicate, or even on bismuth and zinc borosilicate.
[0055] Preferably, the bismuth content is reduced and / or the silica content is increased, compared to the glass frit used for the first layer of enamel, in order to avoid any reaction between the two layers of enamel during the curving which could lead to the appearance of an undesirable tint.
[0056] Such enamels have the advantage of preventing the sticking or transfer of enamel during the bending step, whether between the first sheet of glass and the bending tools, when the first sheet of glass is bent alone, or between the first sheet of glass and the additional sheet of glass, when they are bent together. Pre-cooking step (c)
[0057] The process includes, between step b and step d, a pre-firing step c of the first enamel layer during which the stack of thin layers located under the first enamel layer is at least partially dissolved by said first enamel layer.
[0058] The pre-cooking step is preferably carried out at a temperature between 150 and 800°C, in particular between 500 and 700°C.
[0059] Such pre-firing makes it possible to eliminate the organic medium, or in general any organic component possibly present in the enamel layer.
[0060] During pre-firing, the thin-layer stack is at least partially dissolved by the enamel layer. Depending on the temperature used and the type of enamel or stack, the stack may even be completely dissolved by the enamel layer during pre-firing. Alternatively, it may only be partially dissolved during pre-firing, and then completely dissolved during doming (step e).
[0061] In particular, in the case where the first sheet of glass is curved on its own, particularly by pressing, it is not necessary to carry out a second pre-cooking between step d and step e. Step e
[0062] The curvature can be achieved in particular by gravity (the glass deforming under its own weight) or by pressing, at temperatures typically ranging from 550 to 650°C. The pressing can optionally be followed by rapid cooling in order to provide surface strengthening (tempering or hardening).
[0063] Preferably, the first sheet of glass is curved alone, notably by pressing. The two sheets of glass (first sheet of glass and additional sheet of glass) are then curved separately. In this case, it is important to avoid any sticking or transfer of enamel between the first sheet of glass and the curving tools.
[0064] According to another embodiment, the first glass sheet and the additional glass sheet are curved together, with the enamel layer facing the additional glass sheet. In this case, it is important to avoid any bonding between the two glass sheets. The glass sheets can be kept apart by placing an interlayer powder between them, ensuring a gap of a few tens of micrometers, typically 20 to 50 µm. The interlayer powder is, for example, based on calcium carbonate and / or magnesium carbonate. During the curving process, the inner glass sheet (intended to be positioned inside the passenger compartment) is normally placed on top of the outer glass sheet. Thus, during the curving step, the additional glass sheet is placed on top of the first glass sheet.This method is less preferred because in some cases it may require a pre-firing step between the application of the second layer of enamel and the doming step to prevent any sticking during doming.
[0065] Preferably, after step e, the first enamel layer is opaque and black. Its lightness L*, measured by reflection on the glass side, is preferably less than 5. As previously mentioned, it advantageously forms a band around the periphery of the first glass sheet. In this way, the enamel layer is able to conceal and protect against ultraviolet radiation from the seals, connectors, or sensors. The second enamel layer is also preferably opaque and black.
[0066] If the first layer of enamel has not already completely dissolved the stack of thin layers at the end of the pre-firing described below, this total dissolution is obtained during the doming, which completes the firing of the enamel.
[0067] The complete dissolution of the thin-film stack can be observed, in particular, by electron microscopy. Electrical measurements, especially of square resistance, also allow the dissolution of the stack to be observed. Step f
[0068] The lamination step can be carried out by autoclave treatment, for example at temperatures of 110 to 160°C and under a pressure of 10 to 15 bar. Prior to autoclave treatment, the air trapped between the glass sheets and the lamination interlayer can be removed by calendering or by vacuum.
[0069] As previously stated, the additional sheet is preferably the inner sheet of the laminated glazing, that is, the sheet located on the concave side of the glazing, intended to be positioned inside the vehicle's passenger compartment. In this way, the coatings are arranged on face 2 of the laminated glazing.
[0070] The additional glass sheet may be made of soda-lime silicate glass, or of borosilicate or aluminosilicate glass. It may be clear or tinted glass. Its thickness is preferably between 0.5 and 4 mm, in particular between 1 and 3 mm.
[0071] According to a preferred embodiment, the additional glass sheet has a thickness of between 0.5 and 1.2 mm. The additional glass sheet is, in particular, made of sodium aluminosilicate glass, preferably chemically strengthened. The additional glass sheet is preferably the inner sheet of the laminated glazing. The invention is particularly useful for this type of configuration, for which it is difficult to arrange the stack of thin layers on face 3. Chemical strengthening (also called "ion exchange") consists of contacting the surface of the glass with a molten potassium salt (for example, potassium nitrate), so as to strengthen the surface of the glass by exchanging ions in the glass (here, sodium ions) for ions of a larger ionic radius (here, potassium ions). This ion exchange makes it possible to create compressive stresses on the surface of the glass and over a certain thickness.Preferably, the surface stress is at least 300 MPa, particularly 400 and even 500 MPa, and at most 700 MPa, and the thickness of the compression zone is at least 20 µm, typically between 20 and 50 µm. The stress profile can be determined using a polarizing microscope equipped with a Babinet compensator. The chemical quenching step is preferably carried out at a temperature ranging from 380 to 550°C, and for a duration ranging from 30 minutes to 3 hours. Chemical strengthening is preferably carried out after the bending step but before the lamination step. The resulting glazing is preferably a motor vehicle windshield, in particular a heated windshield.
[0072] According to another preferred embodiment, the additional glass sheet has on the face opposite the face turned towards the laminating interlayer (preferably face 4, the additional sheet being the inner sheet) an additional stack of thin films, in particular a low-emissivity stack, comprising a transparent conductive oxide, in particular indium tin oxide (ITO). The invention is also particularly useful for this type of configuration, where it is difficult to arrange stacks of thin films on both sides of the same glass sheet (faces 3 and 4). In this embodiment, the lamination interlayer and / or the additional glass sheet is preferably tinted, while the glass sheet bearing the coatings can be made of clear glass. The resulting glazing is preferably a motor vehicle roof.
[0073] As an example of this latter preferred embodiment, we can cite a domed laminated roof comprising, from the outside of the vehicle, a clear glass sheet coated on face 2 with a stack of thin films comprising at least one layer of silver and then a layer of enamel, a tinted PVB laminate interlayer, and an additional tinted glass sheet, bearing on face 4 a stack of low-emissivity thin films, in particular based on ITO.
[0074] The lamination interlayer preferably comprises at least one sheet of polyvinylacetal, in particular polyvinylbutyral (PVB).
[0075] The lamination interlayer can be tinted or untinted in order to regulate the optical or thermal properties of the glazing if necessary.
[0076] The lamination interlayer may advantageously possess sound-absorbing properties in order to absorb airborne or structure-borne sounds. In particular, it may be made up of three polymer sheets, including two outer sheets of PVB framing an inner polymer sheet, possibly also made of PVB, with a lower hardness than the outer sheets.
[0077] The lamination interlayer may also possess thermal insulation properties, in particular infrared radiation reflection. For this purpose, it may comprise a low-emissivity thin-film coating, for example, a coating comprising a thin silver layer or a coating alternating dielectric layers with different refractive indices, deposited on an inner PET sheet framed by two outer PVB sheets.
[0078] The thickness of the lamination interlayer is generally in the range of 0.3 to 1.5 mm, in particular 0.5 to 1 mm. The lamination interlayer may have a lower thickness at an edge of the glazing than at the center of the glazing in order to avoid the formation of a double image when using a head-up display (HUD) system. Examples
[0079] The following embodiments illustrate the invention in a non-limiting manner, in relation to [Fig.1].
[0080] [Fig. 1] schematically illustrates an embodiment of the process according to the invention. It represents a schematic cross-section of a portion of the glass sheets and the elements deposited on the glass sheets, near their periphery. The various elements are obviously not represented to scale, so that they can be visualized.
[0081] The first sheet of glass 10 coated with the stack of thin layers 12 is provided in step a, then part of the stack 12 is coated with a first layer of enamel 14, in particular by screen printing (step b).
[0082] The assembly then undergoes a pre-firing (step c), which in the case represented leads to a partial dissolution of the stack 12 by the enamel 14. Alternatively, the dissolution may be total.
[0083] A second layer of enamel 16 is then deposited on the first layer of enamel 14 (step d), in particular by screen printing or digital printing. In the illustrated example, the overlap is perfect, but as described previously, the second layer of enamel 16 may also "overflow" the first layer of enamel 14 or, conversely, not cover the entirety of the latter, preferably over a small width, for example 0.5 or 1 mm.
[0084] The first sheet of glass 10 is then curved, for example by pressing (step e). Since the view shown is only that of the end of the sheet of glass, the curvature is not depicted here. The diagram illustrates the fact that, after curvature, the first layer of enamel 14 has completely dissolved the underlying stack of thin layers 12.
[0085] In step f, the first glass sheet 10 coated with the stack of thin films 12 and the enamel layers 14 and 16 and an additional glass sheet 20 coated with an additional stack of thin films 22 are assembled using the lamination interlayer 30. The diagram here represents each of the separate elements, in exploded view.
[0086] The process implemented by the examples corresponds to the embodiment of [Fig.1].
[0087] 2.1 mm thick glass sheets, previously coated by cathodic sputtering with a stack of thin films comprising three silver layers protected by zinc oxide layers, silicon nitride layers and NiCr blockers, were screen-coated with bismuth borate-based enamel layers with a wet thickness of 25 pm.
[0088] The enamel was then dried (150°C, 1 to 2 minutes) and then pre-fired at approximately 640°C-680°C, resulting in complete dissolution of the stack. The reflectance L* (illuminating D65, reference observer 10°) on the glass side was 4.0 after this step.
[0089] A second layer of bismuth and zinc borosilicate-based enamel (according to tests, enamels marketed under references 1T1417 by Fenzi, and 14331 or 14251 by Vibrantz) was then screen-printed onto the first layer of enamel.
[0090] The first sheet of glass thus coated was then curved by pressing against a form at a temperature of 630-660°C.
[0091] At the end of this step, the value of L* was 4.4 in the case of enamels 14331 and 14251 and 5.0 in the case of enamel 1T1417. The results in terms of bonding or enamel transfer were satisfactory, the best results being obtained with enamel 14251, which is richer in bismuth and less rich in zinc.
[0092] In a comparative example, in the absence of a second layer of enamel, some of the enamel remained stuck to the fabric of the form and fabric marks were observed on the enamel.
[0093] The first sheet of glass was then laminated with an additional sheet of soda-lime silico-glass having on face 4 a stack comprising a layer of ITO.
Claims
Claims
1. Method for obtaining laminated curved glazing, in particular for a motor vehicle windshield or roof, comprising the following successive steps: a. providing a first sheet of glass (10), coated on at least part of one of its faces with a stack of thin layers (12), b. a step of depositing, on part of the surface of the stack of thin layers (12), a first layer of enamel (14), c. a step of pre-firing the first layer of enamel (14) during which the stack of thin layers (12) located under the first layer of enamel (14) is at least partially dissolved by said first layer of enamel (14), d. a step of depositing, at least on part of the first layer of enamel (14), a second layer of enamel (16) different from the first layer of enamel (14), e.a step of bending the first glass sheet (10), the stack of thin layers (12) located under the first enamel layer (14) being completely dissolved by said first enamel layer (14, 16) at least at the end of this step, then f. a step of laminating said first glass sheet (10) with an additional glass sheet (20) by means of a laminating interlayer (30), so that the enamel layers (14) are turned towards said interlayer (30).
2. Method according to claim 1, such that the stack of thin layers (12) comprises at least one functional layer, in particular an electrically conductive functional layer.
3. Method according to the preceding claim, in which the at least one electroconductive functional layer is chosen from metallic layers, in particular silver or niobium, and layers of a transparent conductive oxide, in particular chosen from indium and tin oxide, doped tin oxides and doped zinc oxides.
4. Method according to one of the preceding claims, such that after step e, the first layer of enamel (14) is opaque, black in color, and forms a band at the periphery of the first sheet of glass (10).
5. Method according to one of the preceding claims, in which the deposition of the first layer of enamel (14) is produced by screen printing.
6. Method according to one of the preceding claims, in which the deposition of the second layer of enamel (16) is carried out by screen printing or by digital printing.
7. Method according to one of the preceding claims, in which the second enamel layer (16) is deposited from an enamel composition comprising a glass frit based on bismuth borosilicate, in particular based on bismuth borosilicate and zinc.
8. Method according to one of the preceding claims, in which during step e, the first glass sheet (10) is curved alone, in particular by pressing.
9. Method according to one of the preceding claims, in which the additional glass sheet (20) carries, on the face opposite the face facing the lamination interlayer (30), an additional stack of thin layers (22), in particular a low-emissivity stack comprising a transparent conductive oxide.
10. Laminated curved glazing, in particular for a windshield or roof of a motor vehicle, obtained by the method of one of the preceding claims, comprising a first glass sheet (10) coated, on a part of one of its faces, with a stack of thin layers (12), and, on another part of the same face, with a first enamel layer (14) itself coated on at least a part of its surface with a second enamel layer (16) different from the first enamel layer (14), said first glass sheet (10) being laminated with an additional glass sheet (20) by means of a lamination interlayer (30), said enamel layers (14, 16) being turned towards said lamination interlayer (30).