Aqueous lubricant composition

A water-based lubricant composition with a graft-modified ethylene/α-olefin copolymer and silicone oil addresses dispersibility and adhesion issues, enhancing mold release and efficiency in die casting non-ferrous metals.

JP2024136202AInactive Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023047235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing mold release agents for die casting non-ferrous metals face issues with poor dispersibility in water, adhesion of heat-degraded products to metal molds, and contamination, leading to reduced product quality and efficiency.

Method used

A water-based lubricant composition comprising a graft-modified ethylene/α-olefin copolymer, an amine compound, and a silicone oil, which is well-dispersed in water and prevents adhesion of heat-degraded substances to metals, using specific molecular weight, viscosity, and molecular weight distribution criteria.

Benefits of technology

The composition ensures excellent emulsifying properties and prevents heat-degraded substances from adhering to metal molds, reducing operations and shortening die-casting cycle time, thereby improving work efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136202000001
    Figure 2024136202000001
  • Figure 2024136202000002
    Figure 2024136202000002
  • Figure 2024136202000003
    Figure 2024136202000003
Patent Text Reader

Abstract

To provide an aqueous lubricant composition that allows a lubricating oil as a constituent to be effectively dispersed in water, and can suppress the adhesion of thermal degradation products onto metal surfaces.SOLUTION: An aqueous lubricant composition includes: a graft-modified ethylene-α-olefin copolymer (X) with a main chain derived from an ethylene-α-olefin copolymer (A) that fulfills specified requirements and a graft part derived from an unsaturated monomer (B) that fulfills specified requirements; an amine compound (Y); at least one silicone oil (Z) selected from the group consisting of alkyl-modified silicone oil and alkyl aralkyl-modified silicone oil; and water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based lubricant composition. [Background technology]

[0002] The die casting method is used for casting non-ferrous metals such as aluminum, magnesium, and zinc, in which molten metal (molten non-ferrous metal) is poured into a mold at high speed and pressure. The die casting method has the advantage of being able to produce products with complex shapes with high precision and efficiency, but it has the problem of the casting surface being damaged by seizure on the mold. For this reason, lubricants (mold release agents) are used to prevent seizure.

[0003] Conventionally, release agents for die casting have often been made from emulsified mixtures obtained by dispersing mineral oil, vegetable oil, other fats and oils, waxes, or the like as main components in water. For example, Patent Document 1 discloses an emulsified mixture using a wax mainly composed of polyethylene having an average molecular weight equal to or greater than a certain value in order to improve the adhesion efficiency of a release agent to a mold. Furthermore, Patent Document 2 discloses an emulsified mixture that uses a wax mainly made of polypropylene that contains a large amount of tertiary carbon, which is prone to decomposition reactions, in order to suppress adhesion of oxidative deterioration products generated by heat to the surface of a mold. Furthermore, Patent Document 3 discloses a water-based lubricating oil composition for non-ferrous metal plastic working that has excellent lubrication properties and processability and uses an alkylaralkyl-modified silicone oil as a main component. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 61-103642 [Patent Document 2] Japanese Patent Application Publication No. 6-240286 [Patent Document 3] JP 2003-253290 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in Patent Document 1, there was a problem that oxidation degradation products generated by heat were accumulated on the surface of the metal mold, which caused the appearance of the product to deteriorate and the dimensional accuracy to decrease. In addition, because polyethylene wax is in a solid state, it had a drawback of being poorly dispersible in water. In addition, although Patent Document 2 was able to suppress adhesion of oxidized and deteriorated products of the release agent to the surface of a metal mold, there was still room for improvement in the dispersibility of polypropylene in water. Furthermore, in Patent Document 3, by not using graphite powder or the like, it is possible to prevent the contamination of the machine or the die with the powder. However, there is room for improvement in terms of suppressing adhesion of thermally deteriorated products of the release agent to the surface of the metal die.

[0006] The present invention has been made in consideration of the above problems, and the problem that the present invention aims to solve is to provide a water-based lubricant composition in which the lubricating oil components contained therein are well dispersed in water and further in which adhesion of thermally deteriorated products to metals can be suppressed. [Means for solving the problem]

[0007] The present invention relates to, for example, the following [1] to

[10] . [1] A graft-modified ethylene / α-olefin copolymer (X) having a main chain portion derived from an ethylene / α-olefin copolymer (A) satisfying the following requirements (a-1) to (a-3) and a graft portion derived from an unsaturated monomer (B) satisfying the following requirement (b-1); an amine compound (Y); At least one silicone oil (Z) selected from the group consisting of alkyl-modified silicone oils and alkylaralkyl-modified silicone oils; Water and A water-based lubricant composition comprising: (a-1) the content of ethylene units is 30 to 70 mol %; (a-2) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (a-3) No melting point (Tm) is observed as measured by differential scanning calorimetry (DSC); (b-1) The unsaturated monomer (B) is at least one unsaturated monomer selected from the group consisting of ethylenically unsaturated monomers having a hydroxyl group.

[0008] [2] The water-based lubricant composition according to [1], wherein the ethylene-α-olefin copolymer (A) satisfies the following requirements (a-4) and (a-5): (a-4) Kinematic viscosity at 100°C is 10 to 5,000 mm 2 / s; (a-5) The molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less.

[0009] [3] The water-based lubricant composition according to [1] or [2], wherein the unsaturated monomer (B) is an unsaturated alcohol.

[0010] [4] The water-based lubricant composition according to any one of [1] to [3], wherein the graft-modified ethylene / α-olefin copolymer (X) satisfies the following requirements (x-1) to (x-5): (x-1) the proportion of the graft portion is 0.1% by mass or more and less than 70% by mass (wherein the total amount of the main chain portion and the graft portion is 100% by mass); (x-2) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (x-3) No melting point (Tm) is observed as measured by differential scanning calorimetry (DSC); (x-4) Kinematic viscosity at 100°C is 10 to 5,000 mm 2 / s; (x-5) The molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less.

[0011] [5] The water-based lubricant composition according to any one of [1] to [4], wherein the content of the graft-modified ethylene-α-olefin copolymer (X) is 0.1 to 10 mass % relative to 100 mass % of the water-based lubricant composition.

[0012] [6] The water-based lubricant composition according to any one of [1] to [5], wherein the amine compound (Y) satisfies the following requirements (y-1) and (y-2): (y-1) the molecular weight is 1,000 or less; (y-2) has one or more hydroxyl groups in the molecule.

[0013] [7] The water-based lubricant composition according to any one of [1] to [6], wherein the content of the amine compound (Y) is 10 to 60 parts by mass per 100 parts by mass of the graft-modified ethylene-α-olefin copolymer (X).

[0014] [8] The water-based lubricant composition according to any one of [1] to [7], wherein the content of the silicone oil (Z) is 10 to 50 mass % relative to 100 mass % of the water-based lubricant composition.

[0015] [9] The water-based lubricant composition according to any one of [1] to [8], further comprising a surfactant.

[0016]

[10] The water-based lubricant composition according to [9], wherein the surfactant is a nonionic surfactant. Effect of the Invention

[0017] The water-based lubricant composition of the present invention has excellent emulsification properties, that is, the lubricant oil component contained therein is well dispersed in water.Furthermore, the water-based lubricant composition of the present invention can suppress adhesion of heat-deteriorated products to metal, so that when used as a lubricant, the number of times of removing heat-deteriorated products derived from lubricant from metal molds and around machines can be reduced, and therefore the cycle time of die casting can be shortened, that is, the work efficiency can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [Water-based lubricant composition] The water-based lubricant composition of the present invention (hereinafter also referred to as "the composition") contains a graft-modified ethylene-α-olefin copolymer (X) having a main chain portion derived from an ethylene-α-olefin copolymer (A) satisfying specified requirements and a graft portion derived from an unsaturated monomer (B) satisfying specified requirements, an amine compound (Y), at least one silicone oil (Z) selected from the group consisting of alkyl-modified silicone oils and alkylaralkyl-modified silicone oils, and water.

[0019] <Graft modified ethylene-α-olefin copolymer (X)> The graft-modified ethylene-α-olefin copolymer (X) (hereinafter also referred to as "modified copolymer (X)"), which is one of the components contained in the present composition, is a graft-modified copolymer having a main chain portion derived from the ethylene-α-olefin copolymer (A) and a graft portion derived from an unsaturated monomer (B) that satisfies specified requirements.

[0020] The modified copolymer (X) preferably satisfies one or more of the following requirements (x-1) to (x-5), more preferably satisfies two or more simultaneously, even more preferably satisfies three or more simultaneously, and particularly preferably satisfies all of them simultaneously. (x-1) The proportion of the graft portion is 0.1% by mass or more and less than 70% by mass (wherein the total amount of the main chain portion and the graft portion is 100% by mass). (x-2) The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000. (x-3) No melting point (Tm) is observed as measured by differential scanning calorimetry (DSC). (x-4) Kinematic viscosity at 100°C is 10 to 5,000 mm 2 / s. (x-5) The molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less.

[0021] <Requirements(x-1)> The proportion of the graft moiety in the modified copolymer (X) is preferably 0.1% by mass or more and less than 70% by mass, more preferably 0.5 to 50% by mass, and even more preferably 1.0 to 30% by mass, where the total amount of the main chain moiety and the graft moiety is 100% by mass. When the modified copolymer (X) having the proportion of the graft moiety in the above range is used, adhesion of thermally deteriorated products of the obtained water-based lubricant composition to metals tends to be suppressed. In this specification, the proportion of the graft portion of the modified copolymer can be determined by, for example, quantifying the hydroxyl group content in a sample by measuring the hydroxyl value by an acetylation method, and calculating the proportion of the unsaturated monomer (B) used for modification from the value.

[0022] <Requirements (x-2)> The weight average molecular weight (Mw) of the modified copolymer (X) determined by gel permeation chromatography (GPC) is preferably 1,500 to 30,000, more preferably 1,500 to 13,500, and even more preferably 1,500 to 11,000. When the modified copolymer (X) having a weight average molecular weight within the above range is used, adhesion of thermally deteriorated products of the resulting water-based lubricant composition to metals tends to be suppressed. In this specification, the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) of the modified (co)polymer and the unmodified (co)polymer can be specifically measured according to the method described in the examples described later.

[0023] <Requirements (x-3)> The melting point (Tm) of the modified copolymer (X) measured by differential scanning calorimetry (DSC) is preferably not observed. When such a modified copolymer (X) is used, the adhesion of the thermally deteriorated product of the obtained water-based lubricant composition to metal tends to be suppressed. Here, the melting point (Tm) is not observed means that the heat of fusion (ΔH) (unit: J / g) measured by differential scanning calorimetry (DSC) is not substantially measured. The heat of fusion (ΔH) is not substantially measured means that no peak is observed in the differential scanning calorimetry (DSC) measurement, or the observed heat of fusion is 1 J / g or less. In this specification, the melting point (Tm) and heat of fusion (ΔH) of the modified (co)polymer and the unmodified (co)polymer can be calculated in accordance with JIS K 7121 from a DSC curve obtained by cooling to -100°C and then heating to 150°C at a heating rate of 10°C / min using a differential scanning calorimeter (e.g., DSC Pyris1 or DSC7 manufactured by PerkinElmer).

[0024] <Requirements (x-4)> The modified copolymer (X) preferably has a kinetic viscosity at 100°C of 10 to 5,000 mm, as measured in accordance with the method described in JIS K 2283. 2 / s, and more preferably 15 to 3,500 mm 2 / s, more preferably 20 to 2,500 mm 2 When the modified copolymer (X) having a kinetic viscosity at 100° C. within the above range is used, adhesion of thermally deteriorated products of the resulting water-based lubricant composition to metals tends to be suppressed.

[0025] <Requirements(x-5)> The molecular weight distribution (Mw / Mn) of the modified copolymer (X) determined by gel permeation chromatography (GPC) is preferably 2.5 or less, more preferably 1.4 to 2.1, and more preferably 1.5 to 2.0. When the modified copolymer (X) having a molecular weight distribution within the above range is used, adhesion of thermally deteriorated products of the resulting water-based lubricant composition to metals tends to be suppressed.

[0026] <Ethylene-α-olefin copolymer (A)> The ethylene-α-olefin copolymer (A) (hereinafter also referred to as "copolymer (A)") constituting the main chain portion of the modified copolymer (X) is a copolymer of ethylene and an α-olefin, and the α-olefin copolymerized with ethylene may be an α-olefin having a carbon number of 3 to 20. One type of copolymer (A) or two or more types of copolymers may be used.

[0027] Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, and 1-octene are preferred, and propylene is particularly preferred.

[0028] The monomers constituting the ethylene-α-olefin copolymer (A), ethylene and an α-olefin having 3 to 20 carbon atoms, may consist only of monomers obtained from a biomass-derived raw material, may consist only of monomers obtained from a fossil fuel-derived raw material, or may be a mixture of monomers obtained from a biomass-derived raw material and monomers obtained from a fossil fuel-derived raw material.

[0029] The copolymer (A) satisfies the following requirements (a-1) to (a-3). (a-1) The content of ethylene units is 30 to 70 mol %. (a-2) The weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000. (a-3) No melting point (Tm) is observed as measured by differential scanning calorimetry (DSC).

[0030] <Requirement (a-1)> The content of structural units derived from ethylene in the copolymer (A) (hereinafter simply referred to as "ethylene unit content") is 30 to 70 mol%, preferably 30 to 65 mol%, more preferably 39 to 50 mol%, more preferably 41 to 48 mol%, provided that the sum of the content of structural units derived from ethylene and the content of structural units derived from α-olefin is 100 mol%. In this specification, the content of the structural units derived from each monomer in the (co)polymer is, for example, 13 It can be measured by C-NMR method, and the amount can be determined from the spectrum obtained based on the reports of GJ Ray (Macromolecules, 10, 773 (1977)), JC Randal (Macromolecules, 15, 353 (1982)), K. Kimura (Polymer, 25, 4418 (1984)), etc. Specifically, it can be measured according to the method described in the Examples below.

[0031] <Requirement (a-2)> The weight average molecular weight (Mw) of the copolymer (A) determined by gel permeation chromatography (GPC) is from 1,500 to 30,000, preferably from 1,500 to 13,500, and more preferably from 1,500 to 11,000.

[0032] <Requirement (a-3)> The copolymer (A) does not show a melting point as measured by differential scanning calorimetry (DSC).

[0033] The copolymer (A) preferably further satisfies either of the following requirements (a-4) and (a-5), and more preferably satisfies both of the following requirements (a-4) and (a-5). (a-4) Kinematic viscosity at 100°C is 10 to 5,000 mm 2 / s. (a-5) The molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less.

[0034] <Requirement (a-4)> The copolymer (A) has a kinematic viscosity at 100°C of 10 to 5,000mm, as measured in accordance with the method described in JIS K 2283. 2 / s, preferably 15 to 3,500 mm 2 / s, more preferably 20 to 2,500 mm 2 / s.

[0035] <Requirement (a-5)> The molecular weight distribution (Mw / Mn) of the copolymer (A) determined by gel permeation chromatography (GPC) is not particularly limited, but is preferably 2.5 or less, more preferably 1.4 to 2.1, and more preferably 1.5 to 2.0.

[0036] <Production method of ethylene-α-olefin copolymer (A)> The method for producing the ethylene-α-olefin copolymer (A) according to the present invention is not particularly limited, and examples thereof include a method using a vanadium catalyst consisting of a vanadium compound and an organoaluminum compound as described in JP-B-2-1163 and JP-B-2-7998. As a method for producing a copolymer with high polymerization activity, a method using a catalyst system consisting of a metallocene compound such as zirconocene and an organoaluminum oxy compound (aluminoxane) as described in JP-A-61-221207, JP-B-7-121969 and Japanese Patent No. 2796376 may also be used, and this method is more preferred since it can reduce the chlorine content of the resulting copolymer and the 2,1-insertion of α-olefin.

[0037] In the method using vanadium catalyst, a larger amount of chlorine compound is used as a cocatalyst than in the method using metallocene catalyst, so there is a high possibility that a small amount of chlorine will remain in the obtained copolymer (A). On the other hand, in the method using metallocene catalyst, since substantially no chlorine remains, it is preferable in that deterioration of the resin composition due to chlorine can be prevented. The chlorine content is preferably 100 ppm or less, more preferably 50 ppm or less, even more preferably 20 ppm or less, and particularly preferably 5 ppm or less. The chlorine content can be quantified by various known methods, such as a method in which a copolymer is placed in a sample boat and combusted at a combustion furnace set temperature of 900°C in an Ar / O2 gas stream using Thermo Fisher Scientific ICS-1600, and the generated gas is absorbed in an absorbing solution and quantified by ion chromatography.

[0038] In particular, by using the following method, it is possible to obtain a copolymer (A) having a good balance of performance in terms of molecular weight control, molecular weight distribution, amorphousness, etc.

[0039] The copolymer (A) can be produced by copolymerizing ethylene and an α-olefin having 3 to 20 carbon atoms in the presence of an olefin polymerization catalyst containing a bridged metallocene compound (P) represented by the following general formula [I], and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair.

[0040] [ka]

[0041] [Bridged metallocene compound (P)] The bridged metallocene compound (P) is represented by the above formula [I]. 1 ~R 14 , Q, n and j are explained below.

[0042] (Y, M, R 1 ~R 14 , Q, n and j) Y is a Group 14 atom, examples of which include a carbon atom, a silicon atom, a germanium atom and a tin atom, and is preferably a carbon atom or a silicon atom, and more preferably a carbon atom.

[0043] M is a titanium atom, a zirconium atom or a hafnium atom, and is preferably a zirconium atom.

[0044] R 1 ~R 14 are atoms or substituents selected from the group consisting of hydrogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms and halogen-containing groups, and may be the same or different. 1 From R 14 Adjacent substituents up to may be bonded to each other to form a ring, or may not be bonded to each other.

[0045] Here, examples of the hydrocarbon group having 1 to 20 carbon atoms include an alkyl group having 1 to 20 carbon atoms, a cyclic saturated hydrocarbon group having 3 to 20 carbon atoms, a linear unsaturated hydrocarbon group having 2 to 20 carbon atoms, a cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, an alkylene group having 1 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms.

[0046] Examples of the alkyl group having 1 to 20 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, n-propyl, allyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decanyl, and branched saturated hydrocarbon groups such as isopropyl, isobutyl, s-butyl, t-butyl, t-amyl, neopentyl, 3-methylpentyl, 1,1-diethylpropyl, 1,1-dimethylbutyl, 1-methyl-1-propylbutyl, 1,1-propylbutyl, 1,1-dimethyl-2-methylpropyl, 1-methyl-1-isopropyl-2-methylpropyl, and cyclopropylmethyl. The number of carbon atoms in the alkyl group is preferably 1 to 6.

[0047] Examples of cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms include cyclic saturated hydrocarbon groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, norbornenyl, 1-adamantyl, and 2-adamantyl, and groups in which hydrogen atoms of cyclic saturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 17 carbon atoms such as 3-methylcyclopentyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 4-cyclohexylcyclohexyl, and 4-phenylcyclohexyl. The number of carbon atoms in the cyclic saturated hydrocarbon group is preferably 5 to 11.

[0048] Examples of the linear unsaturated hydrocarbon group having 2 to 20 carbon atoms include alkenyl groups such as ethenyl group (vinyl group), 1-propenyl group, 2-propenyl group (allyl group), 1-methylethenyl group (isopropenyl group), etc., and alkynyl groups such as ethynyl group, 1-propynyl group, 2-propynyl group (propargyl group), etc. The number of carbon atoms in the linear unsaturated hydrocarbon group is preferably 2 to 4.

[0049] Examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms include cyclic unsaturated hydrocarbon groups such as cyclopentadienyl, norbornyl, phenyl, naphthyl, indenyl, azulenyl, phenanthryl, and anthracenyl, groups in which hydrogen atoms of cyclic unsaturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 15 carbon atoms such as 3-methylphenyl (m-tolyl), 4-methylphenyl (p-tolyl), 4-ethylphenyl, 4-t-butylphenyl, 4-cyclohexylphenyl, biphenylyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, and 2,4,6-trimethylphenyl (mesityl), groups in which hydrogen atoms of linear hydrocarbon groups or branched saturated hydrocarbon groups are replaced with cyclic saturated hydrocarbon groups or cyclic unsaturated hydrocarbon groups having 3 to 19 carbon atoms such as benzyl and cumyl. The number of carbon atoms of the cyclic unsaturated hydrocarbon group is preferably 6 to 10.

[0050] Examples of the alkylene group having 1 to 20 carbon atoms include a methylene group, an ethylene group, a dimethylmethylene group (an isopropylidene group), an ethylmethylene group, a methylethylene group, an n-propylene group, etc. The number of carbon atoms in the alkylene group is preferably 1 to 6.

[0051] Examples of the arylene group having 6 to 20 carbon atoms include an o-phenylene group, an m-phenylene group, a p-phenylene group, a 4,4'-biphenylylene group, etc. The number of carbon atoms in the arylene group is preferably 6 to 12.

[0052] Examples of the silicon-containing group include alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, t-butyldimethylsilyl group, and triisopropylsilyl group, which are groups in which carbon atoms in a hydrocarbon group having 1 to 20 carbon atoms are replaced with silicon atoms, arylsilyl groups such as dimethylphenylsilyl group, methyldiphenylsilyl group, and t-butyldiphenylsilyl group, pentamethyldisilanyl group, and trimethylsilylmethyl group, etc. The number of carbon atoms in the alkylsilyl group is preferably 1 to 10, and the number of carbon atoms in the arylsilyl group is preferably 6 to 18.

[0053] Examples of the nitrogen-containing group include an amino group, a group in which the =CH- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms or silicon-containing group is replaced with a nitrogen atom, a group in which the -CH2- structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded, or a group in which the -CH3 structural unit is replaced with a nitrogen atom to which a hydrocarbon group having 1 to 20 carbon atoms is bonded or a nitrile group, such as a dimethylamino group, a diethylamino group, an N-morpholinyl group, a dimethylaminomethyl group, a cyano group, a pyrrolidinyl group, a piperidinyl group, a pyridinyl group, an N-morpholinyl group, and a nitro group. As the nitrogen-containing group, a dimethylamino group and an N-morpholinyl group are preferred.

[0054] Examples of the oxygen-containing group include a hydroxyl group, a group in which the -CH2- structural unit in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group or nitrogen-containing group is replaced with an oxygen atom or a carbonyl group, or a group in which the -CH3 structural unit is replaced with an oxygen atom bonded to a hydrocarbon group having 1 to 20 carbon atoms, such as a methoxy group, ethoxy group, t-butoxy group, phenoxy group, trimethylsiloxy group, methoxyethoxy group, hydroxymethyl group, methoxymethyl group, ethoxymethyl group, t-butoxymethyl group, 1-hydroxyethyl group, 1-methyl ... Examples of the oxygen-containing group include 1-methoxyethyl group, 1-ethoxyethyl group, 2-hydroxyethyl group, 2-methoxyethyl group, 2-ethoxyethyl group, n-2-oxabutylene group, n-2-oxapentylene group, n-3-oxapentylene group, aldehyde group, acetyl group, propionyl group, benzoyl group, trimethylsilylcarbonyl group, carbamoyl group, methylaminocarbonyl group, carboxy group, methoxycarbonyl group, carboxymethyl group, ethoxycarboxymethyl group, carbamoylmethyl group, furanyl group, and pyranyl group. As the oxygen-containing group, a methoxy group is preferable.

[0055] Examples of halogen atoms include Group 17 elements such as fluorine, chlorine, bromine, and iodine.

[0056] Examples of the halogen-containing group include a trifluoromethyl group, a tribromomethyl group, a pentafluoroethyl group, a pentafluorophenyl group, and the like, which are groups in which a hydrogen atom in the above-mentioned hydrocarbon group having 1 to 20 carbon atoms, silicon-containing group, nitrogen-containing group, or oxygen-containing group is substituted with a halogen atom.

[0057] Q may be the same or different and selected in combination from a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, an anionic ligand, and a neutral ligand capable of coordinating with a lone electron pair. Details of the halogen atom and the hydrocarbon group having 1 to 20 carbon atoms are as described above. When Q is a halogen atom, it is preferably a chlorine atom. When Q is a hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group preferably has 1 to 7 carbon atoms.

[0058] Examples of the anionic ligand include alkoxy groups such as methoxy, t-butoxy, and phenoxy groups, carboxylate groups such as acetate and benzoate, and sulfonate groups such as mesylate and tosylate.

[0059] Examples of neutral ligands capable of coordinating with lone electron pairs include organic phosphorus compounds such as trimethylphosphine, triethylphosphine, triphenylphosphine, and diphenylmethylphosphine, and ether compounds such as tetrahydrofuran, diethyl ether, dioxane, and 1,2-dimethoxyethane.

[0060] j is an integer of 1 to 4, and is preferably 2. n is an integer of 1 to 4, preferably 1 or 2, and more preferably 1. R 13 and R 14 are atoms or substituents selected from the group consisting of hydrogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, aryl groups, substituted aryl groups, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms and halogen-containing groups, and may be the same or different. 13 and R 14 may be bonded to each other to form a ring, or may not be bonded to each other.

[0061] Details of the hydrocarbon group having 1 to 20 carbon atoms, the silicon-containing group, the nitrogen-containing group, the oxygen-containing group, the halogen atom and the halogen-containing group are as described above. Examples of the aryl group include, but are not limited to, the above-mentioned examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, and are exemplified by substituents derived from aromatic compounds, such as phenyl, 1-naphthyl, 2-naphthyl, anthracenyl, phenanthrenyl, tetracenyl, chrysenyl, pyrenyl, indenyl, azulenyl, pyrrolyl, pyridyl, furanyl, and thiophenyl groups. The aryl group is preferably a phenyl group or a 2-naphthyl group.

[0062] Examples of the aromatic compounds include aromatic hydrocarbons and heterocyclic aromatic compounds such as benzene, naphthalene, anthracene, phenanthrene, tetracene, chrysene, pyrene, indene, azulene, pyrrole, pyridine, furan, and thiophene.

[0063] The substituted aryl group partially overlaps with the examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms described above, but examples include groups in which one or more hydrogen atoms of the aryl group are substituted with at least one substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms, an aryl group, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom, and a halogen-containing group. Specific examples include a 3-methylphenyl group (m-tolyl group), a 4-methylphenyl group (p-tolyl group), a 3-ethylphenyl group, a 4-ethylphenyl group, a 3,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a biphenylyl group, a 4-(trimethylsilyl)phenyl group, a 4-aryl ... Examples of such an aminophenyl group include a 4-(dimethylamino)phenyl group, a 4-(diethylamino)phenyl group, a 4-morpholinylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-phenoxyphenyl group, a 3,4-dimethoxyphenyl group, a 3,5-dimethoxyphenyl group, a 3-methyl-4-methoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3-(trifluoromethyl)phenyl group, a 4-(trifluoromethyl)phenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 5-methylnaphthyl group, and a 2-(6-methyl)pyridyl group.

[0064] Among them, R 13 and R 14 A bridged metallocene compound (P) in which either one or both of the above are independently an aryl group is preferred, and a bridged metallocene compound (P) in which both of the above are independently an aryl group is more preferred.

[0065] In particular, R 13 and R 14The bridged metallocene compound (P) in which both are independently aryl groups has high polymerization activity for copolymerization of ethylene and α-olefin, and the use of this bridged metallocene compound (P) selectively terminates polymerization by introduction of hydrogen into the molecular end, resulting in fewer unsaturated bonds in the resulting copolymer (A). Therefore, by simply performing a simpler hydrogen addition operation or without performing a hydrogen addition operation, a copolymer (A) having a high degree of saturation and excellent heat resistance can be obtained, which is also excellent in terms of cost. In addition, the copolymer (A) obtained from the compound (P) has a controlled molecular weight distribution due to its high random copolymerization property. Therefore, the present composition containing the graft-modified copolymer (X) having a main chain portion derived from the copolymer (A) obtained by graft-modifying the following unsaturated monomer (B) and a graft portion derived from the unsaturated monomer (B) in the copolymer (A) is considered to have a high level of defoaming property and excellent bleed-out resistance in a well-balanced manner.

[0066] In the bridged metallocene compound (P) represented by the formula [I], n is preferably 1. Such a bridged metallocene compound (hereinafter also referred to as "bridged metallocene compound (P-1)") is represented by the following general formula [II].

[0067] [ka]

[0068] In formula [II], Y, M, R 1 ~R 14 The definitions of Q and j are as described above.

[0069] The bridged metallocene compound (P-1) has a simplified production process and reduced production costs compared to the compound in the above formula [I] where n is an integer of 2 to 4, and thus the use of this bridged metallocene compound (P-1) has the advantage of reducing the production costs of the copolymer (A).

[0070] In the bridged metallocene compound (P) represented by the above general formula [I] and the bridged metallocene compound (P-1) represented by the above general formula [II], M is more preferably a zirconium atom. When ethylene and one or more monomers selected from α-olefins having 3 to 20 carbon atoms are copolymerized in the presence of an olefin polymerization catalyst containing the above bridged metallocene compound in which M is a zirconium atom, the polymerization activity is higher than when M is a titanium atom or a hafnium atom, and the production cost of the copolymer (B) can be advantageously reduced.

[0071] Examples of such bridged metallocene compounds (P) include [Dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Dimethylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [cyclohexylidene(η 5-cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [cyclohexylidene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -2-methyl-4-t-butylcyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene{η 5 -(2-methyl-4-i-propylcyclopentadienyl)}(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5-cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methylphenylmethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5-3,6-di-t-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylsilylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silyl(η 5 -cyclopentadienyl)(η 5-octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -Octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dicyclohexylsilylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [Ethylene(η 5 -cyclopentadienyl)(η 5 -fluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -2,7-di-t-butylfluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -3,6-di-t-butylfluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [ethylene(η 5 -cyclopentadienyl)(η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5-(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Ethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5-(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5-(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5-(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5-(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5-(3-tert-Butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-Butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, Di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -Fluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5-(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](2,7-diphenyl-3,6-di-tert-butylfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride.

[0072] Examples of the bridged metallocene compound (P) include compounds in which the zirconium atom of the above-mentioned compound is replaced with a hafnium atom or a titanium atom, and compounds in which the chloro ligand is replaced with a methyl group. 5 -Tetramethyloctahydrodibenzofluorenyl is 4,4,7,7-tetramethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, η 5 -Octamethyloctahydrodibenzofluorenyl is 1,1,4,4,7,7,10,10-octamethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, respectively. The crosslinked metallocene compound (P) may be used alone or in combination of two or more kinds.

[0073] [Compound (Q)] The compound (Q) according to the present invention is at least one compound selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the crosslinked metallocene compound (P) to form an ion pair. Specific examples of the organometallic compound (Q-1) include organometallic compounds (Q-1a), (Q-1b), and (Q-1c) of Groups 1, 2, 12, and 13 of the periodic table as follows.

[0074] (Q-1a) General formula R a m Al(OR b ) n H p X q An organoaluminum compound represented by. (In the formula, R a and R b may be the same as or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms, X represents a halogen atom, m is 0 < m ≦ 3, n is 0 ≦ n < 3, p is 0 ≦ p < 3, q is 0 ≦ q < 3, and m + n + p + q = 3.)

[0075] Examples of such compounds include tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tri-n-hexylaluminum, and tri-n-octylaluminum; tri-branched alkylaluminums such as triisopropylaluminum, triisobutylaluminum, trisec-butylaluminum, tri-t-butylaluminum, tri-2-methylbutylaluminum, tri-3-methylhexylaluminum, and tri-2-ethylhexylaluminum; tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum; triarylaluminums such as triphenylaluminum and tri(4-methylphenyl)aluminum; dialkylaluminum hydrides such as diisopropylaluminum hydride and diisobutylaluminum hydride; and compounds represented by the general formula (i-C4H9) x Al y (C5H 10 ) z (wherein x, y, and z are positive numbers, and z≦2x), alkenyl aluminum such as isoprenyl aluminum, alkyl aluminum alkoxides such as isobutyl aluminum methoxide and isobutyl aluminum ethoxide, dialkyl aluminum alkoxides such as dimethyl aluminum methoxide, diethyl aluminum ethoxide, and dibutyl aluminum butoxide, alkyl aluminum sesquialkoxides such as ethyl aluminum sesquiethoxide and butyl aluminum sesquibutoxide, and alkyl aluminum sesquialkoxides represented by the general formula R a 2.5 Al(OR b ) 0.5Examples of the alkylaluminum include partially alkoxylated alkylaluminums having an average composition represented by the formula (I) above, alkylaluminum aryloxides such as diethylaluminum phenoxide and diethylaluminum (2,6-di-t-butyl-4-methylphenoxide), dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide and diisobutylaluminum chloride, alkylaluminum sesquihalides such as ethylaluminum sesquichloride, butylaluminum sesquichloride and ethylaluminum sesquibromide, partially halogenated alkylaluminums such as alkylaluminum dihalides such as ethylaluminum dichloride, dialkylaluminum hydrides such as diethylaluminum hydride and dibutylaluminum hydride, alkylaluminum dihydrides such as ethylaluminum dihydride and propylaluminum dihydride, and other partially hydrogenated alkylaluminums, partially alkoxylated and halogenated alkylaluminums such as ethylaluminum ethoxy chloride, butylaluminum butoxy chloride and ethylaluminum ethoxy bromide. a m Al(OR b ) n H p X q Compounds similar to the compound represented by the formula (1) can also be used, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms. Specific examples of such compounds include (C2H5)2AlN(C2H5)Al(C2H5)2.

[0076] (Q-1b) General formula M 2 AlR a 4, a complex alkylation product of a metal of Group 1 of the periodic table and aluminum. (Wherein, M 2 indicates Li, Na or K, and R a represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms. Such compounds include LiAl(C2H5)4, LiAl(C7H 15 ) 4 can be given as an example.

[0077] (Q-1c) General formula R a R b M 3 A dialkyl compound of a metal of Group 2 or 12 of the periodic table represented by the formula: a and R b may be the same or different and each represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; M 3 is Mg, Zn or Cd.)

[0078] As the organoaluminum oxy compound (Q-2), a conventionally known aluminoxane can be used as it is.Specific examples include a compound represented by the following general formula [III] and a compound represented by the following general formula [IV].

[0079] [ka]

[0080] In the formulas [III] and [IV], R represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 2 or more.

[0081] In particular, methylaluminoxanes in which R is a methyl group and n is at least 3, preferably at least 10, are used. There is no problem if these aluminoxanes contain a small amount of an organoaluminum compound.

[0082] In the present invention, when copolymerization of ethylene with an α-olefin having 3 or more carbon atoms is carried out at high temperature, benzene-insoluble organoaluminum oxy compounds as exemplified in JP-A-2-78687 can also be used. In addition, organoaluminum oxy compounds described in JP-A-2-167305, aluminoxanes having two or more alkyl groups described in JP-A-2-24701 and JP-A-3-103407, etc. can also be suitably used. The "benzene-insoluble organoaluminum oxy compounds" that may be used in the present invention are compounds that are insoluble or poorly soluble in benzene, and that have an Al component that dissolves in benzene at 60°C in terms of Al atoms of usually 10% or less, preferably 5% or less, and particularly preferably 2% or less.

[0083] Further, the organoaluminum oxy compound (Q-2) may also include modified methylaluminoxanes as represented by the following general formula [V].

[0084] [ka]

[0085] In formula [V], Rx represents a hydrocarbon group having 1 to 10 carbon atoms, and m and n each independently represent an integer of 2 or more.

[0086] Methylaluminoxane, an example of an organoaluminum oxy compound (Q-2), is commonly used as an activator in olefin polymerization because it is readily available and has high polymerization activity. However, methylaluminoxane is difficult to dissolve in saturated hydrocarbons, and has been used as a solution in aromatic hydrocarbons such as toluene or benzene, which are environmentally undesirable. For this reason, a flexible body of methylaluminoxane represented by formula [V] has been developed and used in recent years as an aluminoxane dissolved in saturated hydrocarbons. This modified methylaluminoxane represented by formula [V] is prepared using trimethylaluminum and alkylaluminum other than trimethylaluminum, for example, trimethylaluminum and triisobutylaluminum, as shown in, for example, U.S. Pat. No. 4,960,878 and U.S. Pat. No. 5,041,584. Aluminoxanes in which Rx is an isobutyl group are commercially available in the form of saturated hydrocarbon solutions under the trade names MMAO and TMAO (see Tosoh Finechem Corporation, Tosoh Research&Technology Review, Vol 47, 55 (2003)).

[0087] Further, the organoaluminum oxy compound (Q-2) may also include a boron-containing organoaluminum oxy compound represented by the following general formula [VI].

[0088] [ka]

[0089] In formula [VI], R c R represents a hydrocarbon group having 1 to 10 carbon atoms. d may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.

[0090] Examples of the compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair (hereinafter, sometimes abbreviated as "ionized ionic compound" or simply "ionic compound") include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and U.S. Patent No. 5,321,106. Further examples include heteropoly compounds and isopoly compounds.

[0091] The ionizing ionic compound preferably used in the present invention is a boron compound represented by the following general formula [VII].

[0092] [ka]

[0093] In formula [VII], R e+ As for H + , carbenium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. f ~R i may be the same or different and are substituents selected from a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom and a halogen-containing group, and are preferably substituted aryl groups.

[0094] Specific examples of the carbenium cation include tri-substituted carbenium cations such as triphenylcarbenium cation, tris(4-methylphenyl)carbenium cation, and tris(3,5-dimethylphenyl)carbenium cation.

[0095] Specific examples of the ammonium cation include trialkyl-substituted ammonium cations such as trimethylammonium cation, triethylammonium cation, tri(n-propyl)ammonium cation, triisopropylammonium cation, tri(n-butyl)ammonium cation, and triisobutylammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation.

[0096] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tris(4-methylphenyl)phosphonium cation, and tris(3,5-dimethylphenyl)phosphonium cation.

[0097] R e+ Of the above specific examples, preferred are carbenium cations and ammonium cations, with triphenylcarbenium cation, N,N-dimethylanilinium cation and N,N-diethylanilinium cation being particularly preferred.

[0098] Among the ionized ionic compounds preferably used in the present invention, examples of compounds containing a carbenium cation include triphenylcarbenium tetraphenylborate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis{3,5-di-(trifluoromethyl)phenyl}borate, tris(4-methylphenyl)carbenium tetrakis(pentafluorophenyl)borate, and tris(3,5-dimethylphenyl)carbenium tetrakis(pentafluorophenyl)borate.

[0099] Among the ionizing ionic compounds preferably used in the present invention, compounds containing a trialkyl-substituted ammonium cation include triethylammonium tetraphenylborate, tripropylammonium tetraphenylborate, tri(n-butyl)ammonium tetraphenylborate, trimethylammonium tetrakis(4-methylphenyl)borate, trimethylammonium tetrakis(2-methylphenyl)borate, tri(n-butyl)ammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(2,4-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis(3,5-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis{4-(trifluoromethyl)phenyl}borate, tri Examples of the borate include (n-butyl)ammonium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, tri(n-butyl)ammonium tetrakis(2-methylphenyl)borate, dioctadecylmethylammonium tetraphenylborate, dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(2,4-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(3,5-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis{4-(trifluoromethyl)phenyl}borate, dioctadecylmethylammonium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, and dioctadecylmethylammonium.

[0100] Among the ionizing ionic compounds preferably used in the present invention, examples of compounds containing an N,N-dialkylanilinium cation include N,N-dimethylanilinium tetraphenylborate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-diethylanilinium tetraphenylborate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-2,4,6-pentamethylanilinium tetraphenylborate, and N,N-2,4,6-pentamethylanilinium tetrakis(pentafluorophenyl)borate.

[0101] Among the ionizing ionic compounds preferably used in the present invention, examples of compounds containing a dialkylammonium cation include di-n-propylammonium tetrakis(pentafluorophenyl)borate and dicyclohexylammonium tetraphenylborate.

[0102] In addition, the ionic compounds exemplified in JP-A-2004-51676 can also be used without any restrictions. The above ionic compounds (Q-3) may be used alone or in combination of two or more.

[0103] Examples of the catalyst system include the following [1] to [4]. [1] Bridged metallocene compound (P) and compound (Q-2) [2] Includes bridged metallocene compound (P), compound (Q-1) and compound (Q-2) [3] Bridged metallocene compound (P), compound (Q-1) and compound (Q-3) are included. [4] Includes bridged metallocene compound (P), compound (Q-2) and compound (Q-3) The bridged metallocene compound (P) and the compounds (Q-1) to (Q-3) may be introduced into the reaction system in any order.

[0104] [Carrier (R)] In the present invention, a support (R) may be used as a constituent component of the olefin polymerization catalyst, if necessary.

[0105] The carrier (R) that may be used in the present invention is an inorganic or organic compound, which is a granular or particulate solid. Among these, the inorganic compound is preferably a porous oxide, an inorganic chloride, a clay, a clay mineral, or an ion-exchangeable layered compound.

[0106] As the porous oxide, specifically, SiO2, Al2O3, MgO, ZrO, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc., or a composite or mixture containing these, such as natural or synthetic zeolite, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-V2O5, SiO2-Cr2O3, SiO2-TiO2-MgO, etc. can be used. Among these, those containing SiO2 and / or Al2O3 as the main component are preferred. Although the properties of such porous oxides vary depending on the type and manufacturing method, the carrier preferably used in the present invention has a particle size of 0.5 to 300 μm, preferably 1.0 to 200 μm, and a specific surface area of ​​50 to 1000 m. 2 / g, preferably 100 to 700m 2 / g and the pore volume is 0.3-3.0 cm 3 The carrier is calcined at 100 to 1000° C., preferably 150 to 700° C., as required, before use.

[0107] Examples of inorganic chlorides that can be used include MgCl2, MgBr2, MnCl2, and MnBr2. The inorganic chlorides can be used as they are, or can be used after being pulverized by a ball mill or a vibration mill. In addition, the inorganic chlorides can be dissolved in a solvent such as alcohol, and then precipitated into fine particles using a precipitating agent.

[0108] Clay is usually composed of clay minerals as the main component. In addition, an ion-exchangeable layered compound is a compound having a crystal structure in which the constituent faces are stacked in parallel with each other with weak bonding force due to ionic bonds, etc., and the ions contained therein are exchangeable. Most clay minerals are ion-exchangeable layered compounds. In addition, these clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used. In addition, examples of clays, clay minerals, and ion-exchangeable layered compounds include clays, clay minerals, and ionic crystalline compounds having layered crystal structures such as hexagonal close packing type, antimony type, CdCl2 type, and CdI2 type. Examples of such clays and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, and halloysite, and examples of ion-exchangeable layered compounds include α-Zr(HAsO4)2·H2O, α-Zr(HPO4)2, α-Zr(KPO4)2·3H2O, α-Ti(HPO4)2, α-Ti(HAsO4)2·H2O, α-Sn(HPO4)2·H2O, γ-Zr(HPO4)2, γ-Ti(HPO4)2, and γ-Ti(NH4PO4)2·H2O, and other crystalline acid salts of polyvalent metals. It is also preferable to subject the clay and clay minerals used in the present invention to chemical treatment. The chemical treatment may be any of surface treatments that remove impurities adhering to the surface, treatments that affect the crystal structure of the clay, etc. Specific examples of the chemical treatment include acid treatment, alkali treatment, salt treatment, and organic matter treatment.

[0109] The ion-exchangeable layered compound may be a layered compound in which the space between layers is expanded by utilizing the ion exchangeability and exchanging the exchangeable ions between layers with other large bulky ions. Such bulky ions play a role of supporting the layered structure and are usually called pillars. The introduction of another substance (guest compound) between layers of a layered compound in this way is called intercalation. Examples of guest compounds include cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (R is a hydrocarbon group, etc.), [Al 13 O4(OH) 24 ] 7+ , [Zr4(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + Metal hydroxide ions such as these can be used. These compounds can be used alone or in combination of two or more. When these compounds are intercalated, polymers obtained by hydrolysis and polycondensation of metal alkoxides such as Si(OR)4, Al(OR)3, Ge(OR)4 (R is a hydrocarbon group, etc.), colloidal inorganic compounds such as SiO2, etc. can also be coexisted. Examples of pillars include oxides produced by intercalating the above metal hydroxide ions between layers and then dehydrating them with heat.

[0110] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred. The organic compound as the carrier (R) may be a granular or fine particle solid having a particle size in the range of 0.5 to 300 μm. Specifically, it may be a (co)polymer produced mainly from an α-olefin having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, or 4-methyl-1-pentene, or a (co)polymer produced mainly from vinylcyclohexane or styrene, or a modified product thereof.

[0111] The method of use and order of addition of each component of the polymerization catalyst may be selected arbitrarily, and at least two of the components in the catalyst may be contacted in advance. The bridged metallocene compound (P) (hereinafter also referred to as "component (P)") is usually 10 -9 ~10 -1 mol, preferably 10 -8 ~10 -2 It is used in amounts that equal mol.

[0112] The organometallic compound (Q-1) (hereinafter also referred to as "component (b-1)") is used in an amount such that the molar ratio of component (Q-1) to the transition metal atom (M) in component (P) [(Q-1) / M] is generally 0.01 to 50,000, preferably 0.05 to 10,000.

[0113] The organoaluminum oxy compound (Q-2) (hereinafter also referred to as "component (Q-2)") is used in an amount such that the molar ratio [(Q-2) / M] of the aluminum atom in component (Q-2) to the transition metal atom (M) in component (P) is generally 10 to 5,000, preferably 20 to 2,000.

[0114] The ionic compound (Q-3) (hereinafter also referred to as "component (Q-3)") is used in an amount such that the molar ratio of component (Q-3) to the transition metal atom (M) in component (P) [(Q-3) / M] is generally 1 to 10,000, preferably 1 to 5,000.

[0115] The polymerization temperature is usually -50 to 300°C, preferably 30 to 250°C, more preferably 100 to 250°C, and further preferably 130 to 200°C. In the polymerization temperature range, as the temperature increases, the solution viscosity during polymerization decreases and the heat of polymerization is easily removed. The polymerization pressure is usually normal pressure to 10 MPa gauge pressure (MPa-G), and preferably normal pressure to 8 MPa-G.

[0116] The polymerization reaction can be carried out in any of batch, semi-continuous and continuous systems. Furthermore, the polymerization can be carried out continuously in two or more polymerization vessels with different reaction conditions. The molecular weight of the resulting copolymer can be adjusted by changing the hydrogen concentration in the polymerization system and the polymerization temperature. It can also be adjusted by the amount of component (Q) used. When hydrogen is added, the appropriate amount is about 0.001 to 5,000 NL per kg of the copolymer produced.

[0117] The polymerization solvent used in the liquid phase polymerization method is usually an inert hydrocarbon solvent, and is preferably a saturated hydrocarbon having a boiling point of 50 to 200° C. under normal pressure. Specific examples of polymerization solvents include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, and alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane, and particularly preferred are hexane, heptane, octane, decane, and cyclohexane. The α-olefin itself to be polymerized can also be used as the polymerization solvent. Incidentally, aromatic hydrocarbons such as benzene, toluene, and xylene, and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane can also be used as the polymerization solvent, but the use of these is not preferred from the viewpoint of reducing the burden on the environment and minimizing the impact on human health.

[0118] The kinetic viscosity of the copolymer (A) at 100°C depends on the molecular weight of the polymer. That is, a high molecular weight results in a high viscosity, and a low molecular weight results in a low viscosity, so the kinetic viscosity at 100°C is adjusted by adjusting the molecular weight as described above. In addition, the molecular weight distribution (Mw / Mn) of the obtained polymer can be adjusted by removing low molecular weight components from the obtained polymer by a conventionally known method such as vacuum distillation. Furthermore, the obtained polymer may be hydrogenated (hereinafter also referred to as hydrogenation) by a conventionally known method. If the double bonds of the obtained polymer are reduced by hydrogenation, the oxidation stability and heat resistance are improved.

[0119] The resulting copolymer (A) may be used alone or in combination of two or more types having different molecular weights or different monomer compositions.

[0120] <Unsaturated Monomer (B)> The unsaturated monomer (B) constituting the graft moiety of the modified copolymer (X), which is one of the components contained in the present composition, satisfies the following requirement (b-1).

[0121] <Requirement (b-1)> The unsaturated monomer (B) is at least one unsaturated monomer selected from the group consisting of ethylenically unsaturated monomers having a hydroxyl group. The ethylenically unsaturated monomer having a hydroxyl group is a compound having a hydroxyl group and an ethylenically unsaturated bond in the molecule, and examples thereof include (meth)acrylic acid esters having a hydroxyl group in the ester moiety, unsaturated alcohols, styrene derivatives containing a hydroxyl group, and hydroxyvinyl ethers. Among these, unsaturated alcohols are preferred.

[0122] Examples of the (meth)acrylic acid ester having a hydroxyl group in the ester moiety include mono(meth)acrylate compounds of polyhydric alcohols, and specific examples thereof include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol mono(meth)acrylate, and polyethylene glycol mono(meth)acrylate.

[0123] Specific examples of the unsaturated alcohol include allyl alcohol, 2-allyloxyethanol, 2-methyl-3-buten-1-ol, 2-methyl-3-buten-2-ol, 3-methyl-3-buten-1-ol, 10-undecen-1-ol, 1-octen-3-ol, 2-methanolnorbornene, 2-butene-1,4-diol, etc. Among these, 2-allyloxyethanol, 2-methyl-3-buten-1-ol, and 2-methyl-3-buten-2-ol are preferred.

[0124] Examples of the hydroxyl group-containing styrene derivative include hydroxystyrene, etc. Specific examples of the hydroxyvinyl ether include hydroxymethyl vinyl ether, hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxymethyl propenyl ether, hydroxyethyl propenyl ether, hydroxypropyl propenyl ether, hydroxybutyl propenyl ether, hydroxymethyl butenyl ether, hydroxyethyl butenyl ether, hydroxypropyl butenyl ether, and hydroxybutyl butenyl ether.

[0125] In addition, as the ethylenically unsaturated monomer (b-2) having a hydroxyl group, N-methylolacrylamide, 2-(meth)acryloyloxyethyl acetylphosphate, glycerin monoallyl ether, allyloxyethanol, etc. can also be used. The unsaturated monomer (B) can be used alone or in combination of two or more kinds. The unsaturated monomer (B) may consist solely of monomers obtained from a biomass-derived raw material, may consist solely of monomers obtained from a fossil fuel-derived raw material, or may be a mixture of monomers obtained from a biomass-derived raw material and monomers obtained from a fossil fuel-derived raw material.

[0126] <Method for producing modified copolymer (X)> The modified copolymer (X) can be prepared by using various conventionally known methods, for example, the following method. (1) A method in which the copolymer (A) is mixed in an extruder, a batch reactor or the like, and the unsaturated monomer (B) is added thereto to carry out graft copolymerization. (2) A method in which the copolymer (A) is dissolved in a solvent, and the unsaturated monomer (B) is added thereto to carry out graft copolymerization.

[0127] In any of the above-mentioned production methods, the graft reaction is preferably carried out in the presence of a radical initiator in order to efficiently graft copolymerize the unsaturated monomer (B). As the radical initiator, for example, an organic peroxide, an azo compound, etc. are used. As the organic peroxide, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, etc. are mentioned, and as the azo compound, azobisisobutylnitrile, dimethylazoisobutyrate, etc. are mentioned.

[0128] Specific examples of such radical initiators that are preferably used include dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,4-bis(tert-butylperoxyisopropyl)benzene.

[0129] These radical initiators are used in an amount of usually 0.001 to 1 part by mass, preferably 0.003 to 0.5 parts by mass, and more preferably 0.05 to 0.3 parts by mass, based on 100 parts by mass of the copolymer (A).

[0130] The reaction temperature in the graft reaction using the above-mentioned radical initiator or in the graft reaction carried out without using any radical initiator is set in the range of usually 60 to 350°C, preferably 120 to 300°C.

[0131] The content of the modified copolymer (X) in the composition is preferably 0.1 to 10 mass%, more preferably 0.2 to 8 mass%, and more preferably 0.5 to 5 mass%, based on 100 mass% of the composition. When the content of the modified copolymer (X) is within the above range, the defoaming effect of the modified copolymer (X) is sufficiently exhibited.

[0132] <Amine compound (Y)> The composition contains an amine compound (Y). The amine compound (Y) preferably satisfies the following requirements (y-1) and (y-2). (y-1) The molecular weight is 1,000 or less. (y-2) has one or more hydroxyl groups in the molecule.

[0133] <Requirement (y-1)> The molecular weight of the amine compound (Y) is preferably not more than 1,000, more preferably not more than 800, and even more preferably not more than 500. When the molecular weight of the amine compound (Y) is within the above range, the modified copolymer (X) tends to have excellent emulsification property in water.

[0134] <Requirement (y-2)> The amine compound (Y) has one or more hydroxyl groups in the molecule. From the viewpoint of emulsification property of the modified copolymer (X) in water, the content of the amine compound (Y) can be appropriately changed depending on the number of hydroxyl groups in the molecule. It is particularly preferable that at least one of the hydroxyl groups present in the molecule of the amine compound (Y) is bonded to a primary carbon.

[0135] Examples of the amine compound (Y) include primary amine compounds such as 2-aminomethyl-1-propanol, 2-(2-aminoethoxy)ethanol, 2-aminoethanol, and 1-amino-2-propanol; secondary amine compounds such as diethanolamine and 2-methylaminoethanol; and tertiary amine compounds such as triethanolamine and 2-(dimethyl)aminoethanol. From the viewpoint of the emulsification property of the modified copolymer (X) in water, etc., primary amine compounds are preferred, and 2-aminomethyl-1-propanol and 2-(2-aminoethoxy)ethanol are more preferred.

[0136] The amine compound (Y) can be used alone or in combination of two or more kinds. The content of the amine compound (Y) can be appropriately changed depending on the number of hydroxyl groups in the molecule, but is preferably 10 to 60 parts by mass, more preferably 10 to 50 parts by mass, and even more preferably 15 to 50 parts by mass, per 100 parts by mass of the modified copolymer (X).

[0137] <Silicone oil (Z)> The present composition contains, as a lubricating oil component, at least one silicone oil (Z) selected from the group consisting of alkyl-modified silicone oils and alkylaralkyl-modified silicone oils. The silicone oil (Z) preferably satisfies the following requirement (z-1): (z-1) Viscosity at 25°C is 20mm 2 / s or more.

[0138] <Requirements (z-1)> The viscosity of the silicone oil (Z) at 25°C is preferably 20mm 2 / s or more, preferably 50 mm 2 / s or more, and more preferably 200 mm 2 When the viscosity of the silicone oil (Z) is within the above range, when the composition is used as a lubricant (mold release agent), the releasability from a mold is excellent.

[0139] Examples of the silicone oil (Z) include alkyl-modified silicone oil and alkylaralkyl-modified silicone oil, with alkylaralkyl-modified silicone oil being preferred.

[0140] The silicone oil (Z) may be blended in the form of an emulsion when preparing the composition. The emulsion is not particularly limited as long as it does not impair the effects of the present invention, but the non-volatile content concentration is preferably about 10 to 70 mass%. The non-volatile content concentration refers to the concentration of non-volatile components other than the dispersion solvent, including silicone oil (Z) and additives such as emulsifiers that are added as necessary.

[0141] The silicone oil (Z) can be used alone or in combination of two or more kinds. The content of the silicone oil (Z) is preferably from 10 to 50 mass %, more preferably from 12 to 45 mass %, and even more preferably from 15 to 40 mass %, based on 100 mass % of the present composition.

[0142] <Surfactants> The composition may further contain a surfactant, which promotes emulsification of the modified copolymer (X) and the silicone oil (Z) in water. Examples of the surfactant include anionic surfactants such as alkylnaphthalenesulfonates, sodium dodecylbenzenesulfonate, sodium lauryl sulfate, sodium salts of formaldehyde condensates, sodium alkyldiphenyletherdisulfonate, sodium melamine resin sulfonate, special polyacrylates, potassium oleate, olefin-maleic acid copolymers, sodium carboxymethylcellulose, potassium stearate, sodium stearate, and triethanolamine stearate; fatty acid monoglycerides, sorbitan fatty acid esters, polyglycerin fatty acid partial esters, polyoxyethylene alkyl esters, and the like. nonionic surfactants such as phenyl ether, polyoxyethylene sorbitan fatty acid partial esters, polyoxyethylene sorbitol fatty acid partial esters, polyoxyethylene glycerin fatty acid partial esters, polyoxyethylene fatty acid amines, polyoxyethylene (hydrogenated) castor oil, polyoxyethylene glycol fatty acid esters, hydroxyethyl cellulose, polyvinyl alcohol, and methyl cellulose; amphoteric surfactants such as alkyl ammonium chloride, trimethyl alkyl ammonium bromide, alkyl pyridinium chloride, and casein; and water-soluble polyvalent metal salts, among which nonionic surfactants are preferred.

[0143] The surfactants may be used alone or in combination of two or more. When the composition contains a surfactant, the content of the surfactant is preferably 10 to 50 parts by mass, more preferably 15 to 45 parts by mass, and even more preferably 20 to 40 parts by mass, based on 100 parts by mass of the modified copolymer (X).

[0144] ≪Water≫ The composition contains water, and the content of water is preferably 10 to 70% by mass, more preferably 20 to 70% by mass, and even more preferably 30 to 65% by mass, based on 100% by mass of the composition. Water is mainly used as a dispersion medium for emulsifying, dispersing, or solubilizing the lubricating oil components, but a water-soluble solvent may be added as long as it does not have a negative effect such as emulsion destruction in the emulsification, dispersion, or solubilization of the entire system, and does not cause quality degradation such as corrosion, reaction, or deterioration of the metal mold when used as a lubricant (mold release agent).

[0145] Examples of the water-soluble solvent include glycol-based solvents such as ethylene glycol, diethylene glycol, and triethylene glycol; carbitol-based solvents such as methyl carbitol and ethyl carbitol; and pyrrolidone-based solvents such as 2-pyrrolidone and N-methylpyrrolidone. These can be used alone or in combination of two or more. The amount of the water-soluble solvent added is preferably 1 to 70 parts by mass, more preferably 5 to 65 parts by mass, based on 100 parts by mass of water.

[0146] <Other ingredients> The present composition may contain other components, as necessary, in addition to the modified copolymer (X), the amine compound (Y), the silicone oil (Z), the surfactant, and water, as long as the effects of the present invention are not impaired. Examples of other components include resin components other than the modified copolymer (X), basic compounds other than the amine compound (Y), lubricating oil components other than the silicone oil (Z), emulsifiers, anticorrosives, antioxidants, preservatives, rust inhibitors, metal deactivators, anti-wear additives, antifoaming agents, pour point depressants, detergent dispersants, hard water softeners, chelating agents, pH adjusters, dyes, pigments, antifoaming agents, and fragrances. The other components may be used alone or in combination of two or more.

[0147] <Method for producing water-based lubricant composition> This composition can be produced, for example, by the following methods: (1) mixing an aqueous dispersion composition containing the modified copolymer (X), the amine compound (Y), the silicone oil (Z) and a surfactant with an aqueous solution of the silicone oil (Z); (2) emulsifying an oil droplet component containing the modified copolymer (X), the amine compound (Y), the silicone oil (Z) and a surfactant in water. The above methods will be described in detail below.

[0148] ·Method(1) First, the modified copolymer (X), the amine compound (Y), the surfactant, water, and other components as necessary are mixed by stirring appropriately to prepare an aqueous dispersion composition. During stirring and mixing, the components and the mixed liquid may be heated to 40 to 70°C as necessary. The order of addition of the components is not particularly limited as long as the components can be uniformly dissolved or dispersed. For example, a uniform aqueous dispersion composition tends to be obtained by adding the amine compound (Y) and water to a mixture of the modified copolymer (X) and the surfactant in this order while stirring and mixing. In order to uniformly dissolve or disperse the components, the components may be mixed in an organic solvent and stirred and mixed. The organic solvent may be aqueous or non-aqueous, and is not particularly limited as long as the components can be uniformly dissolved or dispersed. However, a low-boiling organic solvent that can be distilled off later is preferable.

[0149] Next, the silicone oil (Z) and water are mixed by stirring or shaking appropriately to prepare an aqueous solution containing a lubricating oil component. The order of addition of the components is not particularly limited as long as the components can be uniformly dissolved or dispersed, but for example, by stirring and mixing the silicone oil (Z)-containing emulsion and water, an aqueous solution tends to be easily obtained at room temperature. The silicone oil (Z) concentration of the aqueous solution is not particularly limited as long as the components can be uniformly dissolved or dispersed, and may be appropriately adjusted taking into account the physical properties of the silicone oil (Z), such as the viscosity, and the non-volatile content concentration, etc., of the silicone oil (Z)-containing emulsion, if used.

[0150] The aqueous dispersion composition and the aqueous solution containing the lubricating oil component are mixed by suitable stirring or shaking to emulsify the lubricating oil component in the water, thereby obtaining the present composition. The means used for mixing may be any known stirrer or shaker.

[0151] ·Method(2) First, the modified copolymer (X), the amine compound (Y), the silicone oil (Z), the surfactant, and other components as necessary are appropriately stirred and mixed to prepare an oil droplet component. During stirring and mixing, the components and the mixed liquid may be heated to 40 to 70°C as necessary. The order of addition of the components is not particularly limited as long as the components can be uniformly dissolved or dispersed. In order to uniformly dissolve or disperse the components, they may be mixed in an organic solvent and stirred and mixed. The organic solvent is not particularly limited, whether it is aqueous or non-aqueous, as long as the components can be uniformly dissolved or dispersed, but a low-boiling organic solvent that can be distilled off later is preferred. Among the components, water-soluble components (e.g., the amine compound (Y) and the surfactant) may be added during emulsification, which will be described later.

[0152] Next, the obtained oil droplet component is emulsified in water to obtain the present composition. Examples of the emulsification method include a method in which water and, if necessary, a water-soluble component (e.g., an amine compound (Y) or a surfactant) are added to the oil droplet component under strong stirring to cause phase inversion emulsification. Other components that are added as necessary may be added to the oil droplet component before emulsification, or may be added to the aqueous dispersion after emulsification. In addition, in the present composition, when the organic solvent optionally blended during stirring and mixing is not necessary, the organic solvent may be distilled off from the aqueous dispersion after emulsification. The means used for the phase inversion may be any known means, but preferred examples include a kneader, a Banbury mixer, and a multi-screw extruder.

[0153] The present composition is desirably prepared so that the solid content thereof is usually 1 to 50% by mass, preferably 3 to 40% by mass.

[0154] This composition can be suitably used as a die-casting release agent (lubricant). When used as a die-casting release agent, this composition can reduce the number of times that lubricant-derived heat-deteriorated products need to be removed from metal dies and around machines, so that it is expected to shorten the die-casting cycle time, i.e., improve work efficiency. EXAMPLES

[0155] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the above. In the examples and comparative examples, the physical properties were measured or evaluated by the following methods.

[0156] [Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] The values ​​were determined using the following high-speed GPC measuring device. Measuring device: Tosoh HLC8320GPC Mobile phase: THF (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., stabilizer-free, liquid chromatography grade) Column: 2 Tosoh TSKgel Super MultiporeHZ-M were connected in series. Sample concentration: 5mg / mL Mobile phase flow rate: 0.35mL / min Measurement temperature: 40℃ Standard sample for calibration curve: Tosoh PStQuick MP-M

[0157] [Kinematic viscosity at 100℃] Based on JIS K 2283, the measurement was carried out using a fully automatic viscometer CAV-4 manufactured by Canon.

[0158] [Ethylene content] The ECP500 nuclear magnetic resonance spectrometer manufactured by JEOL Ltd. was used. The solvent was a mixed solvent of orthodichlorobenzene / heavy benzene (80 / 20% by volume), the sample concentration was 55 mg / 0.6 mL, the measurement temperature was 120°C, and the observation nuclei were 13 The measurements were performed using a C (125 MHz) with a sequence of single pulse proton decoupling, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 s, an accumulation count of 10,000 or more, and a chemical shift reference value of 27.50 ppm. 13 The values ​​were calculated from C-NMR spectra based on the reports of "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170), GJ Ray (Macromolecules, 10, 773 (1977)), JC Randal (Macromolecules, 15, 353 (1982)), and K. Kimura (Polymer, 25, 4418 (1984)).

[0159] [Melting Point] Measurement was performed using a Seiko Instruments X-DSC-7000. Approximately 8 mg of sample was placed in a simple, airtight aluminum sample pan and placed in a DSC cell. The DSC cell was heated from room temperature to 150°C at 10°C / min under a nitrogen atmosphere, then held at 150°C for 5 minutes, then cooled at 10°C / min, and the DSC cell was cooled to -100°C (cooling down process). Next, the cell was held at -100°C for 5 minutes, then heated to 150°C at 10°C / min, and the temperature at which the enthalpy curve obtained during the heating process showed a maximum value was taken as the melting point, and the sum of the endothermic heats associated with melting was taken as the heat of fusion. If no peak was observed or the value of the heat of fusion was 1 J / g or less, the melting point (Tm) was considered not to be observed. The melting point and heat of fusion were determined based on JIS K 7121.

[0160] [Emulsion stability evaluation] The obtained water-based lubricant composition was stored at room temperature for one week, and then the appearance was visually evaluated. The evaluation criteria are as follows. When the water-based dispersion is used as a water-based lubricant for aluminum die casting, etc., the higher the emulsion stability, the more preferable it is in terms of quality stability. ○: No turbidity, precipitates or sedimentation ×: One or more of the following occurs: turbidity, precipitate, or sedimentation

[0161] [Evaluation of adhesion to metal] 20 g of the obtained water-based lubricant composition was weighed out and placed in a stainless steel (SUS304) petri dish, and a heat resistance test was carried out at 250°C for 2 hours, after which the condition was evaluated by visual inspection and touch. The evaluation criteria are as follows. When the water-based dispersion is used as a water-based lubricant for aluminum die casting or the like, it is preferable that the amount of adhesion to the metal is smaller, since this provides better dimensional stability during molding and reduces the frequency of cleaning the lubricant that has adhered to the die. ○: No adhesion to metal ×: Adhesion to metal

[0162] [Evaluation of survival rate] 20 g of the obtained water-based lubricant composition was weighed out and placed in a stainless steel (SUS304) petri dish, and a heat resistance test was carried out at 250° C. for 2 hours. The residual rate was calculated from the weight after the test, and evaluation was carried out. In addition, when the aqueous dispersion is used as an aqueous lubricant for aluminum die casting, etc., the higher the residual ratio, the better, since the lubricity can be maintained and the adhesion to the mold can be prevented. If the residual ratio is less than 5.0%, the lubricity is insufficient and the adhesion to the mold occurs, and if the residual ratio is 5.0% or more, the sufficient lubricity can be maintained and the adhesion to the mold can be prevented.

[0163] The ethylene-α-olefin copolymers used in the examples and comparative examples were prepared according to the following production examples (production Method).

[0164] [Production Example 1-1] [Ethylene-α-olefin copolymer (A-1)] 760 mL of heptane and 120 g of propylene were charged into a 2 L stainless steel autoclave that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 150°C. Then, 0.85 MPa of hydrogen and 0.19 MPa of ethylene were fed to adjust the total pressure to 3 MPaG. Next, 0.4 mmol of triisobutylaluminum, [methylphenylmethylene (η 5-cyclopentadienyl)(η 5 0.0002mmol of N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate was added with nitrogen and polymerization was started by changing the stirring speed to 400rpm. Then, polymerization was carried out at 150℃ for 5 minutes while maintaining the total pressure at 3MPaG by continuously supplying only ethylene. After stopping the polymerization by adding a small amount of ethanol to the system, unreacted ethylene, propylene, and hydrogen were purged. The obtained polymerization solution was washed three times with 1000mL of 0.2mol / L hydrochloric acid and then three times with 1000mL of distilled water, dried over magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude ethylene-propylene copolymer.

[0165] In a 1L stainless steel autoclave, 100mL of a hexane solution of 0.5% Pd / alumina catalyst and 500mL of a 30% hexane solution of the crude ethylene-α-olefin copolymer were added, the autoclave was sealed, and the atmosphere was replaced with nitrogen. The temperature was then raised to 140°C while stirring, and the system was replaced with hydrogen. The pressure was then raised to 1.5MPa with hydrogen, and the hydrogenation reaction was carried out for 15 minutes. The reaction solution was filtered to remove the hydrogenation catalyst, and the solvent was distilled off under reduced pressure. The mixture was dried at 80°C under reduced pressure for 24 hours to obtain ethylene-propylene copolymer, ethylene-α-olefin copolymer (A-1).

[0166] The resulting ethylene-α-olefin copolymer (A-1) had a weight average molecular weight (Mw): 5100, a molecular weight distribution (Mw / Mn): 1.7, and a kinematic viscosity at 100°C: 150 mm 2 / s, ethylene content: 48 mol %, and no melting point was observed.

[0167] [Production Example 1-2] [Ethylene-α-olefin copolymer (A-2)] 760 mL of heptane and 120 g of propylene were charged into a 2 L stainless steel autoclave that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 150°C. Then, 0.85 MPa of hydrogen and 0.19 MPa of ethylene were fed to adjust the total pressure to 3 MPaG. Next, 0.4 mmol of triisobutylaluminum, [diphenylmethylene (η 5 -3-n-butylcyclopentadienyl)(η 5 0.0002mmol of N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate was added with nitrogen and polymerization was started by changing the stirring speed to 400rpm. Then, polymerization was carried out at 150℃ for 5 minutes while maintaining the total pressure at 3MPaG by continuously supplying only ethylene. After stopping the polymerization by adding a small amount of ethanol to the system, unreacted ethylene, propylene, and hydrogen were purged. The obtained polymerization solution was washed three times with 1000mL of 0.2mol / L hydrochloric acid and then three times with 1000mL of distilled water, dried over magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude ethylene-propylene copolymer.

[0168] In a 1L stainless steel autoclave, 100mL of a hexane solution of 0.5% Pd / alumina catalyst and 500mL of a 30% hexane solution of the crude ethylene-α-olefin copolymer were added, the autoclave was sealed, and the atmosphere was replaced with nitrogen. The temperature was then raised to 140°C while stirring, and the system was replaced with hydrogen. The pressure was then raised to 1.5MPa with hydrogen and the hydrogenation reaction was carried out for 15 minutes. The reaction solution was filtered to remove the hydrogenation catalyst, and the solvent was distilled off under reduced pressure. The mixture was dried at 80°C under reduced pressure for 24 hours to obtain ethylene-propylene copolymer, ethylene-α-olefin copolymer (A-2).

[0169] The resulting ethylene-α-olefin copolymer (A-2) had a weight average molecular weight (Mw): 4,800, a molecular weight distribution (Mw / Mn): 1.7, and a kinematic viscosity at 100°C: 150 mm 2 / s, ethylene content: 49 mol %, and no melting point was observed.

[0170] The graft-modified copolymers used in the examples and comparative examples were obtained by the following production examples (production methods). .

[0171] [Production Example 2-1] [Graft Modified Copolymer (X-1)] In a 500 ml glass reactor equipped with a stirrer equipped with a nitrogen inlet tube, a water-cooled condenser and a thermometer, 120 g of the copolymer (A-1) obtained in Production Example 1-1, 15 g of 2-allyloxyethanol and 3 g of di-tert-butyl peroxide were charged, and nitrogen replacement was performed for 1 hour to expel dissolved oxygen. After that, the temperature in the reactor was raised to 150°C, and the reaction was performed for 3 hours, after which the temperature in the reactor was raised to 180°C and impurities (unreacted 2-allyloxyethanol and decomposition products of di-tert-butyl peroxide) were removed under reduced pressure (10 Torr). By the above operations, a graft-modified copolymer (X-1) was obtained.

[0172] The graft ratio of the obtained graft-modified copolymer (X-1) was 7% by mass. The graft ratio was determined by quantifying the hydroxyl content in the sample by measuring the hydroxyl value by the acetylation method, and the content of the hydroxyl-containing graft monomer component was calculated from the value. In addition, the weight average molecular weight (Mw): 4800, molecular weight distribution (Mw / Mn): 1.7, 100°C kinematic viscosity: 190mm 2 / s and no melting point was observed.

[0173] [Production Example 2-2] [Graft Modified Copolymer (X-2)] Except for changing the copolymer (A-1) obtained in Production Example 1-1 to the copolymer (A-2) obtained in Production Example 1-2, the reaction was carried out in the same manner as in Production Example 2-1, and impurities were removed in the same manner. The above-mentioned operations gave a graft-modified copolymer (X-2).

[0174] The graft ratio of the obtained graft-modified copolymer (X-2) was 6% by mass. The graft ratio was determined by quantifying the hydroxyl content in the sample by measuring the hydroxyl value by the acetylation method, and calculating the content of the hydroxyl-containing graft monomer component from the value. In addition, the weight average molecular weight (Mw): 4600, the molecular weight distribution (Mw / Mn): 1.8, the kinetic viscosity at 100°C: 180 mm 2 / s and no melting point was observed.

[0175] Details of each component used in the examples and comparative examples are as follows. [Amine compound (Y)] As the amine compound (Y-1), AMP-90 (2-amino-2-methyl-1-propanol, manufactured by Angus Chemical Company, AMP-90 is a registered trademark of the company) was used. As the amine compound (Y-2), 2-(2-aminoethoxy)ethanol (DGA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used.

[0176] [Silicone oil (Z)-containing emulsion] Silicone oil (Z)-containing emulsion (eZ-1) is an alkyl aralkyl modified silicone oil emulsion DOWSI TM SM 7001 Ex Emulsion (Dow Toray Industries, Inc., non-volatile content 54%) was used.

[0177] [Surfactants] As the surfactant (C-1), Emulgen 1108 (Kao Corporation, polyoxyethylene alkyl ether) was used.

[0178] [Examples 1 to 4, 9, Comparative Examples 1 to 2] Either of the modified copolymers (X-1) to (X-2) or the copolymers (A-1) to (A-2) and the surfactant (C-1) were mixed in the amounts shown in Table 1, and the mixture was heated to 70°C while stirring at a stirring speed of 50 rpm. Next, a mixed solution of either of the amine compounds (Y-1) to (Y-2) and pure water was added, and the mixture was stirred for 30 minutes at a stirring speed of 150 rpm. Then, 70°C hot water was added, and the mixture was stirred for 60 minutes at a stirring speed of 250 rpm, and then cooled for 30 minutes to obtain an aqueous dispersion composition. The obtained aqueous dispersion composition was mixed with an aqueous solution of a silicone oil (Z)-containing emulsion (eZ-1) and pure water in a ratio of 38:62, and stirred and mixed at room temperature for 30 minutes at a stirring speed of 250 rpm to obtain a water-based lubricant composition. The obtained water-based lubricant composition was evaluated for emulsion stability, adhesion to metal, and residual rate according to the above-mentioned method. The mass ratios and evaluation results of the obtained water-based lubricant compositions are shown in Table 1.

[0179] [Examples 5 to 8] Any of the modified copolymers (X-1) to (X-2) was mixed in the amounts shown in Table 1, and the mixture was heated to 70°C while stirring at a stirring speed of 50 rpm. Next, a mixed solution of any of the amine compounds (Y-1) to (Y-2) and pure water was added, and the mixture was stirred for 30 minutes at a stirring speed of 150 rpm. Then, 70°C hot water was added, and the mixture was stirred for 60 minutes at a stirring speed of 250 rpm, and then cooled for 30 minutes to obtain an aqueous dispersion composition. The obtained aqueous dispersion composition was mixed with an aqueous solution of silicone oil (Z)-containing emulsion (eZ-1) and pure water in a ratio of 38:62, and stirred and mixed at a stirring speed of 250 rpm at room temperature for 30 minutes to obtain a water-based lubricant composition. The obtained water-based lubricant composition was evaluated for emulsion stability, adhesion to metal, and residual rate according to the above-mentioned method. The mass ratio and evaluation results of the obtained water-based lubricant composition are shown in Table 1.

[0180] [Comparative Example 3] The modified copolymer (X-1) and the surfactant (C-1) were mixed in the amounts shown in Table 1, and the mixture was heated to 70°C while stirring at a stirring speed of 50 rpm. Next, 70°C hot water was added, and the mixture was stirred for 60 minutes at a stirring speed of 250 rpm, and then cooled for 30 minutes to obtain an aqueous dispersion composition. The aqueous dispersion composition obtained was mixed with an aqueous solution of silicone oil (Z)-containing emulsion (eZ-1) and pure water in a ratio of 38:62, and stirred and mixed at room temperature for 30 minutes at a stirring speed of 250 rpm to obtain a water-based lubricant composition. The mass ratio and evaluation results of the obtained water-based lubricant composition are shown in Table 1.

[0181] [Comparative Example 4] The surfactant (C-1) was mixed in the amount shown in Table 1, and the temperature was raised to 70°C while stirring at a stirring speed of 50 rpm. Next, 70°C hot water was added, and the mixture was stirred for 60 minutes at a stirring speed of 250 rpm, and then cooled for 30 minutes to obtain an aqueous dispersion composition. The obtained aqueous dispersion composition was mixed with an aqueous solution of silicone oil (Z)-containing emulsion (eZ-1) and pure water in a ratio of 38:62, and stirred and mixed at a stirring speed of 250 rpm at room temperature for 30 minutes to obtain a water-based lubricant composition. The mass ratio and evaluation results of the obtained water-based lubricant composition are shown in Table 1.

[0182] [Comparative Examples 5 to 6] Any one of the amine compounds (Y-1) to (Y-2) and pure water were mixed in the amounts shown in Table 1, and the mixture was heated to 70°C while stirring at a stirring speed of 250 rpm, and then stirred for 60 minutes. After that, the mixture was allowed to cool for 30 minutes to obtain an aqueous dispersion composition. The obtained aqueous dispersion composition was stirred and mixed with an aqueous solution of silicone oil (Z)-containing emulsion (eZ-1) and pure water in a ratio of 38:62 at a stirring speed of 250 rpm at room temperature for 30 minutes to obtain a water-based lubricant composition. The mass ratio and evaluation results of the obtained water-based lubricant composition are shown in Table 1.

[0183] [Comparative Examples 7 to 8] The surfactant (C-1) was mixed in the amount shown in Table 1, and the temperature was raised to 70°C while stirring at a stirring speed of 50 rpm. Next, a mixed solution of any one of the amine compounds (Y-1) to (Y-2) and pure water was added, and the mixture was stirred for 30 minutes at a stirring speed of 150 rpm. Then, 70°C hot water was added, and the mixture was stirred for 60 minutes at a stirring speed of 250 rpm, and then cooled for 30 minutes to obtain an aqueous dispersion composition. The obtained aqueous dispersion composition was mixed with an aqueous solution of silicone oil (Z)-containing emulsion (eZ-1) and pure water in a ratio of 38:62, and stirred and mixed at room temperature for 30 minutes at a stirring speed of 250 rpm to obtain a water-based lubricant composition. The mass ratio and evaluation results of the obtained water-based lubricant composition are shown in Table 1.

[0184] [Comparative Example 9] The silicone oil (Z)-containing emulsion (eZ-1) and pure water were mixed in a ratio of 38:62, and stirred and mixed at room temperature for 30 minutes at a stirring speed of 250 rpm to obtain a water-based lubricant composition. The mass ratio and evaluation results of the obtained water-based lubricant composition are shown in Table 1.

[0185] [Table 1]

Claims

1. A graft-modified ethylene / α-olefin copolymer (X) having a main chain portion derived from an ethylene / α-olefin copolymer (A) that satisfies the following requirements (a-1) to (a-3) and a graft portion derived from an unsaturated monomer (B) that satisfies the following requirement (b-1); an amine compound (Y); At least one silicone oil (Z) selected from the group consisting of alkyl-modified silicone oils and alkylaralkyl-modified silicone oils; Water and A water-based lubricant composition comprising: (a-1) the content of ethylene units is 30 to 70 mol%; (a-2) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (a-3) No melting point (Tm) is observed as measured by differential scanning calorimetry (DSC); (b-1) The unsaturated monomer (B) is at least one unsaturated monomer selected from the group consisting of ethylenically unsaturated monomers having a hydroxyl group.

2. The water-based lubricant composition according to claim 1, wherein the ethylene / α-olefin copolymer (A) satisfies the following requirements (a-4) and (a-5): (a-4) Kinematic viscosity at 100 ° C. is 10 to 5,000 mm 2 / s; (a-5) The molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less.

3. The water-based lubricant composition according to claim 1 , wherein the unsaturated monomer (B) is an unsaturated alcohol.

4. The water-based lubricant composition according to claim 1, wherein the graft-modified ethylene / α-olefin copolymer (X) satisfies the following requirements (x-1) to (x-5): (x-1) the proportion of the graft portion is 0.1% by mass or more and less than 70% by mass (wherein the total amount of the main chain portion and the graft portion is 100% by mass); (x-2) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (x-3) No melting point (Tm) is observed as measured by differential scanning calorimetry (DSC); (x-4) Kinematic viscosity at 100 ° C. is 10 to 5,000 mm 2 / s; (x-5) The molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less.

5. 2. The water-based lubricant composition according to claim 1, wherein the content of the graft-modified ethylene / α-olefin copolymer (X) is 0.1 to 10 mass % relative to 100 mass % of the water-based lubricant composition.

6. The water-based lubricant composition according to claim 1, wherein the amine compound (Y) satisfies the following requirements (y-1) and (y-2): (y-1) the molecular weight is 1,000 or less; (y-2) has one or more hydroxyl groups in the molecule.

7. 2. The water-based lubricant composition according to claim 1, wherein the content of the amine compound (Y) is 10 to 60 parts by mass based on 100 parts by mass of the graft-modified ethylene / α-olefin copolymer (X).

8. 2. The water-based lubricant composition according to claim 1, wherein the content of the silicone oil (Z) is 10 to 50 mass % relative to 100 mass % of the water-based lubricant composition.

9. The water-based lubricant composition according to claim 1 , further comprising a surfactant.

10. The water-based lubricant composition according to claim 9, wherein the surfactant is a nonionic surfactant.

Citation Information

Patent Citations

  • Water soluble parting agent for die casting

    JP1986103642A

  • Lubricant composition for metal die casting

    JP1994240286A

  • Water-based lubricating oil composition for plastically working non-ferrous metal

    JP2003253290A