Black complex oxide particle
Black composite oxide particles with controlled Fe, Mg, and Al ratios and Cl content address blackness and magnetization issues, ensuring stable volume resistivity and safety for various applications.
Patent Information
- Application Number
- JP2023045378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Existing inorganic black pigments face issues with blackness, cohesiveness due to magnetic force, and fluctuations in volume resistivity under varying environmental conditions, particularly in toner applications.
Black composite oxide particles composed of specific ratios of Fe, Mg, and Al, with controlled crystallinity and particle size, and adjusted Cl content, to achieve high safety, excellent blackness, low magnetization, and stable volume resistivity.
The particles provide high safety, excellent blackness, low magnetization, and minimal environmental variation in volume resistivity, making them suitable for paints, printing inks, toners, rubbers, plastics, and ceramics.
Smart Images

Figure 2024134926000001 
Figure 2024134926000002
Abstract
Description
Technical Field
[0001] The present invention mainly relates to black composite oxide particles suitable as black pigments for paints, printing inks, toners, rubber / plastics, and ceramics.
Background Art
[0002] Black pigments used in applications such as paints, printing inks, toners, rubber / plastics, and ceramics are required to have characteristics such as blackness, coloring power, and hiding power, and to be inexpensive. As inorganic black pigments, carbon black, iron oxide-based pigments represented by magnetite, and other composite oxide pigments are widely used.
[0003] In these inorganic black pigments, it is generally required to have a particle size in the nanometer to sub-micron range. In particular, regarding carbon black, various alternative pigments have been studied due to concerns about safety.
[0004] Patent Document 1 proposes black composite oxide particles containing a composite oxide containing Fe, Mg, and Al as metal components, where the amount of Fe is 30 to 55% by mass and the atomic ratio of Fe 3+ / Fe 2+ is 0.8 to 10, the amount of Mg is 1 to 10% by mass, and the amount of Al is 1 to 10% by mass. Patent Document 2 proposes Mg x Fe y O(Fe2O3) 1+z (where 0.3 < x < 1, 0 < y < 0.7, x + y = 1, 0 < z < 0.5) and Mg-containing black iron oxide particles with an average particle size of 0.01 to 0.5 μm. Patent Document 3 proposes a composite oxide black pigment that is a composite oxide of main component metals containing copper, manganese, and aluminum, and the content ratio of each metal to the total of the metal elements is 25 to 45 mol% for copper, 25 to 70 mol% for manganese, and 2 to 40 mol% for aluminum, and substantially does not contain chromium, cobalt, and nickel.
Prior Art Documents
[0005] [Patent Document 1] JP 2003-238164 A [Patent Document 2] JP 2003-286030 A [Patent Document 3] JP 2015-98509 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, inorganic oxide pigments as described in Patent Documents 1 to 3 have problems with blackness and coagulation due to magnetic force compared to carbon black. On the other hand, inorganic oxide pigments are easier to make high resistivity than carbon black, and when used in toner, they have the characteristic that it is easy to control the resistance and chargeability to an appropriate level, but it is necessary to reduce the fluctuation of the chargeability of the toner under high temperature and high humidity conditions and low temperature and low humidity conditions. In particular, since a large amount of pigment is added as a colorant in black toner, it is required to suppress the environmental fluctuation of the volume resistivity in order to reduce the effect of this environmental fluctuation of the charge amount.
[0007] Therefore, an object of the present invention is to provide black complex oxide particles which are highly safe, have excellent blackness, low magnetization, and little variation in volume resistivity due to environmental factors. [Means for solving the problem]
[0008] As a result of intensive research into the above-mentioned problems, the present inventors have found that black complex oxide particles that are highly safe, have excellent blackness, low magnetization, and have little variation in volume resistivity due to the environment can be obtained by containing specific contents of Fe, Mg, and Al as metal components, having a half-width indicating crystallinity in a specific range, and containing a specific content of Cl.
[0009] That is, the present invention relates to a method for producing a steel sheet comprising the steps of: When the Fe content is W1 weight%, the Mg content is W2 weight%, and the Al content is W3 weight%, the following formula is satisfied: 42≦W1≦60 4≦W2≦11 4≦W3≦11 Fulfilling The half-width of the diffraction peak based on the (311) plane, which shows a spinel structure in X-ray crystal structure analysis, is 0.100° or more and 0.220° or less; Furthermore, the present invention provides black complex oxide particles containing Cl in an amount of 5 ppm or more and 100 ppm or less.
[0010] The black complex oxide particles according to the present invention are formed by mixing a compound represented by the following formula: 0.07≦W2 / W1≦0.26 0.07≦W3 / W1≦0.26 0.4≦W3 / W2≦2.3 It is preferable that the following is satisfied.
[0011] The black complex oxide particles according to the present invention have a volume cumulative 50% particle diameter D50 of 0.05 μm or more and 0.7 μm or less, and a volume cumulative 90% particle diameter D90 of 1.0 μm or less, as measured by a laser diffraction scattering method; The volume cumulative 50% particle diameter D50 and the BET specific surface area S are expressed by the following formula: 1.3935×D50 -1.144 ≦S≦3.5303×D50 -0.974 It is preferable that the following is satisfied.
[0012] In the black complex oxide particles according to the present invention, it is preferable that the blackness L value, the hue a value, and the hue b value are 20 or less, 2.0 or less, and 2.0 or less, respectively, as measured by a color difference meter conforming to JIS K5101-1991.
[0013] In the black complex oxide particles according to the present invention, the saturation magnetization Ms in an applied magnetic field of 79.6 kA / m is 30 Am 2 It is preferable that the concentration is not more than 1 / kg.
[0014] In the black complex oxide particles according to the present invention, the common logarithm of volume resistivity RvH (Ωcm) under high temperature and high humidity conditions (30° C., relative humidity 80%) is preferably 7.0 or more.
[0015] In the black complex oxide particles according to the present invention, the environmental variation ratio of volume resistivity (log 10 RvL / log 10 It is preferable that RvH is 1.00 or more and 1.25 or less. Effect of the Invention
[0016] The black complex oxide particles according to the present invention are highly safe, have excellent blackness, low magnetization, and exhibit little variation in volume resistivity due to environmental factors. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The black complex oxide particles according to the present invention are composed of Fe, Mg, and Al as the main metal components. As oxides of each element, when only Fe is present, magnetite (Fe3O4), known as a black pigment, is generated, but when Mg is present, it reacts with Fe to generate brown magnesium ferrite (MgFe2O4), and when Al is present, hercynite (FeAl2O4), a black oxide, is generated. However, when three elements, Fe, Mg, and Al, are used, these elements exist in a solid solution in the spinel structure, so it is important to adjust them to a specific ratio in controlling blackness and magnetization.
[0018] The black complex oxide particles according to the present invention contain Fe, Mg, and Al as metal components, and when the Fe content is W1 weight %, the Mg content is W2 weight %, and the Al content is W3 weight %, the following formula is satisfied: 42≦W1≦60 4≦W2≦11 4≦W3≦11 It is important to satisfy the following.
[0019] In the black complex oxide particles according to the present invention, when the Fe content is less than 42% by weight, the magnetization is low but the blackness tends to be low. On the other hand, when the Fe content exceeds 60% by weight, the blackness is high but the magnetization tends to be high. Therefore, from the viewpoint of achieving both blackness and magnetization, it is important to satisfy 42≦W1≦60. W1 is preferably 45 or more, more preferably 47 or more. On the other hand, W1 is preferably 57 or less, more preferably 55 or less.
[0020] In the black complex oxide particles according to the present invention, if the Mg content is less than 4% by weight, the blackness tends to be high but the magnetization tends to be high. If the Mg content exceeds 11% by weight, the magnetization tends to be low but the blackness tends to be low. Therefore, from the viewpoint of achieving both blackness and magnetization, it is important to satisfy 4≦W2≦11. W2 is preferably 5 or more, and more preferably 6 or more. W2 is preferably 10 or less, and more preferably 9 or less.
[0021] In the black complex oxide particles according to the present invention, when the Al content is less than 4% by weight, the blackness is high but the magnetization tends to be high. On the other hand, when the Al content exceeds 11% by weight, the magnetization is low but the blackness tends to be low. Therefore, from the viewpoint of achieving both blackness and magnetization, it is important to satisfy 4≦W3≦11. W3 is preferably 5 or more, and more preferably 6 or more. On the other hand, W3 is preferably 10 or less, and more preferably 9 or less.
[0022] In the black complex oxide particles according to the present invention, it is preferable to further adjust the weight ratios of Mg and Al to Fe, and the weight ratio of Al to Mg, to achieve a better balance between the blackness and magnetization. 0.07≦W2 / W1≦0.26 0.07≦W3 / W1≦0.26 0.4≦W3 / W2≦2.3 It is preferable that the above ratio is satisfied. Within this range, blackness and magnetization can be more balanced. W2 / W1 is more preferably 0.10 or more, and more preferably 0.20 or less. W3 / W1 is more preferably 0.10 or more, and more preferably 0.20 or less. W3 / W2 is more preferably 0.6 or more, and more preferably 2.0 or less.
[0023] It is important that the black complex oxide particles according to the present invention further contain Cl in addition to Fe, Mg, and Al. However, if the Cl content is less than 5 ppm, the environmental variation of the volume resistivity under low temperature and low humidity tends to be relatively large. Also, if the Cl content exceeds 100 ppm, the environmental variation of the volume resistivity under high temperature and high humidity tends to be relatively large. Therefore, from the viewpoint of further stabilizing the environmental variation of the volume resistivity, it is important that the Cl content is 5 ppm or more and 100 ppm or less. The Cl content is preferably 10 ppm or more, and more preferably 20 ppm or more. Also, the Cl content is preferably 80 ppm or less, and more preferably 50 ppm or less.
[0024] It is important that the half-width of the diffraction peak based on the (311) plane, which represents a spinel structure in X-ray crystal structure analysis, of the black complex oxide particles according to the present invention is 0.100° or more and 0.190° or less. When the half-width is less than 0.100, there are few lattice defects in the spinel structure, and the structure is close to a single spinel crystal structure, so that the magnetization tends to be high and the resistance tends to be low. When the half-width is greater than 0.190, the blackness tends to be low. The half-width is more preferably 0.120° or more and 0.170° or less. The half-width of the diffraction peak based on the (311) plane, which represents a spinel structure, can be appropriately adjusted by the manufacturing method such as wet or dry, the composition ratio of the metal components, the firing temperature, the firing atmosphere, etc.
[0025] In the black complex oxide particles according to the present invention, it is preferable to adjust the particle size distribution. Specifically, the volume cumulative 50% particle diameter D50 is preferably 0.05 μm or more and 0.7 μm or less, and more preferably 0.10 μm or more and 0.5 μm or less. By setting D50 to 0.05 μm or more, the desired blackness is easily obtained. In addition, by setting D50 to 0.7 μm or less, it becomes easy to disperse the toner having a particle size of several μm, and the desired color tone and characteristics of the toner are easily obtained. In addition, the volume cumulative 90% particle diameter D90 is preferably 1.0 μm or less, and more preferably 0.7 μm or less. By setting D90 to 1.0 μm or less, it becomes easy to disperse the toner having a particle size of several μm, and the desired color tone and characteristics of the toner are easily obtained. The lower limit of D90 can be, for example, 0.3 μm or more. The particle size distribution for calculating the above D50 and D90 can be measured by a laser diffraction scattering method.
[0026] In the black complex oxide particles according to the present invention, the volume cumulative 50% particle diameter D50 and the BET specific surface area S are expressed by the following formula: 1.3935×D50 -1.144 ≦S≦3.5303×D50 -0.974 It is preferable to satisfy the above. Since particles usually have a particle size distribution and surface irregularities cannot be completely eliminated, it is technically difficult to reduce the BET specific surface area below the above lower limit. By making the BET specific surface area equal to or less than the above upper limit, the particles do not have too many pores relative to the particle size, and are less susceptible to changes such as humidity. In addition, when used after surface treatment to make the particles hydrophilic or hydrophobic, the particles are not easily broken due to sufficient strength, and the untreated parts are not easily exposed, so the properties tend to be stable.
[0027] In the black complex oxide particles according to the present invention, when the blackness and hue are measured by a color difference meter conforming to JIS K5101-1991, it is preferable that the L value is 20 or less, the a value is 2.0 or less, and the b value is 2.0 or less. When these L values, a values, and b values satisfy the above conditions, the blackness is high and the hue has a weak reddish or yellowish tinge, making it suitable as a black pigment. The L value is more preferably 19 or less, and even more preferably 17 or less.
[0028] The black complex oxide particles according to the present invention have a saturation magnetization of 30 Am at a magnetic field of 79.6 kA / m, taking into consideration applications in fields not requiring magnetism, such as non-magnetic toner applications. 2 / kg or less, and 25Am 2 It is more preferable that the amount is not more than 1 / kg.
[0029] In the black complex oxide particles according to the present invention, from the viewpoint of maintaining the chargeability when added to a toner and suppressing a decrease in chargeability, particularly under high temperature and high humidity conditions (30° C., relative humidity 80%), the common logarithm of the volume resistivity RvH (Ωcm) under high temperature and high humidity conditions (30° C., relative humidity 80%) is preferably 7.0 or more, more preferably 7.5 or more. In addition, the environmental variation ratio of volume resistivity (log 10 RvL / log 10 RvH) is preferably from 1.00 to 1.25, and more preferably 1.20 or less.
[0030] The black complex oxide particles according to the present invention are usually produced by a dry method, for example, by measuring predetermined amounts of raw materials, pulverizing and mixing the resulting slurry, granulating the slurry, and firing the slurry at 1000° C. or higher and 1300° C. or lower in an inert atmosphere or a weakly oxidizing atmosphere.
[0031] The black complex oxide particles according to the present invention can also be produced by a wet method. However, compared to the dry method, there are many crystal nuclei for generating spinel crystals, but the crystals do not grow easily because of the reaction at a low temperature, and the half-width of the diffraction peak based on the (311) plane that represents the spinel structure tends to be large because of the low crystallinity. Therefore, the blackness is likely to be insufficient and the particles are likely to change over time. In addition, since the crystals do not grow easily, there are many voids in the particles, and the BET specific surface area relative to the particle diameter tends to be large. Therefore, the particles are susceptible to changes such as humidity and cause changes over time. There is also a method in which the particles are produced by a wet method and then sintered, but since there are many crystal nuclei, it is difficult to control the spinelization reaction, and the particles become too highly magnetized or sintered too much, which increases the hardness and makes it difficult to reduce the particle size. Furthermore, since the particles produced by the wet method have uniform crystal grains, when a magnetic field is applied, the magnetic moment is easily aligned, so that the particles tend to become highly magnetized.
[0032] As the raw material of Fe, it is preferable to use Fe2O3. As the raw material of Mg, it is preferable to use one or more compounds selected from Mg(OH)2, MgO, and MgCO3. As the raw material of Al, it is preferable to use Al2O3. As the raw material of Cl, a chlorine source such as magnesium chloride or sodium chloride can be used, but since it is a small amount compared to Fe, Mg, and Al, it is preferable to adjust the Cl content by Cl, which is a trace component contained in each of the above raw materials (especially Fe2O3). Note that Fe2O3 is preferably made from iron chloride as a raw material, since Fe2O3 made from iron sulfate or iron sulfate as a raw material contains almost no Cl and it is difficult to adjust it to a desired Cl content. In addition, the Cl content can also be adjusted by the firing temperature and firing time.
[0033] After weighing out the raw materials in an appropriate amount to obtain the desired elemental composition, they are ground and mixed in a ball mill or a vibration mill for 0.5 hours or more (preferably 1 hour or more and 20 hours or less), and the ground mixture is added with water and finely ground using a bead mill or the like to obtain a slurry. The degree of grinding can be controlled by adjusting the diameter, composition, and grinding time of the beads used as media. From the viewpoint of uniformly dispersing the raw materials, it is preferable to use fine beads having a particle size of 1 mm or less as media. In addition, in order to uniformly disperse the raw materials, it is preferable to grind the ground material so that the volume average particle size (50% cumulative volume particle size D50) is 2.5 μm or less, and more preferably 2.0 μm or less.
[0034] Next, it is preferable to add a dispersant, a binder, etc. to the obtained slurry as necessary to adjust the viscosity to 2 poise or more and 4 poise or less. Polyvinyl alcohol (PVA) or polyvinylpyrrolidone (PVP) can be used as the binder. Then, the slurry with the viscosity adjusted to the above range is sprayed using a spray dryer and dried to obtain a granulated product.
[0035] The obtained granules are preferably fired in an inert atmosphere or a weakly oxidizing atmosphere at a temperature of 1000 to 1300°C for 2 to 6 hours. The Cl content can also be controlled by the firing temperature and firing time. Here, an inert atmosphere or a weakly oxidizing atmosphere means that the oxygen concentration is 0.0% by volume to 0.1% by volume (1000 ppm). By setting the firing temperature at 1000°C or higher, the spinelization reaction is likely to occur, so that the blackness becomes high. By setting the firing temperature at 1300°C or lower, the blackness remains high and the crystal grain growth of spinelization does not proceed too much, the hardness becomes low, and it becomes easy to reduce the particle size by crushing or the like. From the viewpoint of blackness and hardness, the firing temperature is preferably 1100°C to 1250°C.
[0036] The obtained fired product can be pulverized to a desired particle size using a dry pulverizer such as a pin mill, a hammer mill, a bead mill, or a jet mill, or a wet bead mill. When wet pulverization is performed, the product is dried to obtain particles. In this case, an anti-aggregation agent such as a surfactant can be used to prevent agglomeration due to drying. Then, if necessary, the product is classified using an air classifier, to obtain particles having a desired particle size distribution.
[0037] The black complex oxide particles according to the present invention as described above are highly safe, have excellent blackness, low magnetization, and little variation in volume resistivity due to the environment. Because of their high safety and excellent blackness, they are suitable as black pigments for paints, printing inks, toners, rubbers and plastics, and ceramics. In addition, the black complex oxide particles according to the present invention are low in magnetization and little variation in volume resistivity due to the environment, and are therefore particularly suitable as black pigments for non-magnetic toners to replace carbon black and oxide pigments containing environmentally hazardous substances, which are less safe. The toner using the black complex oxide particles according to the present invention can reduce the impact on the natural environment and the human body, and can obtain high-quality printed matter. EXAMPLES
[0038] <Example 1> Weighed out 16.09 kg of Fe2O3 (iron chloride-based raw material, Cl content: 1500 ppm), 4.64 kg of Mg(OH)2, and 4.15 kg of Al2O3, and ground them using a dry media mill (vibration mill, 1 / 8 inch diameter stainless steel beads) for 6 hours (until D50 was about 5 μm). Then, water was added, and the mixture was ground using a wet media mill (horizontal bead mill, 1 mm diameter zirconia beads) for 6 hours. The particle size (primary particle size of the ground) of this slurry was measured using a microtrack, and D50 was about 2 μm. An appropriate amount of dispersant was added to the obtained slurry, and 0.4 wt% of PVA (10% solution) was added as a binder to the solid content, and then granulated using a spray dryer.
[0039] Thereafter, the mixture was kept in a tunnel-type electric furnace at a firing temperature of 1200°C and an oxygen concentration of 0.0% by volume for 3 hours. At this time, the heating rate was 200°C / hour, and the cooling rate was 150°C / hour. The obtained fired material was pulverized stepwise using a hammer mill (Maekawa Industries Co., Ltd.), a pin mill (Makino Sangyo Co., Ltd.), and a dynamic mill (Nippon Coke Industrial Co., Ltd.), and particles of the desired particle size were classified using an ultrafine powder classifier CNI (Nippon Pneumatic Industrial Co., Ltd.), to obtain black composite oxide particles.
[0040] <Example 2> Black complex oxide particles were obtained in the same manner as in Example 1, except that Fe2O3 (iron chloride-based raw material, Cl content: 900 ppm) was used instead of Fe2O3 used as the raw material in Example 1.
[0041] <Example 3> Black complex oxide particles were obtained in the same manner as in Example 1, except that the raw material used in Example 1 was changed from Fe2O3 to Fe2O3 (iron chloride-based raw material, Cl content: 2900 ppm) and the firing temperature was changed to 1150°C.
[0042] <Examples 4 to 8> Black complex oxide particles were obtained in the same manner as in Example 1, except that the compounding ratio of Fe2O3, Mg(OH)2, and Al2O3 used as raw materials in Example 1 was appropriately changed.
[0043] <Comparative Example 1> Black complex oxide particles were obtained in the same manner as in Example 1, except that the raw material used in Example 1 was changed from Fe2O3 to Fe2O3 (iron chloride-based raw material, Cl content: 3600 ppm) and the firing temperature was changed to 1150°C.
[0044] <Comparative Example 2> Black complex oxide particles were obtained in the same manner as in Example 1, except that the raw material used in Example 1 was changed from Fe2O3 to Fe2O3 (iron chloride raw material, Cl content: 900 ppm) and the firing temperature was changed to 1300°C. <Comparative Examples 3 to 9> Black complex oxide particles were obtained in the same manner as in Example 1, except that the compounding ratio of Fe2O3, Mg(OH)2, and Al2O3 used as raw materials in Example 1 was appropriately changed. In Comparative Example 9, the oxygen concentration during firing was set to 0.5% by volume.
[0045] <Comparative Example 10> Black composite oxide particles were obtained by a wet method. Specifically, 12.5 mol / L aqueous sodium hydroxide solution was added to 5 L of 0.15 mol / L aqueous sodium carbonate solution to adjust the pH to 11, and the liquid temperature was raised to 80° C. and maintained at that temperature. Meanwhile, 2 L of a mixed sulfate aqueous solution containing 0.75 mol / L ferrous sulfate, 0.10 mol / L ferric sulfate, 0.5 mol / L magnesium sulfate, and 0.25 mol / L aluminum sulfate was prepared and added to the alkaline aqueous solution containing sodium carbonate over a period of 30 minutes while mixing and stirring.
[0046] After the addition was completed, mixing and stirring was continued for 4 hours. During this addition and mixing and stirring, the initial temperature and pH of the reaction solution were adjusted to be maintained. The slurry containing the black complex oxide particles thus obtained was naturally cooled, neutralized to pH 6 using dilute sulfuric acid, and then washed, dehydrated, and dried by conventional methods to obtain the final black complex oxide particles.
[0047] The black complex oxide particles obtained in Examples 1 to 8 and Comparative Examples 1 to 10 were evaluated for the following points. The results are shown in Table 1 (Examples 1 to 8) and Table 2 (Comparative Examples 1 to 10).
[0048] <Concentration of metal components in black composite oxide particles> The content of metal components in the black complex oxide particles was determined by chemical analysis (ICP). Specifically, 0.2 g of black complex oxide particles was weighed out, and 60 ml of pure water, 20 ml of 1N hydrochloric acid, and 20 ml of 1N nitric acid were added to the black complex oxide particles and heated to prepare an aqueous solution in which the black complex oxide particles were completely dissolved. The resulting aqueous solution was placed in an ICP analyzer (ICPS-1000IV, manufactured by Shimadzu Corporation) to measure the content of the metal components Fe, Mg, and Al.
[0049] <Cl content in raw material or black composite oxide particles> The Cl content in the raw material or the black complex oxide particles was measured by combustion ion chromatography under the following conditions. -Combustion equipment: Mitsubishi Chemical Analytech AQF-2100H -Sample size: 50mg - Combustion temperature: 1100℃ - Burn time: 10 minutes -Ar flow rate: 400ml / min -O2 flow rate: 200ml / min -Humidifying Air flow rate: 100ml / min -Absorption solution: eluent containing 1% hydrogen peroxide -Analyzer: Tosoh IC-2010 -Column: TSKgel SuperIC-Anion HS (4.6mmI.D.×1cm+4.6mmI.D.×10cm) -Eluent: NaHCO3(3.8mmol / L)+Na2CO3(3.0mmol / L) -Flow rate: 1.5mL / min -Column temperature: 40℃ -Injection volume: 30μL - Measurement mode: Suppressor method -Detector: CM detector -Standard sample: Kanto Chemical Co., Ltd. anion mixed standard solution
[0050] <Full width at half maximum of the diffraction peak due to the (311) plane that represents the spinel structure> The half-width (°, 2θ) of the diffraction peak based on the (311) plane, which is the main peak of the spinel phase, was measured by powder X-ray diffraction under the following measurement conditions. -X-ray diffraction equipment: PANalytical X'pert MPD (including high-speed detector) - Source: Co-Kα -Tube voltage: 45kV -Tube current: 40mA -Scanning mode: General batch - Divergence slit(°):1 / 2 - Light-receiving slit (mm): 5.5 - Measurement interval: 0.010° / second - Counting time (seconds): 10.16 / step - Scanning range (2θ): 15~90°
[0051] <Particle size distribution> The particle size distribution of the black composite oxide particles was measured by the laser diffraction scattering method. First, 10 g of the black composite oxide particles and 80 ml of water were placed in a 100-ml beaker, and 2 drops of sodium hexametaphosphate were added as a dispersant. Next, the black composite oxide particles were dispersed using an ultrasonic homogenizer (UH-150 type, manufactured by SMT). At this time, the output level of the ultrasonic homogenizer was set to 4, and dispersion was carried out for 20 seconds. Then, the bubbles formed on the surface of the beaker were removed, and the obtained slurry was introduced into a laser diffraction type particle size distribution measuring device (SALD-7500nano, manufactured by Shimadzu Corporation) for measurement. By this measurement, the 50% diameter (volume cumulative 50% particle diameter D50) and 90% diameter (volume cumulative 90% particle diameter D90) in the volume particle size distribution were determined. The measurement conditions were a pump speed of 7, a built-in ultrasonic irradiation time of 30, and a refractive index of 1.70 - 050i.
[0052] <BET specific surface area> The BET specific surface area of the black composite oxide particles was measured using a specific surface area measuring device (Macsorb HM model-1208, manufactured by Mountech). First, about 10 g of the black composite oxide particles were placed on a medicine wrapping paper and degassed using a vacuum dryer to confirm that the vacuum degree was -0.1 MPa or less. Then, the black composite oxide particles were heated at 200°C for 2 hours to remove the moisture adhering to the surface of the black composite oxide particles. About 0.5~4 g of the moisture-removed black composite oxide particles were placed in a standard sample cell dedicated to the measuring device and accurately weighed using a precision balance. Next, the weighed black composite oxide particles were set in the measuring port of the measuring device for measurement. The measurement was performed by the one-point method. The measurement atmosphere was a temperature of 20°C and a relative humidity of 55%.
[0053] <Saturation magnetization> The black complex oxide particles were packed into a cell with an inner diameter of 5 mm and a height of 2 mm, and set in a vibrating sample magnetic measurement device (VSM-C7-10A, manufactured by Toei Kogyo Co., Ltd.) to measure the saturation magnetization of the black complex oxide particles in an applied magnetic field of 79.6 kA / m.
[0054] <Volume resistivity> First, the cross-sectional area is 4 cm 2 The black complex oxide particles were filled into a cylinder made of fluororesin to a height of 4 mm. Then, electrodes were attached to both ends, and a 1 kg weight was placed on top of the electrodes to measure the electrical resistance. The electrical resistance was measured using a Keithley 2182A nanovoltmeter, with a measurement voltage of 1000 V applied, and the resistance was measured 60 seconds later to calculate the volume resistivity. The measurement environments were room temperature and room humidity (temperature 20°C, relative humidity 55%), high temperature and high humidity (temperature 30°C, relative humidity 80%), and low temperature and low humidity (temperature 10°C, relative humidity 20%), and the common logarithm of each volume resistivity (room temperature and room humidity: RvN, high temperature and high humidity: RvH, low temperature and low humidity: RvL) was calculated. In addition, the environmental fluctuation ratio (log 10 RvL / log 10 RvH) was calculated.
[0055] <Blackness and hue> The blackness and hue of the black complex oxide particles were measured in accordance with JIS K5101-1991. Specifically, 1.4 cc of castor oil was added to 2.0 g of black complex oxide particles and kneaded with a Huber-type Marler. 7.5 g of lacquer was added to 2.0 g of the kneaded sample and further kneaded, and then the mixture was applied to a mirror-coated paper using a 4 mil applicator and dried. Then, the blackness (L value) and hue (a value, b value) were measured with a color difference meter (color analyzer TC-1800 type, manufactured by Tokyo Denshoku).
[0056] [Table 1]
[0057] [Table 2]
[0058] From the above results, it is clear that the black complex oxide particles obtained in Examples 1 to 8 are highly safe, have excellent blackness, low magnetization, and exhibit little variation in volume resistivity due to the environment.
Claims
1. Contains Fe, Mg, and Al as metal components; When the Fe content is W1 weight %, the Mg content is W2 weight %, and the Al content is W3 weight %, the following formula is satisfied: 42≦W1≦60 4≦W2≦11 4≦W3≦11 Fulfilling The half-width of the diffraction peak based on the (311) plane, which represents a spinel structure in X-ray crystal structure analysis, is 0.100° or more and 0.190° or less; Further, it contains Cl in an amount of 5 ppm or more and 100 ppm or less. Black complex oxide particles.
2. The following formula: 0.07≦W2 / W1≦0.26 0.07≦W3 / W1≦0.26 0.4≦W3 / W2≦2.3 Fulfill The black complex oxide particles according to claim 1.
3. The volume cumulative 50% particle diameter D50 measured by a laser diffraction scattering method is 0.05 μm or more and 0.7 μm or less, and the volume cumulative 90% particle diameter D90 measured by a laser diffraction scattering method is 1.0 μm or less. The volume cumulative 50% particle diameter D50 and the BET specific surface area S are expressed by the following formula: 1.3935×D50 -1.144 ≦S≦3.5303×D50 -0.974 Fulfill The black complex oxide particles according to claim 1.
4. When the blackness and hue are measured using a color difference meter conforming to JIS K5101-1991, the L value is 20 or less, the a value is 2.0 or less, and the b value is 2.0 or less. The black complex oxide particles according to claim 1 .
5. Saturation magnetization Ms is 30 Am at a load magnetic field of 79.6 kA / m. 2 / kg or less The black complex oxide particles according to claim 1 .
6. The common logarithm of volume resistivity RvH (Ωcm) under high temperature and high humidity conditions (30°C, relative humidity 80%) is 7.0 or more. The black complex oxide particles according to claim 1 .
7. The environmental variation ratio of volume resistivity (log 10 RvL / log 10 RvH) is 1.00 or more and 1.25 or less. The black complex oxide particles according to claim 1 .
Citation Information
Patent Citations
Electrophotographic developing carrier, two-component developer and image forming method
JP1997211897A
Black compound oxide particle and its production method
JP2003238164A
Black compound oxide particle / powder having ability to reflect infrared light and its manufacturing method, and black pigment, and paint and resin composition using black pigment having ability to reflect infrared light
JP2008044805A
Carrier core material for electrophotographic developer and method for producing the same, carrier for the electrophotographic developer, and the electrophotographic developer
JP2011075918A
Iron oxide powder for brake friction material