Block manufacturing method
A two-step heat treatment process using sodium dihydrogen phosphate as an inorganic binder effectively addresses the issue of thermal decomposition gases in mold manufacturing, ensuring strong and gas-free blocks suitable for casting.
Patent Information
- Application Number
- JP2023045648
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing molds with complicated shapes using organic binders like alkali phenolic resins generate thermal decomposition gases, leading to casting defects and environmental deterioration, while reducing the binder amount compromises mold strength.
A two-step heat treatment process using a mixture of refractory granular material, sodium dihydrogen phosphate, and water, where the mixture is first heated to 100-250°C to form a primary block, and then heated to 400°C or higher to polymerize sodium dihydrogen phosphate, forming a network that binds the materials without generating significant thermal decomposition gases.
The method produces blocks with practical strength and minimal gas generation, maintaining structural integrity and reducing environmental impact during high-temperature casting processes.
Smart Images

Figure 2024135117000004 
Figure 2024135117000001 
Figure 2024135117000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a block. [Background technology]
[0002] A self-hardening mold has been known as one type of casting mold (hereinafter simply referred to as "mold"). A self-hardening mold is manufactured by adding a binder and a hardener to a refractory granular material such as silica sand, kneading the mixture, and then filling a wooden, resin, or metal mold (hereinafter collectively referred to as "molding mold") with the resulting mixed sand and allowing the binder to harden. However, the above method requires a mold of the same shape as the casting mold, and it takes time to make the mold when manufacturing a mold of a complex shape. In addition, although a mold of a complex shape may be manufactured by increasing the number of molds, increasing the number of molds causes the process to become complicated. In addition, even if a mold of a complex shape can be manufactured or the number of molds can be increased, if the casting mold cannot be removed from the mold, the mold cannot be manufactured.
[0003] In view of this, a method has been proposed in which the mixed sand is solidified into a simple shape, for example a block such as a rectangular parallelepiped, by hardening the binder, and then the sand is cut into the desired shape to produce a mold. For example, Patent Document 1 discloses a method for producing a mold by solidifying mixed sand into a block using a mixture of a carbon dioxide-curing alkaline phenolic resin and an epoxy compound as a binder, and then cutting the resulting block. Patent Document 2 discloses a method for producing a mold by solidifying mixed sand into a block using a binder consisting of an ester-hardening alkaline phenolic resin and its hardener, and then cutting the resulting block. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 3923749 [Patent Document 2] Patent No. 6489394 Summary of the Invention [Problem to be solved by the invention]
[0005] However, as described in Patent Documents 1 and 2, when a casting is produced by pouring a liquid obtained by melting a metal such as iron, copper, or aluminum at a high temperature into a mold obtained by using an organic binder such as an alkaline phenol resin, the organic binder is likely to thermally decompose and generate gas (pyrolysis gas), which can cause defects in the casting or deteriorate the working environment. The higher the pouring temperature, the more likely the organic binder is to thermally decompose and generate gas. Reducing the amount of organic binder used can reduce the amount of gas generated during pouring, but it also reduces the strength of the mold.
[0006] An object of the present invention is to provide a method for producing blocks which is less likely to generate gases caused by thermal decomposition of a binder and which is capable of producing blocks having practical strength. [Means for solving the problem]
[0007] The present invention has the following aspects. [1] A first heat treatment step of filling a mixture containing a refractory granular material, sodium dihydrogen phosphate, and water into a mold and heat treating it at 100 to 250 ° C to obtain a primary block; A second heat treatment step of heat treating the primary block to 400° C. or higher; A method for producing a block comprising the steps of: Effect of the Invention
[0008] According to the present invention, there can be provided a method for producing blocks which is less likely to generate gases caused by thermal decomposition of the binder and which is capable of producing blocks having a practical strength. [Brief description of the drawings]
[0009] [Figure 1] 1 is a graph showing the results of the amount of gas generated in Examples 9 to 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Block manufacturing method] Hereinafter, one embodiment of the method for producing a block of the present invention will be described. The method for manufacturing a block of this embodiment includes a first heat treatment step in which a mixture containing a refractory granular material, sodium dihydrogen phosphate, and water is filled into a mold and heat-treated at 100 to 250°C to obtain a primary block, and a second heat treatment step in which the primary block is heat-treated at 400°C or higher.
[0011] <Mixture> The mixture includes a refractory granular material, sodium dihydrogen phosphate, and water. The mixture may contain components other than the refractory granular material, sodium dihydrogen phosphate, and water (hereinafter also referred to as "optional components") as long as the effects of the present invention are not impaired.
[0012] (Fire-resistant granular material) Refractory granular materials include sand, ceramic, metal, and the like. These refractory granular materials may be used alone or in combination of two or more.
[0013] Examples of sand include natural sand such as silica sand, chromite sand, zircon sand, olivine sand, amorphous silica, alumina sand, and mullite sand; and artificial sand. In addition, used artificial sand or natural sand that has been recovered (recovered sand), or sand that has been regenerated (by roasting, dry regeneration such as grinding, etc.) can also be used. These sands may be used alone or in combination of two or more types. Artificial sand is generally obtained by using bauxite as a raw material, either by a melting method (atomization method), a sintering method, or a flame fusion method. The specific conditions for the melting method, the sintering method, or the flame fusion method are not particularly limited, and artificial sand may be produced using known conditions described in, for example, JP-A-5-169184, JP-A-2003-251434, JP-A-2004-202577, etc. Examples of the metal include nickel, cobalt, molybdenum, iron, stainless steel, aluminum, titanium, copper, etc. These metals may be used alone or in combination of two or more.
[0014] The average particle size of the refractory granular material is preferably 10 to 600 μm, more preferably 50 to 600 μm, even more preferably 65 to 550 μm, and particularly preferably 75 to 500 μm. If the average particle size of the refractory granular material is equal to or greater than the above lower limit, a block with high strength can be obtained. If the average particle size of the refractory granular material is equal to or less than the above upper limit, when the block obtained by the present invention is used as a mold as it is, or when the block is machined and used as a mold, the surface of the casting cast using this mold is excellent. The average particle size of the refractory granular material is the particle size (median size) corresponding to a cumulative frequency of 50% based on the volume distribution of the refractory granular material measured by dynamic light scattering.
[0015] The refractory granular material is selected depending on the intended use of the resulting block. For example, when the block is used as a mold as it is, or when the block is cut and used as a mold, sand is suitable as the refractory granular material. Since natural sand is cheaper than artificial sand, it is preferable to use natural sand alone or in combination with artificial sand from the viewpoint of reducing the manufacturing cost, and it is preferable to use a mixture of natural sand and artificial sand if the fire resistance of the mold is also taken into consideration. A casting mold is a model for casting metal, and is dismantled to remove the casting after casting. In other words, if the casting is the final object (final product), then the casting mold is meant to be destroyed in the end. On the other hand, if the block is the final object (not intended to be ultimately destroyed), metal is a suitable refractory granular material. In this specification, a block obtained using sand is also referred to as a "sand block", and a block obtained using metal is also referred to as a "metal block".
[0016] (Sodium dihydrogen phosphate) Sodium dihydrogen phosphate is an inorganic binder. Sodium dihydrogen phosphate is polymerized by thermal dehydration condensation to generate condensed sodium phosphate or sodium polyphosphate. A network of inorganic substances such as condensed sodium phosphate or sodium polyphosphate generated by polymerization of sodium dihydrogen phosphate in the second heat treatment step described later is efficiently formed. As a result, the refractory granular materials are sufficiently bonded together. The sodium dihydrogen phosphate may be in the form of a hydrate or anhydrous form.
[0017] (Method of producing the mixture) The mixture is obtained by kneading the refractory granular material, sodium dihydrogen phosphate, water, and optional ingredients, if necessary. When the refractory granular material is sand, the mixture is also referred to as "sand mix."
[0018] The content of sodium dihydrogen phosphate in the mixture is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 3 parts by mass, and even more preferably 1 to 2 parts by mass, based on 100 parts by mass of the refractory granular material. If the content of sodium dihydrogen phosphate is equal to or greater than the above lower limit, a block having practical strength is easily obtained. If the content of sodium dihydrogen phosphate is equal to or less than the above upper limit, a block having practical disintegrability is easily obtained. The content of water in the mixture is preferably 0.15 to 7.5 parts by mass, more preferably 0.75 to 4.5 parts by mass, and even more preferably 1.5 to 3 parts by mass, based on 100 parts by mass of the refractory granular material. If the content of water is equal to or more than the lower limit, sodium dihydrogen phosphate is sufficiently dissolved and impregnated into the refractory granular material. Therefore, in the first heat treatment step described below, water evaporates and sodium dihydrogen phosphate solidifies, so that the refractory granular material is appropriately bonded to each other. If the content of water is equal to or less than the upper limit, a delay in the treatment time in the first heat treatment step can be prevented.
[0019] Sodium dihydrogen phosphate may be dissolved in water and used in the form of an aqueous solution (hereinafter also referred to as "aqueous sodium dihydrogen phosphate solution"). That is, a mixture may be prepared by kneading a refractory granular material, an aqueous sodium dihydrogen phosphate solution, and optional components as necessary. The content of sodium dihydrogen phosphate relative to the total mass of the aqueous sodium dihydrogen phosphate solution is preferably from 10 to 70 mass %, more preferably from 30 to 60 mass %.
[0020] The refractory granular material may be used in a state in which its surface is coated with sodium dihydrogen phosphate. That is, a mixture may be prepared by kneading a coating material in which the refractory granular material is coated with sodium dihydrogen phosphate, water, and optional components as necessary. The refractory granular material may be coated with the optional components exemplified above, in addition to sodium dihydrogen phosphate, as necessary, within the range that does not impair the effects of the present invention. The proportion of sodium dihydrogen phosphate in the coating material is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 3 parts by mass, and even more preferably 1 to 2 parts by mass, per 100 parts by mass of the refractory granular material.
[0021] The coating material can be obtained, for example, by adding a solution containing sodium dihydrogen phosphate and, if necessary, optional components (hereinafter, also referred to as "solution (α)") to a heated refractory granular material. The sodium dihydrogen phosphate and the optional components may be added separately to the refractory granular material. In this case, a solution containing sodium dihydrogen phosphate (hereinafter also referred to as "solution (α1)") and a solution containing the optional components (hereinafter also referred to as "solution (α2)") are added to the heated refractory granular material to obtain a coating material. The order of adding the solutions (α1) and (α2) is not particularly limited, and the solution (α1) may be added to the refractory granular material and then the solution (α2) may be added, or the solution (α2) may be added to the refractory granular material and then the solution (α1) may be added, or the solutions (α1) and (α2) may be added simultaneously.
[0022] Solvents used for solution (α), solution (α1), and solution (α2) include water, alcohol, and mixtures thereof. Examples of alcohol include methanol, ethanol, 1-propanol, and 2-propanol. Among these, water is preferred as the solvent. The total amount of sodium dihydrogen phosphate relative to the total mass of solution (α) and solution (α1) is preferably 10 to 55 mass %, more preferably 30 to 40 mass %.
[0023] The heating temperature of the refractory granular material is preferably not higher than 250° C., more preferably not higher than 200° C., and even more preferably not higher than 150° C. If the temperature of the refractory granular material is not higher than the above upper limit, the thermal decomposition of sodium dihydrogen phosphate can be suppressed. In particular, when obtaining a dry coating material, the heating temperature of the refractory granular material is preferably equal to or higher than the boiling point of the solvent contained in the solution (α), solution (α1), and solution (α2), more preferably 100 to 250°C, even more preferably 100 to 200°C, and particularly preferably 100 to 150°C. However, when the solvent contained in the solution (α), solution (α1), and solution (α2) is alcohol, it has a lower boiling point than water and is easily evaporated even below the boiling point of the alcohol. Therefore, the heating temperature of the refractory granular material is not limited to the above range, and when the solvent contained in the solution (α), solution (α1), and solution (α2) is alcohol, a dry coating material may be obtained even if the heating temperature of the refractory granular material is higher than 60°C and lower than 100°C. On the other hand, when obtaining a wet coating material, the heating temperature of the refractory granular material is preferably lower than the boiling point of the solvent contained in solution (α), solution (α1), and solution (α2), more preferably 60°C or lower, even more preferably 10 to 50°C, and particularly preferably 20 to 30°C. The coating material may be in a dry or wet state.
[0024] When preparing a mixture using a wet coating material, it is preferable to use water as the solvent for the solutions (α), (α1), and (α2). It is preferable to adjust the amount of water added so that the total amount of the solvent contained in the coating material and the water added to the coating material is 0.15 to 7.5 parts by mass, more preferably 0.75 to 4.5 parts by mass, and even more preferably 1.5 to 3 parts by mass, relative to 100 parts by mass of the refractory granular material.
[0025] <First heat treatment step> The first heat treatment step is a step in which the mixture is filled into a mold and heated to 100 to 250° C. to obtain a primary block. The mixture is heated to 100-250℃, causing the water to evaporate. Also, the sodium dihydrogen phosphate dissolved in the water in the mixture solidifies as the water evaporates, bonding the refractory granular materials together appropriately. By "adequately bonded" is meant that the refractory granular material is bonded to one another to such an extent that the primary block can be removed from the mold without the primary block disintegrating.
[0026] The molding mold is not particularly limited, and examples thereof include a wooden mold (wooden mold), a resin mold (resin mold), a metal mold (metal mold), etc., which may be appropriately selected depending on the heating temperature in the first heat treatment step.
[0027] The heating temperature of the mixture is 100 to 250° C., more preferably 120 to 230° C., further preferably 130 to 220° C., and particularly preferably 150 to 200° C. If the heating temperature of the mixture is equal to or higher than the lower limit, water is likely to evaporate and sodium dihydrogen phosphate is likely to solidify. If the heating temperature of the mixture is equal to or lower than the upper limit, deformation of the casting mold due to heating can be suppressed. The heating time for the mixture is not particularly limited as long as it is a time that allows water to evaporate sufficiently, and may be appropriately determined depending on the shape and size of the mixture. The mixture may be heated using a heating device such as an electric furnace or an oven.
[0028] The primary block obtained in the first heat treatment step may be demolded from the mold and subjected to the second heat treatment step, or, if the mold can withstand the heating temperature in the second heat treatment step, the primary block may be subjected to the second heat treatment step as it is without being demolded. From the viewpoint of the handleability of the primary block, it is preferable to subject the primary block to the second heat treatment step after removing it from the mold and cooling it to preferably about 25 to 80°C, more preferably about 40 to 80°C. If the cooling temperature is equal to or higher than the lower limit, the primary block can be prevented from absorbing moisture, and good handling strength can be maintained. If the cooling temperature is equal to or lower than the upper limit, the handleability of the primary block is improved. As the cooling method, a known method can be used, for example, a method of allowing the material to cool naturally, a method of forced cooling using air blowing, etc. can be mentioned. On the other hand, from the viewpoint of energy efficiency and work efficiency, it is preferable to subject the primary block to the second heat treatment step while maintaining the temperature, without removing the primary block from the mold.
[0029] <Second heat treatment process> The second heat treatment step is a step of heat treating the primary block at 400° C. or higher. By heating the primary block to 400°C or higher, sodium dihydrogen phosphate polymerizes through a dehydration condensation reaction, forming a network of inorganic substances such as condensed sodium phosphate and sodium polyphosphate, which sufficiently bonds the refractory granular materials together.
[0030] The heating temperature of the primary block is 400°C or higher, preferably 400 to 1000°C, more preferably 500 to 800°C, and even more preferably 550 to 750°C. If the heating temperature of the primary block is equal to or higher than the lower limit, the dehydration condensation reaction of sodium dihydrogen phosphate proceeds sufficiently. This dehydration condensation reaction tends to proceed more as the heating temperature of the primary block increases, but if the heating temperature is too high, the effect will simply plateau. In addition, the higher the heating temperature, the more energy is consumed, resulting in higher costs. In addition, when the obtained block is used as a mold as it is, or when the block is cut and used as a mold, the collapsibility tends to decrease. In consideration of these points, the heating temperature of the primary block is preferably 1000°C or lower. Since the thermal decomposition and dehydration condensation reaction proceed at 400°C or higher, in the present invention, it is not necessary to heat the primary block at a higher temperature than necessary, and from the viewpoint of more effectively reducing energy consumption while further increasing collapsibility, 800°C or lower is preferable. In particular, from the viewpoint of easily obtaining a block with high strength, 750° C. or less is more preferable. The heating time for the primary block is not particularly limited as long as the above-mentioned dehydration condensation reaction proceeds sufficiently, and may be appropriately determined depending on the shape and size of the primary block. The primary block may be heated using a heating device such as an electric furnace or an oven.
[0031] The primary block is heat-treated at 400° C. or higher and then cooled to room temperature (for example, 25° C.) (cooling step) to obtain a block. As the cooling method, a known method can be used, for example, a method of allowing the material to cool naturally at room temperature, a method of forced cooling using a blower, etc.
[0032] The block thus obtained is a heat-treated version of the primary block, and can therefore also be called a "secondary block." When the refractory granular material is sand, a sand block is obtained.
[0033] <Action and effect> In the block manufacturing method of the present embodiment described above, sodium dihydrogen phosphate, an inorganic binder, is used as the binder, and two-stage heat treatment is performed at specific temperatures, so that sodium dihydrogen phosphate polymerizes to form a network of inorganic substances such as condensed sodium phosphate and sodium polyphosphate. As a result, the refractory granular materials are sufficiently bonded together to obtain a block with practical strength. In addition, the block obtained in this manner is less likely to absorb moisture, so that it can maintain its strength well even in a humid environment. Moreover, the method for producing a block of the present embodiment does not require the use of an organic binder. Therefore, for example, when the obtained block is used as a mold as is, or the block is machined and used as a mold, no thermal decomposition gas is generated from the organic binder, the working environment during pouring is unlikely to deteriorate, and the occurrence of casting defects can be suppressed. As described above, according to the present invention, the thermal decomposition gas of the binder is hardly generated, and blocks having a practical strength can be manufactured.
[0034] As an inorganic binder, for example, water glass is known. Even if water glass is used instead of sodium dihydrogen phosphate, a block with practical strength can be obtained. However, when a block obtained using water glass is used as a mold as it is, or when the block is cut and used as a mold, the heat-resistant temperature of the mold is about 800°C. Therefore, when molten metal with a temperature exceeding the heat-resistant temperature of the mold is poured, the water glass softens, the mold becomes easily deformed, and the dimensional accuracy of the casting at high temperatures decreases, so that the metal used for casting is limited. On the other hand, molds made using sodium dihydrogen phosphate have better heat resistance than molds made using water glass. Therefore, the molds are less likely to deform even when molten metal exceeding 800°C is poured into them, and the dimensional accuracy of the castings is high even at high temperatures, so there are fewer restrictions on the metals that can be used for casting.
[0035] The block obtained by the present invention is suitable as a mold block. When the refractory granular material is sand, the obtained block may be used as a mold as it is, or the mold may be manufactured by cutting the block. For example, if a mold of a relatively simple shape is to be produced, a block may be produced using a molding die having the same shape as the mold, and the obtained block may be used as the mold as is. In this case, one aspect of the method for producing a block according to the present embodiment may also be considered as a method for producing a mold.
[0036] On the other hand, when producing a mold of a complex shape, a block can be produced using a molding die of a simple shape, and the resulting block can then be machined to produce a mold of the complex shape; it is not necessarily necessary to use a molding die of the same shape as the desired object, such as the mold. In this case, the method for manufacturing a mold includes a block molding step of manufacturing a block by the block manufacturing method of this embodiment described above, and a cutting step of cutting the obtained block into a desired shape.
[0037] When cutting a block, for example, an NC machine is used to cut the block into a desired shape. Specifically, first, shape data of an object such as a mold is created using 3D CAD (computer aided design). Next, the block is cut using an NC machine based on the 3D CAD shape data to manufacture the object. EXAMPLES
[0038] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The materials used in each example are shown below. Various measurement methods are also shown below.
[0039] [Measurement and evaluation method] <Measurement of bending strength> The bending strength of the primary blocks and blocks obtained in each of the Examples and Comparative Examples was measured using the measurement method described in JACT Test Method SM-1.
[0040] <Gas generation rate measurement> The block was heat-treated in an atmosphere of 1000°C for 5 minutes, exposing the mold to the same atmosphere as when the casting was made. The amount of gas generated during the heat treatment was measured according to JACT test method M-5 "Gas generation amount measurement method".
[0041] [Example 1] As the refractory granular material, artificial sand obtained by a fusion method (manufactured by Ito Kiko Co., Ltd., "Alsand #750", average particle size 212 μm) was used. As the solution (α-1), an aqueous solution in which 40 parts by mass of sodium dihydrogen phosphate was dissolved in 60 parts by mass of water was used.
[0042] <Preparation of mixed sand> 100 parts by mass of the refractory granular material and 2.5 parts by mass of the solution (α-1) (1 part by mass in terms of pure sodium dihydrogen phosphate) were put into a Shinagawa universal mixer (MIXER, manufactured by Shinagawa Kogyosho Co., Ltd.) and mixed to obtain mixed sand. The composition of the mixed sand is shown in Table 1.
[0043] <Block creation> Seven resin molding dies were prepared, each having five rectangular parallelepiped patterns measuring 10 mm in length, 60 mm in width, and 10 mm in height. The resulting mixed sand was immediately filled into each prepared mold under conditions of a temperature of 25° C. and a humidity of 50%, and heat-treated at 150° C. for 1 hour to obtain a primary block (first heat treatment step). The primary blocks were removed from the mold and cooled to room temperature (25°C), after which the bending strengths of the five primary blocks were measured and the average value was calculated. The results are shown in Table 1. The remaining 30 primary blocks were divided into groups of 5 and heated at 350°C, 400°C, 500°C, 600°C, 700°C or 800°C for 1 hour to obtain blocks (second heat treatment step). After cooling to room temperature (25°C), the bending strength of five blocks from each group was measured and the average value was calculated. The results are shown in Table 1.
[0044] [Example 2] Except for changing the amount of solution (α-1) to 5 parts by mass (2 parts by mass calculated as the pure content of sodium dihydrogen phosphate), primary blocks and blocks were prepared in the same manner as in Example 1, and their bending strengths were measured. The results are shown in Table 1.
[0045] [Example 3] A primary block was prepared in the same manner as in Example 1. The bending strength of the five primary blocks immediately after cooling was measured and the average value was calculated. The results are shown in Table 2. The remaining primary blocks were divided into groups of 5 and left for 5 or 10 minutes under conditions of 25°C and 50% humidity. After leaving, the bending strength of the 5 primary blocks in each group was measured and the average value was calculated. The results are shown in Table 2.
[0046] [Example 4] A primary block and a block were prepared in the same manner as in Example 1. However, the heating temperature of the primary block in the second heat treatment step was set to 350°C. The bending strength of the five blocks immediately after cooling was measured and the average value was calculated. The results are shown in Table 2. The remaining blocks were divided into groups of 5 and left for 5 or 10 minutes at a temperature of 25°C and a humidity of 50%. After leaving the blocks, the bending strength of the 5 blocks in each group was measured and the average value was calculated. The results are shown in Table 2.
[0047] [Example 5] A primary block and a block were prepared in the same manner as in Example 1. However, the heating temperature of the primary block in the second heat treatment step was set to 400°C. The bending strength of the five blocks immediately after cooling was measured and the average value was calculated. The results are shown in Table 2. The remaining blocks were divided into groups of 5 and left for 5 or 10 minutes at a temperature of 25°C and a humidity of 50%. After leaving the blocks, the bending strength of the 5 blocks in each group was measured and the average value was calculated. The results are shown in Table 2.
[0048] [Example 6] A primary block was prepared in the same manner as in Example 1, except that the amount of solution (α-1) was changed to 5 parts by mass (2 parts by mass calculated as the pure content of sodium dihydrogen phosphate). The bending strength of the five primary blocks immediately after cooling was measured and the average value was calculated. The results are shown in Table 3. The remaining primary blocks were divided into groups of 5 and left for 5, 10, 15, 20 or 25 minutes under conditions of 25°C temperature and 50% humidity. After leaving, the bending strength of the 5 primary blocks in each group was measured and the average value was calculated. The results are shown in Table 3.
[0049] [Example 7] Except for changing the blending amount of solution (α-1) to 5 parts by mass (2 parts by mass calculated as the pure content of sodium dihydrogen phosphate), the primary block and the block were prepared in the same manner as in Example 1. However, the heating temperature of the primary block in the second heat treatment step was 350°C. The bending strength of the five blocks immediately after cooling was measured and the average value was calculated. The results are shown in Table 3. The remaining blocks were divided into groups of 5 and left at 25°C and 50% humidity for 5, 10, 15, 20 or 25 minutes. After leaving the blocks, the bending strength of the 5 blocks in each group was measured and the average value was calculated. The results are shown in Table 3.
[0050] [Example 8] Except for changing the blending amount of solution (α-1) to 5 parts by mass (2 parts by mass calculated as the pure content of sodium dihydrogen phosphate), the primary block and the block were prepared in the same manner as in Example 1. However, the heating temperature of the primary block in the second heat treatment step was 400°C. The bending strength of the five blocks immediately after cooling was measured and the average value was calculated. The results are shown in Table 3. The remaining blocks were divided into groups of 5 and left at 25°C and 50% humidity for 5, 10, 15, 20 or 25 minutes. After leaving the blocks, the bending strength of the 5 blocks in each group was measured and the average value was calculated. The results are shown in Table 3.
[0051] [Table 1]
[0052] [Table 2]
[0053] [Table 3]
[0054] As is clear from Table 1, by heat treating the primary block at 400° C. or higher in the second heat treatment step, a block with practical strength could be produced. Furthermore, as is clear from Tables 2 and 3, the primary blocks obtained in Examples 3 and 6, and the blocks in Examples 4 and 7 obtained by heat-treating the primary blocks at 350°C in the second heat treatment step were prone to a decrease in bending strength due to moisture absorption when left under conditions of a temperature of 25°C and a humidity of 50%. In contrast, the blocks in Examples 5 and 8 obtained by heat-treating the primary blocks at 400°C in the second heat treatment step were less susceptible to moisture absorption and were able to maintain good bending strength when left under conditions of a temperature of 25°C and a humidity of 50% compared to Examples 3, 4, 6, and 7.
[0055] [Example 9] Except for changing the blending amount of solution (α-1) to 5 parts by mass (2 parts by mass calculated as the pure content of sodium dihydrogen phosphate), a primary block and a block were prepared in the same manner as in Example 1. However, the heating temperature of the primary block in the second heat treatment step was set to 600°C. The amount of gas generated was measured using the obtained block, and the results are shown in Figure 1.
[0056] [Example 10] As the organic binder, a furan resin (Gun-ei Chemical Industry Co., Ltd., N-furan resin "GFA-160", pure content 90 mass %) was used. As the curing agent, a mixture of 60 parts by mass of an aqueous sulfonic acid solution (manufactured by Gun-ei Chemical Industry Co., Ltd., N-Furan curing agent "GH-20") and 40 parts by mass of an aqueous sulfonic acid solution (manufactured by Gun-ei Chemical Industry Co., Ltd., N-Furan curing agent "GH-70") was used.
[0057] <Preparation of mixed sand> 100 parts by mass of fire-resistant granular material, 0.8 parts by mass of furan resin (0.72 parts by mass in terms of pure furan resin content), and 0.3 parts by mass of hardener were put into a Shinagawa universal mixer (MIXER, manufactured by Shinagawa Kogyosho Co., Ltd.) and mixed to obtain mixed sand.
[0058] <Block creation> The obtained mixed sand was immediately filled into a mold similar to that in Example 1 under conditions of a temperature of 25° C. and a humidity of 50% and cured, and the cured product was removed one hour after the start of curing (mold removal time: 1 hour). The resulting cured product was allowed to stand for 24 hours from the start of curing under conditions of a temperature of 25° C. and a humidity of 50%, to obtain a block. The amount of gas generated was measured using the obtained block, and the results are shown in Figure 1.
[0059] [Example 11] As the organic binder, a resol type phenolic resin, which is an alkaline phenolic resin (manufactured by Gun-ei Chemical Industry Co., Ltd., Alpha System resin "AR-170", purity 45% by mass, moisture content 55% by mass) was used. As the hardener, an organic ester (Alpha System Hardener "AH-530", a mixture of triacetin and ethylene glycol diacetate, manufactured by Gun-ei Chemical Industry Co., Ltd.) was used.
[0060] <Block preparation> 100 parts by mass of fire-resistant granular material, 1 part by mass of alkaline phenolic resin (0.45 parts by mass in terms of the pure content of alkaline phenolic resin), and 0.2 parts by mass of hardener were put into a Shinagawa universal mixer (MIXER, manufactured by Shinagawa Kogyosho Co., Ltd.) and mixed to obtain mixed sand.
[0061] <Block creation> The obtained mixed sand was immediately filled into a mold similar to that in Example 1 under conditions of a temperature of 25° C. and a humidity of 50% and cured, and the cured product was removed one hour after the start of curing (mold removal time: 1 hour). The resulting cured product was allowed to stand for 24 hours from the start of curing under conditions of a temperature of 25° C. and a humidity of 50%, to obtain a block. The amount of gas generated was measured using the obtained block, and the results are shown in Figure 1.
[0062] As is clear from FIG. 1, the block obtained in Example 9, which used sodium dihydrogen phosphate as an inorganic binder, did not generate gas. In contrast, the blocks obtained in Examples 10 and 11, which used an organic binder, were prone to gas generation. These results demonstrate that the present invention makes it possible to produce blocks with practical strength without generating gases caused by thermal decomposition of the binder.
Claims
[Claim 1] a first heat treatment step of filling a mold with a mixture containing a refractory granular material, sodium dihydrogen phosphate, and water, and heat treating the mixture at 100-250° C. to obtain a primary block; A second heat treatment step of heat treating the primary block to 400° C. or higher; A method for producing a block comprising the steps of:
Citation Information
Patent Citations
Multifunctional tuner
JP1989089394A