Manufacturing method for steel product
A controlled hot processing and direct quenching method for hot die steel using a specific alloy composition addresses cracking and toughness issues, resulting in refined grains and enhanced mechanical properties.
Patent Information
- Application Number
- JP2023046519
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing hot die steel manufacturing methods, such as direct quenching, face issues with cracking during quenching and reduced toughness in the final product due to complex heat treatment processes.
A manufacturing method involving a specific composition of C, Si, Mn, Cr, Ni, Mo, and V, followed by hot processing at controlled temperatures and direct quenching to suppress cracking and maintain toughness, including steps like high-temperature soaking and controlled cooling.
The method effectively prevents cracking during quenching and maintains high toughness in the final product, achieving refined grain structures and improved mechanical properties.
Smart Images

Figure 2024135704000001 
Figure 2024135704000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a steel material. [Background technology]
[0002] SKT4 and its equivalents, as specified in JIS G4404, are hot die steels having high toughness and good wear resistance, and are used in applications such as forging dies. As a hot processing method for hot die steels such as SKT4, a method is known in which a steel ingot is hot forged, and then the forged material is reheated and subjected to a refining treatment such as quenching and tempering to obtain desired mechanical properties. For example, Patent Document 1 discloses a method for manufacturing a hot tool, which includes a process of heating an ingot to 1200 to 1280°C and hot forging it.
[0003] On the other hand, since the above-mentioned manufacturing method requires many heat treatment steps and is costly, a direct quenching process is also known as a manufacturing method for simplifying the heat treatment steps and reducing the heat treatment cost, in which quenching is performed without reheating from the temperature after hot forging. For example, Patent Document 2 discloses a method in which SMn443 rolled material is heated to 1050°C and then directly quenched. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5744300 [Patent Document 2] Japanese Patent Application Publication No. 60-77915 Summary of the Invention [Problem to be solved by the invention]
[0005] As described in Patent Document 1, direct quenching is an effective technique for reducing heat treatment costs, but there are concerns about the occurrence of cracks during quenching and cooling. In addition, there are cases where the toughness of products after quenching and tempering is low. Therefore, an object of the present invention is to provide a method for producing a steel material that can suppress cracks during quenching and a decrease in toughness in a product after quenching and tempering even when direct quenching is performed. [Means for solving the problem]
[0006] The present invention has been made in consideration of the above-mentioned problems. That is, the present invention provides: This method for producing a steel material includes a preparation step of preparing a material for hot working consisting, by mass%, of 0.0.50-0.60% C, 0.10-0.40% Si, 0.60-1.00% Mn, 0.80-1.40% Cr, 1.30-2.00% Ni, 0.20-0.55% Mo, 0.05-0.20% V, and the balance being Fe and unavoidable impurities; a first hot working step of hot working the material for hot working at a hot working start temperature of 1170-1300°C to obtain an intermediate hot worked material; a second hot working step of hot working the intermediate hot worked material at a hot working start temperature of 1000-1150°C to obtain a hot worked material; and a direct quenching step of directly quenching the hot worked material to obtain a steel material. Preferably, the steel material after the direct quenching step is tempered. Effect of the Invention
[0007] According to the present invention, even if direct quenching is performed, cracks during quenching and a decrease in toughness of the product after quenching and tempering can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described. <Preparation process> First, in this embodiment, a hot working material having a composition equivalent to SKT4 and an improved material as specified in JIS G4404 is prepared (preparation process). Specifically, a hot working material having a composition consisting of, in mass%, C: 0.0.50-0.60%, Si: 0.10-0.40%, Mn: 0.60-1.00%, Cr: 0.80-1.40%, Ni: 1.30-2.00%, Mo: 0.20-0.55%, V: 0.05-0.20%, and the balance: Fe and unavoidable impurities is prepared. The reasons for limiting the components of the present invention are described below (hereinafter, mass% will be simply referred to as %).
[0009] C: 0.50-0.60% C is an important essential element for hot work tool steel, as some of it dissolves in the matrix to impart strength, and some of it forms carbides to increase wear resistance and seizure resistance. However, excessive addition of C can reduce toughness and hot strength, so the C content is set to 0.50-0.60%.
[0010] Silicon: 0.10 to 0.40% Silicon is a deoxidizing agent during steelmaking and also an element that improves the machinability of the material. However, since too much silicon leads to the formation of ferrite, the content is set to 0.10 to 0.40% in the present invention.
[0011] Mn: 0.60-1.00% Mn has the effect of improving hardenability, suppressing the formation of ferrite, and obtaining appropriate hardness after quenching and tempering. In addition, its presence as nonmetallic inclusion MnS has a significant effect on improving machinability, but if it is too much, it increases the viscosity of the matrix and reduces machinability, so the content is set to 0.60-1.00%.
[0012] Cr: 0.80~1.40% Cr is an element that enhances hardenability and forms carbides, and is effective in strengthening the matrix and improving wear resistance. It also contributes to improving temper softening resistance and high-temperature strength, and is an essential element for the hot work tool steel of the present invention. However, excessive addition of Cr reduces hardenability and high-strength properties, so the content is set to 0.80 to 1.40%.
[0013] Ni: 1.30~2.00% Ni is an element that suppresses the formation of ferrite. In addition, together with C, Cr, Mn, Mo, etc., Ni gives the steel of the present invention excellent hardenability, and is an effective element for forming a martensite-based structure and preventing a decrease in toughness even when the cooling rate during quenching is slow. In addition, Ni also has the effect of improving the essential toughness of the matrix. However, if it is too much, the viscosity of the matrix increases and the machinability decreases, so it is set to 1.30 to 2.00%.
[0014] Mo+1 / 2W: 0.20~0.55% Mo and W can be added alone or in combination to impart strength and improve softening resistance by precipitating or agglomerating fine carbides during tempering. The amount of W added can be determined together as the Mo equivalent of (Mo+1 / 2W) since the atomic weight of W is about twice that of Mo (obviously, only one of them can be added, or both can be added together). However, if the amount is too high, it will cause a decrease in machinability and toughness, so the value of (Mo+1 / 2W) is set to 0.20 to 0.55%.
[0015] V: 0.05~0.20% V forms carbides and has the effect of strengthening the matrix and improving wear resistance. It also increases temper softening resistance, inhibits grain coarsening, and contributes to improving toughness. However, if it is too much, it will cause a decrease in machinability and toughness, so the content should be 0.05 to 0.20%. The balance is Fe and unavoidable impurities.
[0016] In this embodiment, a material for hot working having the above-mentioned composition is prepared. This material for hot working can be a steel ingot or a cast piece obtained by a melting process. Since the steel ingot obtained in the melting process has a bias in the components, a process of performing a high-temperature soaking treatment called a segregation diffusion treatment may be included.
[0017] <First hot processing process> The hot working material is heated to a hot working start temperature of 1170 to 1300 ° C, and then hot working is performed at this hot working start temperature to obtain an intermediate hot working material (first hot working process). Examples of the hot working include forging and rolling at the above-mentioned temperatures. In the first hot working process, the steel ingot obtained in the casting process is rolled down to destroy internal defects and cast structure in this process, and the first hot working is performed at a working start temperature of 1170 to 1300 ° C to promote the bonding of defects and the refinement of austenite grains by dynamic recrystallization. Here, the "first hot working" in the present invention may be forging such as hot free forging and hot die forging, or may be hot rolling. In this first hot working process, if the amount of roll down to the intermediate hot working material is insufficient, the amount of roll down can be increased by performing an upset forging process. In the first hot working process, the hot working material may be heated many times. This first hot working step can be applied to a general "blooming step."
[0018] <Second hot processing process> Next, the intermediate hot-worked material after the first hot working step is hot-worked at a hot working start temperature of 1000 to 1150 ° C to obtain a hot-worked material (second hot working step). This is to perform hot working in a predetermined temperature range on the structure obtained in the first hot working step to refine the structure. By refining the structure in the second hot working step, it is expected that the toughness of the die can be improved. The upper limit of the preferred second hot working start temperature is 1100 ° C. If the second hot working start temperature is higher than 1150 ° C (for example, higher than the first hot working start temperature) and direct quenching is performed as described below, coarse crystal grains and a mixed grain structure are generated due to the progress of secondary recrystallization, which may be a factor in reducing the toughness of the steel material. On the other hand, if the start temperature of the second hot working is less than 1000 ° C, there is a tendency that refinement of crystal grains by dynamic recrystallization is less likely to occur. The temperature of the intermediate hot-worked material after the first hot working step should be controlled by the part that will eventually be processed into a product, for example, the temperature inside the intermediate hot-worked material. In actual operation, the internal temperature of the intermediate hot-worked material when the first hot working step is completed (i.e., before moving to the second hot working step) is generally maintained at the processing start temperature of the first hot working or is close to the processing start temperature of the second hot working due to reheating during hot working, etc. However, if the internal temperature of the intermediate hot-worked material after the first hot working step has dropped, it may be reheated in the temperature range of the second hot working step before carrying out the second hot working step. Alternatively, even if the temperature of the intermediate hot-worked material at the end of the first hot working step has dropped, it may be moved to the second hot working step without reheating as it is as long as it is within the processing start temperature range of the second hot working.
[0019] In the present invention, it is preferable to cool the intermediate hot-worked material after the first hot working step before the subsequent second hot working step. That is, it is a step of conditioning the intermediate hot-worked material, and for example, the surface of the material may be ground and polished before the second hot working step is performed. In the second hot working step, since hot working is performed at a lower temperature, the ductility is reduced and cracks may occur on the surface, making it impossible to manufacture the specified dimensions, so grinding and polishing of the surface of the material may be performed. Furthermore, grinding and polishing of the surface of the material may be performed after annealing after the first hot working step. In addition, it is preferable to end the hot working of the hot-worked material after the second hot working step while maintaining a material temperature of A3 point or higher, and move to the direct quenching step described later.
[0020] <Direct hardening process> In this embodiment, the hot-worked material obtained by the second hot working process is directly quenched to obtain a steel material (direct quenching process). In this embodiment, the hot-worked material obtained by the first and second hot working processes is cooled to the Ms point or Bs point or lower to obtain a quenched structure. If the temperature of the hot-worked material is too low, a ferrite structure is generated during the cooling process, and a quenched structure cannot be obtained. Therefore, the lower limit of the temperature of the hot-worked material before starting cooling is preferably the A3 point or higher. The cooling method is not particularly limited, and existing cooling methods may be applied.
[0021] In the above-mentioned direct quenching process, the temperature of the hot-worked material should be the temperature of the part that will be finally processed into the product, that is, the temperature inside the hot-worked material. However, in actual operation, the temperature of the hot-worked material is generally controlled at its surface. The internal temperature of the hot-worked material can be confirmed by performing a simulation or the like before the actual operation, and can be controlled by the surface temperature of the hot-worked material (this also applies to the internal temperature of the intermediate hot-worked material described above).
[0022] In addition, in actual operation, the internal temperature of the hot-worked material when the second hot working step is completed (i.e., before moving to the direct quenching step) is generally maintained at the start temperature of the second hot working step due to reheating during hot working, while the surface temperature of the hot-worked material is generally lower than the start temperature. In such a case, performing the direct quenching step by oil cooling is preferable in that the temperature difference that can occur inside and outside the hot-worked material can be mitigated compared to water cooling, thereby suppressing material cracking due to thermal stress, and also in that a cooling rate sufficient for martensitic transformation and bainite transformation can be maintained compared to air cooling. EXAMPLES
[0023] A steel ingot of an alloy equivalent to SKT4 (A3 point: 780°C, derived in advance by simulation using thermodynamic calculation software) shown in Table 1 was obtained. After that, the first hot working and the second hot working were performed by forging under the conditions shown in Table 2, and then direct quenching was performed from a temperature of the A3 point or higher using oil as a coolant, and the steel was tempered to the same level of hardness in the tempering process to obtain the steel materials of the present invention and the comparative example. Although not shown in Table 2, a grinding process was introduced between the first hot working process and the second hot working process to grind the surface of the intermediate hot working material when manufacturing the steel materials of the present invention and the comparative example. In addition, each steel material was manufactured with the same forging ratio, and the forging ratio was 6 in total for the first hot working process and the second hot working process. The temperature of the first hot working process was unified at 1280°C, and the temperature of the second hot working process was variously distributed as shown in Table 2. The steel was then tempered to the same hardness level, and test pieces were taken from inside the steel to measure the Charpy impact value, hardness, and grain size number. The Charpy impact value was evaluated using a 2mm U-notch in accordance with JIS Z2242. The hardness was measured using a Rockwell hardness tester. The grain size number (GS) was determined using the grain size standard plate I in accordance with JIS-G-0551. The measurement results are shown in Table 2. As can be seen from Table 2, among the steel materials having the target hardness, the examples of the present invention all had finer crystal grains than the comparative examples, and steel materials having high Charpy impact values and excellent toughness were obtained.
[0024] [Table 1]
[0025] [Table 2]
Claims
1. a preparation step of preparing a material for hot working comprising, in mass%, 0.50-0.60% C, 0.10-0.40% Si, 0.60-1.00% Mn, 0.80-1.40% Cr, 1.30-2.00% Ni, 0.20-0.55% Mo, 0.05-0.20% V, and the balance being Fe and unavoidable impurities; A first hot working step of hot working the hot working material at a hot working start temperature of 1170 to 1300 ° C to obtain an intermediate hot worked material; A second hot working step of hot working the intermediate hot worked material at a hot working start temperature of 1000 to 1150 ° C. to obtain a hot worked material; The method for producing a steel material includes a direct quenching step of directly quenching the hot worked material to obtain a steel material.
2. The method for producing a steel material according to claim 1 , further comprising the step of tempering the steel material after the direct quenching step.
Citation Information
Patent Citations
Inspecting device of storage element
JP1982044300A
Manufacture of directly quenched steel material having superior impact characteristic
JP1985077915A