Zinc plated steel sheet having excellent fatigue strength of electrical resistance spot welds, and manufacturing method thereof

By controlling the concentration profiles of oxygen, silicon, and manganese in the galvanized steel sheet's surface layer, the manufacturing process addresses LME and microcracking issues, enhancing fatigue strength and weld integrity in high-strength galvanized steel sheets.

JP2024138314AActive Publication Date: 2024-10-08CLEANSOLUTION CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024104095
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-03
Filing Date
2024-06-27
Publication Date
2024-10-08
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

High-strength galvanized steel sheets experience liquid metal embrittlement (LME) and reduced fatigue strength in electrical resistance spot welds due to microcracks and zinc penetration during welding, which compromises the integrity of the welds.

Method used

A galvanized steel sheet with controlled concentration profiles of oxygen, silicon, and manganese, forming a soft layer near the surface to absorb tensile stress and prevent cracking, achieved through specific manufacturing processes including hot rolling, pickling, cold rolling, and hot-dip galvanizing, with controlled depth differences and concentrations to suppress LME.

Benefits of technology

The controlled concentration profiles enhance the fatigue strength and weldability of the galvanized steel sheets by reducing microcracks and preventing LME, ensuring high tensile strength and improved spot weld integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138314000001_ABST
    Figure 2024138314000001_ABST
Patent Text Reader

Abstract

To provide a zinc plated steel sheet having excellent fatigue strength of electrical resistance spot welds, and a manufacturing method thereof.SOLUTION: According to an aspect of the present disclosure, a zinc plated steel sheet includes a base steel sheet and a zinc-based plating layer formed on a surface of the base steel sheet. Concentration profiles of oxygen and one or two of silicon and manganese measured in a depth direction from the surface of the base steel sheet have forms in which the maximum points appear in the depth direction from the surface. An absolute value of a difference between a depth at which the maximum point of the concentration profile of oxygen is formed and a depth at which the maximum point of the concentration profile of one of silicon and manganese is formed is 0.5 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a galvanized steel sheet having excellent fatigue strength at electric resistance spot welds, and a method for manufacturing the same. This relates to a method. [Background technology]

[0002] Due to issues such as environmental pollution, regulations on automobile exhaust gases and fuel efficiency are becoming stricter day by day. As a result, there is a strong demand for lighter automotive steel sheets to reduce fuel consumption. Accordingly, various types of high-strength steel plates with high strength per unit thickness have been developed. It has been released.

[0003] High-strength steel generally means steel with a strength of 490 MPa or more, but this does not necessarily mean The present invention is not limited to the above, and includes transformation induced plasticity. ced Plasticity (TRIP) steel, Twin Induce plasticity (TRIP) steel d Plasticity (TWIP) steel, Dual Phase (DP) steel , and complex phase (CP) steel may also fall into this category.

[0004] On the other hand, automotive steel is in the form of plated steel sheets, whose surfaces are plated to ensure corrosion resistance. Among them, zinc-coated steel sheets (GI steel sheets) or alloyed zinc-coated steel sheets ( GA has high corrosion resistance due to the sacrificial corrosion protection properties of zinc, and is therefore widely used as an automotive material. It is often used.

[0005] By the way, when the surface of high-strength steel plate is plated with zinc, it is said that spot weldability becomes brittle. In the case of high strength steel, the tensile strength and yield strength are both high, The tensile stress generated during welding is difficult to eliminate through plastic deformation, resulting in microcracks on the surface. When high-strength galvanized steel sheets are welded, the zinc, which has a low melting point, melts into the steel sheet. This can penetrate into microcracks in the metal, resulting in liquid metal embrittlement. This phenomenon, called "LME" (Liquid Metal Embrittlement) occurs, causing the steel plate to break. Not only will the fatigue strength of the steel plate deteriorate, but the fatigue strength may also decrease. This is a major obstacle to achieving high strength. Summary of the Invention [Problem to be solved by the invention]

[0006] According to one aspect of the present invention, there is provided a galvanized steel sheet having excellent fatigue strength at electric resistance spot welds. and a method for producing the same are provided.

[0007] The object of the present invention is not limited to the above. Those having knowledge of the present invention will be able to understand the further object of the present invention from the overall content of the specification of the present invention. There is no difficulty in understanding it. [Means for solving the problem]

[0008] The present invention provides a galvanized steel sheet comprising a base steel sheet and a galvanizing agent formed on the surface of the base steel sheet. A zinc-coated steel sheet including a zinc-based coating layer, The concentration profile of one or two of the oxygen, silicon, and manganese determined on the surface The oxygen concentration profile has a maximum point in the depth direction. The depth at which the concentration profile of one of the silicon and manganese is formed. The difference in depth between the galvanized steel sheets may be 0.5 μm or less in absolute value.

[0009] In addition, a method for producing a galvanized steel sheet according to one aspect of the present invention comprises: 0°C, hot rolling the steel slab to obtain a steel plate, a step of obtaining a hot-rolled steel sheet by coiling the hot-rolled steel sheet at a temperature of 90 to 750°C; The hot-rolled steel sheet is then cold-rolled at a rolling reduction of 35 to 60%. In the step of obtaining a cold-rolled steel sheet, the cold-rolled steel sheet is heated to 650 to 900°C and cooled to 30°C in an atmosphere with a dew point of -10 to 30°C. and hot-dip galvanizing the annealed cold-rolled steel sheet. good. Effect of the Invention

[0010] As described above, the present invention is directed to the formation of a coating layer by removing O, Si formed inside the base steel sheet. By appropriately controlling the Mn concentration profile, the surface of the base steel sheet, i.e., the plating This allows the base steel sheet to be softened near the interface between the layer and the base steel sheet. By doing so, the tensile stress generated during spot welding is eliminated by the plastic deformation of the soft layer, The number and length of cracks are reduced, resulting in high strength and excellent fatigue strength of spot welds. Galvanized steel sheets can be produced. [Brief description of the drawings]

[0011] [Figure 1] 1 is a graph showing GDOES profiles of oxygen (O) and silicon (Si) or manganese (Mn) for measuring maximum depth difference according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below with reference to several embodiments.

[0013] In the present invention, the galvanized steel sheet includes not only galvanized steel sheet (GI steel sheet) but also alloy steel sheet. Not only galvanized steel sheets (GA), but also zinc-based coating layers that mainly contain zinc are formed. It is important to note that this is a concept that includes all types of plated steel sheets. This means that the zinc content of the plating layer is the highest among all the elements. In lead-plated steel sheets, the proportion of iron is sometimes higher than that of zinc, and the remaining components other than iron are Steel sheets with the highest percentage of lead are within the scope of the present invention.

[0014] The inventors of the present invention have discovered that liquid metal embrittlement (LME) occurs during welding on the surface of the steel plate. The cause of this is microcracks that may lead to fatigue failure. Focusing on this, we have been researching ways to suppress microcracks on the surface. The present invention was arrived at by finding that it is necessary to soften the surface.

[0015] Generally, in the case of high strength steel, in order to secure the hardening ability and austenite stability of the steel, Therefore, it contains large amounts of elements such as carbon (C), manganese (Mn), and silicon (Si). However, these elements serve to increase the susceptibility of the steel to cracking. Steels containing large amounts of these elements tend to easily develop microcracks, ultimately resulting in failure during welding. This can cause liquid metal embrittlement.

[0016] According to the research results of the present inventors, oxygen (O) formed in the depth direction from the surface of the base steel sheet Concentration profile of silicon (Si) and / or manganese (Mn) When the relationship between the temperature and the temperature distribution is properly controlled, the resistance of spot welds to LME increases, and This can increase the fatigue strength of spot welds.

[0017] That is, as shown in FIG. 1, the depth at which the maximum point appears in the oxygen (O) concentration profile. (meaning the depth from the surface of the base steel sheet) and silicon (Si) and / or manganese ( The difference in depth at which the maximum point appears in the Mn concentration profile must be controlled within 0.5 μm. There is.

[0018] Thus, a maximum point appears in the concentration profile of oxygen and silicon and / or manganese. When the depth is matched, silicon and / or manganese are in the form of oxides inside the base steel sheet. This means that the surface silicon and / or manganese are fixed at a certain depth. The concentration of can be reduced.

[0019] Normally, silicon and / or manganese diffuse to the surface during the annealing process, forming a surface oxide. Not only that, but the activity of silicon and / or manganese on the surface Thus, the activity of surface silicon and / or manganese (proportional to their content) The higher the concentration, the higher the concentration of these elements. This means that the oxygen activity of the surface is reduced, making it more difficult to remove the carbon that is present on the surface. Thus, the surface silicon and manganese content increases and decarburization does not occur. increases the susceptibility of the surface to cracks, making them more susceptible to crack initiation, which More LMEs are likely.

[0020] By the way, in the present invention, the concentration profile of oxygen and silicon and / or manganese is Controlling the relationship not only reduces the concentration of silicon and / or manganese at the surface, This allows smooth decarburization and allows a soft layer to form on the surface. In this case, even if tensile stress acts during welding, the stress is absorbed by the occurrence of plastic deformation. This makes it possible to effectively suppress the occurrence of cracks.

[0021] Therefore, the present invention is directed to a depth at which a maximum point in the concentration profile of oxygen (O) occurs (hereinafter referred to as a depth at which a maximum point in the concentration profile of oxygen (O) occurs). (also simply called "maximum depth") and the concentration of silicon (Si) and / or manganese (Mn) By controlling the difference in depth at which the maximum point of the roughness profile occurs to within 0.5 μm, In one embodiment of the present invention, the difference in depth is 2 It can be understood that the absolute value of the difference between the depths at which the maxima of two profiles are formed. According to one embodiment of the invention, the difference in depth can be limited to within 0.3 μm. In one embodiment, the value may be limited to within 0.2 μm, or within 0.1 μm. Since the maximum points may be formed at the same position, the lower limit of the difference in the values ​​is not particularly set, and it is 0 μm. In addition, one or more maximum points may be formed in the concentration profile for each element. However, the maximum point in the present invention means the maximum point closest to the surface.

[0022] In one embodiment of the present invention, the oxygen maximum depth is In this way, when controlling the maximum depth of each element, can more effectively inhibit silicon and / or manganese from diffusing to the surface. can.

[0023] According to one embodiment of the present invention, the oxygen maximum depth and at least one of silicon and manganese are When the difference between the maximum depths of the two elements satisfies the above-mentioned range, the advantageous effects of the present invention can be obtained. However, in order to more reliably obtain the effects of the present invention, the oxygen maximum depth and the silicon and manganese maximum depths may fall within the above ranges.

[0024] The concentration profiles of oxygen, silicon and manganese were determined using various methods known in the art. However, in one embodiment of the present invention, GDOES(Glow Discharge Optical Emission Sp The profile measured from the surface to the inside of the base steel sheet using a CT scanner was used. It can be used.

[0025] In one embodiment of the present invention, in order to more reliably form a soft layer, the oxygen concentration at the maximum point is It is even more advantageous for the oxygen concentration to be 0.3% by weight or more. The silicon and manganese present inside the plate are firmly fixed and prevented from migrating to the surface. According to one embodiment of the present invention, the oxygen concentration at the maximum point is It may be 0.4% by weight or more, and in some cases may be 0.5% by weight or more. There is no need to set an upper limit for the oxygen concentration at the maximum point. However, the upper limit for the oxygen concentration at the maximum point is usually 1 It may be defined as 0.0% or less by weight, 0.8% or less by weight, or 0.7% or less by weight.

[0026] Therefore, in one embodiment of the present invention, the overall composition of the steel is a high alloy steel for high strength. However, in the surface area where cracks occur, a soft layer is formed. At the same time, by controlling the distribution of the internal oxide, resistance to LME and The fatigue strength of the welded joint can be improved.

[0027] In the present invention, the maximum point and the concentration at the maximum point of each element can be determined as follows. First, the GDOES profile is obtained as shown in Figure 1. The S profile can be obtained at a depth interval of 10 to 30 nm. In one embodiment, a depth interval of 20 nm was used. The initial data obtained As shown in FIG. 1, the shape has a maximum point, but the exact position of the maximum point cannot be determined. In this case, the oxygen concentration at each point is measured at that point and at two points before and after. When the five-point average value of the data points is used, the shape is relatively smooth. can be done.

[0028] From the oxygen concentration profile obtained by this process, the maximum point and the corresponding The oxygen concentration at the minimum point can be calculated by the smoothed oxygen concentration profile. The maximum point is the point that shows the highest value after the minimum point. In one embodiment of the present invention, the maximum point of the oxygen concentration profile is It may appear at a depth of 4 μm from the surface. If the maximum point appears too close to the surface However, since it may be difficult for a soft layer to form on the surface, the above maximum point is located at a certain depth or more from the surface. Conversely, if the local maximum is very far away from the surface, However, the depletion effect of silicon, manganese, etc. may not be sufficient, so Depending on the morphology, the above maximum point may appear at a depth of up to 15 μm from the surface of the steel sheet. According to another embodiment of the present invention, the maximum point of the oxygen concentration profile is 10 μm from the surface. It may appear at a depth of within 10 μm from the surface, and more preferably at a depth of within 10 μm from the surface.

[0029] In one embodiment of the present invention, the GDOES oxygen concentration profile in the depth direction is The value measured at the center of the plate width can be used. The plate often has higher values ​​at the edges in the width direction compared to the center in the width direction, In order to improve pot weldability more effectively, the profile measured at the edge is used. In this case, the edge portion means both ends of the steel plate. If there is a problem with the soundness of the test piece, such as contamination, the test piece may be removed within 1 mm of the edge in the width direction. It may also mean a point on the side.

[0030] The steel plate targeted by this invention is a high-strength steel plate with a strength of 490 MPa or more. However, the present invention is not limited to the above. The weight ratio is C: 0.05-1.5%, Si: 2.0% or less, Mn: 1.0-30% , S-Al (acid-soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or less , B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less It may have a composition including Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less. The remaining components are iron and other impurities not listed above. The inclusion of elements that may be contained in steel up to a total content of 1.0% or less is not excluded. In the present invention, the content of each component element is expressed on a weight basis unless otherwise specified. The above composition refers to the bulk composition of the steel plate, i.e., the composition at 1 / 4 of the steel plate thickness. (The same applies below).

[0031] In some embodiments of the present invention, the high strength steel plate is a TRIP steel or the like. These steels can have the following compositions in more detail:

[0032] Steel composition 1: C: 0.05-0.30% (preferably 0.10-0.25%), Si: 0 0.5-2.5% (preferably 1.0-1.8%), Mn: 1.5-4.0% (preferably 2.0~3.0%), S-Al: 1.0% or less (preferably 0.05% or less), Cr: 2 0.0% or less (preferably 1.0% or less), Mo: 0.2% or less (preferably 0.1% or less) ), B: 0.005% or less (preferably 0.004% or less), Nb: 0.1% or less (preferably or 0.05% or less), Ti: 0.1% or less (preferably 0.001 to 0.05%), Sb+Sn+Bi: 0.05% or less, N: 0.01% or less, balance Fe and unavoidable impurities In some cases, elements not listed above that may be contained in the steel may be included in the total amount of 1. It may further include a range of up to 0%.

[0033] Steel composition 2: C: 0.05-0.30% (preferably 0.10-0.2%), Si: 0. 5% or less (preferably 0.3% or less), Mn: 4.0 to 10.0% (preferably 5.0 to 9.0%), S-Al: 0.05% or less (preferably 0.001 to 0.04%), Cr: 2.0% or less (preferably 1.0% or less), Mo: 0.5% or less (preferably 0.1 to 0 .35%), B: 0.005% or less (preferably 0.004% or less), Nb: 0.1% or less below (preferably 0.05% or less), Ti: 0.15% or less (preferably 0.001 to 0. 1%), Sb+Sn+Bi: 0.05% or less, N: 0.01% or less, balance Fe and unavoidable Impurities may be included. In some cases, elements that may be included in the steel but are not listed above may be included. It may further include up to a total range of 1.0% or less.

[0034] In addition, when the lower limit of the content of each of the above-mentioned component elements is not specified, these may be arbitrarily selected. This means that it may be regarded as an optional element and its content may be 0%.

[0035] According to one embodiment of the present invention, the surface of the steel sheet has one or more plating layers. The above plating layer is GI (Galvanized) or GA (Galva-an In the present invention, as described above, The difference between the oxygen maximum depth and the silicon and / or manganese maximum depth was appropriately controlled. Therefore, even if a zinc-based plating layer is formed on the surface of the steel sheet, the liquid phase metal generated during spot welding This can reduce the problem of embrittlement (LME).

[0036] According to one embodiment of the present invention, when the zinc-based plating layer is a GA layer, the degree of alloying ( The Fe content in the coating layer is limited to 8 to 13% by weight, preferably 10 to 12% by weight. If the alloying degree is insufficient, the zinc in the zinc-based coating layer will break down into microcracks. There is still a possibility that the liquid metal may penetrate the rack and cause liquid metal embrittlement problems, and conversely, alloying If the strength is too high, problems such as powdering may occur.

[0037] The coating weight of the zinc-based coating layer is 30 to 70 g / m 2It may be. If the coating weight is too low, it is difficult to obtain sufficient corrosion resistance. If the temperature is too high, problems such as increased manufacturing costs and liquid phase metal embrittlement may occur. The more preferable range of the coating weight is 40 to 60 g / m 2 And The plating weight refers to the amount of plating layer that is attached to the final product. When the layer is a GA layer, the coating weight increases due to alloying. The weight of the alloy may be slightly reduced. This is not necessarily limited to the above, as it depends on the degree of alloying. Although it is not a given, the coating weight before alloying (i.e., the amount of coating that is deposited from the plating bath) is , and may be a value reduced by about 10% therefrom.

[0038] Hereinafter, an embodiment of the present invention will be described. However, the steel plate of the present invention is The steel sheet according to the present invention does not necessarily have to be manufactured according to the following embodiment. It should be noted that this is a preferred method for producing

[0039] First, a steel slab having the above composition is prepared, and then hot-rolled and coiled. The conditions for hot rolling and the like are not particularly limited, but in the present invention, In one embodiment, the slab heating temperature and coiling temperature can be limited as follows:

[0040] Slab heating: 950~1350℃ In order to fully dissolve the solid solution elements and reduce rolling resistance, the slab is heated at a temperature of 950°C or higher. In the present invention, since a large amount of alloying elements may be included, The lab heating temperature is 1000° C. or higher, preferably 1100° C. or higher, and more preferably 1 150℃ or higher. However, if the slab heating temperature is too high, it may cause problems such as oxidation of the solid solution elements. Problems may occur, the austenite grain size may become coarse, and the Therefore, the upper limit of the heating temperature is 1,350°C, preferably The heating temperature can be set to 1,300°C or less, and more preferably 1,280°C or less.

[0041] Winding temperature: 590 to 750°C The hot-rolled steel sheets are then wound into coils and stored. The steel sheet undergoes a slow cooling process. This process causes the oxides in the surface layer of the steel sheet to However, if the coiling temperature of the hot-rolled steel sheet is too low, these elements are removed. The coil is cooled slowly at a temperature lower than that required for the oxidation and removal of elements, so the full effect can be obtained. It's difficult.

[0042] Pickling treatment: Carried out at a strip speed of 180 to 250 mpm In order to remove hot rolling scale from the hot rolled steel sheet that has undergone the above process, it is placed in a hydrochloric acid bath. The hydrochloric acid concentration in the hydrochloric acid bath during pickling is in the range of 10 to 30 volume %. The strip speed is 180-250mpm. If the pickling speed exceeds 250mpm, The scale on the surface of the hot-rolled steel sheet may not be completely removed, and the pickling speed may be 18 If the temperature is lower than 180 mpm, the surface layer of the base steel may be corroded by hydrochloric acid. Perform at 0mpm or above.

[0043] Cold rolling: reduction rate 35-60% After pickling, cold rolling is performed. The cold rolling reduction is in the range of 35 to 60%. If the cold rolling reduction rate is less than 35%, there is no particular problem, but the driving force for recrystallization during annealing is insufficient. When the cold rolling reduction rate exceeds 60%, it may be difficult to control the microstructure. When this happens, the thickness of the internal oxide layer secured during hot rolling becomes thinner, and the depth of the internal oxide layer does not become sufficient after annealing. It is also difficult to have a maximum value of oxygen concentration.

[0044] The above-mentioned cold rolling process may be followed by a process of recrystallization annealing the steel sheet. During the annealing process, the concentration profiles of oxygen, silicon, and manganese in the surface layer of GDOES were significantly Therefore, in one embodiment of the present invention, each element of the GDOES in the surface layer is The annealing process can be controlled under conditions that appropriately control the concentration profile in the depth direction of the element. Among these, the strip threading speed and the dew point in the annealing furnace can be controlled by the following conditions.

[0045] Threading speed: 40~130mpm In order to ensure sufficient productivity, the threading speed of the above cold-rolled steel sheets must be 40 mpm or more. However, if the threading speed is too fast, it is disadvantageous from the viewpoint of securing the material. In one embodiment of the invention, the upper limit of the threading speed can be set at 130 mpm.

[0046] Dew point control in annealing furnace: Controlled from 650-900℃ to -10-30℃ In order to obtain a suitable range of decarburization rate in the surface layer, it is advantageous to control the dew point in the annealing furnace. If the dew point is too low, surface oxidation occurs instead of internal oxidation, resulting in the formation of Si and Mn on the surface. These oxides have a detrimental effect on plating. Therefore, the dew point needs to be controlled to -10°C or higher. On the other hand, if the dew point is too high, However, since there is a risk of oxidation of Fe, the dew point must be controlled to 30°C or less. Thus, the temperature for dew point control is 650℃, which is the temperature at which sufficient internal oxidation effect is achieved. In one embodiment of the present invention, the temperature and dew point in the annealing furnace are as follows: The temperature and dew point of the soaking zone can be used as the basis. However, if the temperature is too high, S The formation of surface oxides such as i prevents oxygen from diffusing into the interior of the material, and also acts as a soaking point. During heating, excessive austenite is generated, which reduces the carbon diffusion rate and causes internal oxidation. The austenite level may decrease, and the size of the austenite in the soaking zone may grow excessively, causing material softening. It also puts a strain on the annealing furnace, shortening the life of the equipment and increasing the process cost. Therefore, the temperature at which the dew point is controlled should be 900°C or less. It may be.

[0047] At this time, the dew point is measured by feeding humidified nitrogen gas (N2+H2O) containing water vapor into the annealing furnace. According to one embodiment of the present invention, the nitrogen gas is 5 to 10%. This allows the dew point to be controlled within a suitable range. Cut.

[0048] The steel sheet annealed by this process is immediately immersed in a plating bath for hot-dip galvanizing. The hot-dip galvanized steel sheet is then subjected to a process of alloying heat treatment as necessary. The preferable conditions for the plating and alloying heat treatment are as follows.

[0049] Temperature of steel sheet in the plating bath: 420~500℃ When the temperature at which the steel sheet is drawn into the plating bath is low, the wettability at the contact interface between the steel sheet and the liquid zinc is poor. Since there is not enough water, it is necessary to maintain the temperature at 420 degrees or higher. The temperature is too high. In this case, the reaction between the steel sheet and the liquid zinc occurs too much, and the Fe-Zn alloy phase, zeta( The Zetta phase occurs, the adhesion of the coating layer decreases, and the Fe element of the steel sheet in the coating bath dissolves. There is a problem that the amount of outflow becomes excessive and dross is generated in the plating bath.

[0050] Al concentration in plating bath: 0.10-0.25% The Al concentration in the plating bath should be adjusted appropriately to ensure the wettability of the plating layer and the fluidity of the plating bath. It is necessary to maintain a positive concentration. For this purpose, in the present invention, the Al concentration in the plating bath is set to 0.1 The range of 0 to 0.25% is controlled. Also, the amount of GA (alloyed molten zinc) varies depending on whether or not alloying is performed. Galvanized (Pb-plated) steel sheet and GI (Hot-dip galvanized, Galvani In one embodiment of the present invention, the dross in the plating bath is s) In order to maintain the proper level of formation and ensure the coating surface quality and performance, in the case of GA steel sheets In the case of GI steel sheets, the Al content can be 0.10 to 0.15%. The content can be controlled to 0.2 to 0.25%.

[0051] Alloying (GA) temperature: 480~560℃ Below 480℃, the amount of Fe diffusion is small and the degree of alloying is insufficient, resulting in poor plating properties. If the temperature exceeds 560℃, powdering due to excessive alloying may occur. The problem of ferrite transformation of retained austenite causes deterioration of the material. Therefore, the alloying temperature is set within the above range.

[0052] In this way, the zinc-coated steel sheet of the present invention can be obtained. In one embodiment, in order to further improve the weldability of the edge portion, the heating process of the edge portion is It may further include:

[0053] Heating the edge of hot rolled coil: 600-800℃ for 5-24 hours In one embodiment of the present invention, the oxygen depth profile of the edge GDOES shows In order to further increase the difference between the minimum and maximum values, the edge of the hot rolled coil is heated. The heating of the edges of the hot rolled coil means heating both ends of the coil in the width direction, In other words, this means heating the edge portion, which causes the edge portion to become oxidized. The coil is first heated to a temperature suitable for melting. That is, the inside of the coil is kept at a high temperature. However, the edges cool relatively quickly, which brings them to a temperature suitable for internal oxidation. Therefore, the time that the oxide is maintained at the edge is shorter than that at the center. Heating the edge does not actively remove oxidizing elements from the edge. This can be used as one way to

[0054] That is, when the edge portion is heated, the edge portion is heated in the opposite manner to the cooling after winding. First, the plate is heated, and the temperature of the edge in the width direction is maintained to match the internal oxidation. As a result, the thickness of the internal oxide layer at the edge portion increases. The heating temperature of the edge part must be 600°C or higher (based on the temperature of the steel plate edge part). However, if the temperature is too high, excessive scale will form on the edge during heating. Or, porous high-oxidation scale (hematite) is formed, resulting in poor surface condition after pickling. Therefore, the temperature of the edge portion may be 800° C. or less. The heating temperature of the edge portion is 600 to 750°C.

[0055] In addition, the GDOES of the surface layer between the edge and center in the width direction that occurred during winding In order to eliminate the non-uniformity of the difference between the minimum and maximum values ​​in the oxygen depth profile, The heating time of the edge part must be 5 hours or more. However, if the heating time of the edge part is long, If the thickness is too small, the scale will be excessively formed or the GDOES of the surface of the edge will be reduced. The difference between the minimum and maximum values ​​in the oxygen depth profile is sometimes too high. Therefore, the heating time for the edge portion may be 24 hours or less.

[0056] According to one embodiment of the present invention, the edge portion is heated by combustion heating through adjustment of the air-fuel ratio. In other words, the oxygen fraction in the atmosphere is increased by adjusting the air-fuel ratio. The higher the oxygen partial pressure, the higher the oxygen concentration in contact with the surface of the steel sheet, and the greater the decarburization. Although not necessarily limited to this, one of the advantages of the present invention is that the In the embodiment, the nitrogen atmosphere containing 1 to 2% oxygen can be controlled by adjusting the air-fuel ratio. A person having ordinary skill in the art to which the present invention pertains can easily calculate the air-fuel ratio. Since the oxygen fraction can be controlled through adjustment of EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples. However, the following examples are for illustrative purposes only. The following description is provided for illustrative purposes only and is not intended to limit the scope of the present invention. It should be noted that the scope of the present invention is not limited to the scope of the claims. This is because it is determined by the matters stated and those that can be reasonably inferred from them.

[0058] (Example) Steel slabs having the composition shown in Table 1 below (the remaining components not shown in the table are F e and inevitable impurities. Note that B and N in the table are expressed in ppm units, and the remaining components are The content is expressed in weight percent, and the content of any component not shown in the table means 0 weight percent. ) is heated to 1,230℃ and hot rolled, and then the edges of the hot rolled coil are heated. After that, the steel plate is passed through a 100mm long pickling line at a threading speed of 210mpm for 19. The steel is pickled with a 2% hydrochloric acid solution, then cold-rolled. The resulting cold-rolled steel sheet is then annealed in an annealing furnace. Immediately after plating, GA was added to a plating bath containing 0.13% Al, and GI was added to a plating bath containing 0.24% Al by weight. The steel was immersed in a zinc-based plating bath at 56°C to perform hot-dip galvanizing. If necessary, the plate is subjected to alloying (GA) heat treatment, and finally, alloyed hot-dip galvanized steel plate is obtained. Ta.

[0059] In all the examples, the drawing temperature of the steel sheet into the hot dip galvanizing bath was 475°C. Other conditions for each of the other examples are as shown in Table 2.

[0060] [Table 1]

[0061] [Table 2]

[0062] The properties of hot-dip galvanized steel sheets manufactured by the above process were measured, and the The results of observing whether or not liquid metal embrittlement (LME) occurred are shown in Table 3. Spot welding The steel plate was cut in the width direction, and the test was performed along each edge of the cut. After applying the welding current twice, hold time for one cycle is The spot welding was performed with three different layers. GA 980DP 1.4t(C 0.12wt%, Si 0.1wt%, Mn 2.2 The new materials (having a composition of 100% by weight) were layered in this order and spot welded. After welding a soft electrode 15 times to a soft material, the electrode was worn down and then used to spot weld the material. Measure the upper limit current at which the expulsion occurs. After measuring the upper limit current, Spot welding was performed eight times at currents 0.5 and 1.0 kA lower than the welding current. The cross section of the welded part is precisely machined by electric discharge machining, then epoxy mounted and polished. The crack length was measured using an optical microscope. The magnification of the optical microscope was set to 100 times. If no cracks are found at this magnification, it is assumed that liquid metal embrittlement has not occurred. If a crack was found, its length was measured using image analysis software. B-type cracks occurring at the shoulder of the pot weld are 100μm or less, and C-type cracks are 100μm or less. The rack was judged to be in good condition when not observed.

[0063] Maximum in the GDOES concentration profile of oxygen, silicon, and manganese in the surface layer The depth and concentration at that time were calculated by averaging five points of data obtained from the GDOES profile. The calculation was performed using the concentration values ​​for each depth. The concentration profile of manganese and arsenic was obtained, and the depth at which the maximum point for each element appeared in the profile was determined. After calculating the maximum depth, the smaller value of the difference between the maximum depths of oxygen, silicon, and manganese was used as the depth difference. It was decided.

[0064] The tensile strength was measured by preparing a sample in the C direction according to JIS-5 standard and conducting a tensile test. The degree of alloying and the plating weight were measured by a wet dissolution method using a hydrochloric acid solution.

[0065] Powdering and Flaking tests were conducted on the GA steel sheets. The plating is done by bending the plated material 90 degrees, then attaching tape to the bent part and peeling it off. The length of the plated layer peeled off from the tape was checked to see how many mm it had adhered to. If the thickness exceeds 1 mm, it is considered defective. In the flaking test, the material is processed into an inverted U shape. It was confirmed whether the plating layer fell off in the processed area.

[0066] For GI steel sheets, an adhesive for automobile construction was applied to the surface, and the steel sheet was bent at 90 degrees. When sealer is peeled off, check whether the plating layer has peeled off and adhered to the surface where the sealer has fallen. A sealer bending test (SBT) was conducted on the unplated steel plate. The surface quality is checked visually to see if there are any defects such as chipping or no plating. If it was visible, it was judged to be defective.

[0067] [Table 3]

[0068] In Table 3 above, 1) is the oxygen concentration profile and silicon and / or manganese proton The smaller value of the difference in the maximum depth of the file is the powdering length (mm) for 2) and the maximum depth (mm) for 3). The length (μm) of B-type LME cracks that occurred during electric resistance spot welding was indicates the length (μm) of C-type LME cracks that occurred during electric resistance spot welding. In the table, ND means Not Detected.

[0069] Inventive Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10, the steel composition is as set forth in the present invention. The manufacturing method also meets the scope of the present invention. The adhesion amount and LME crack length of the spot welds were also good.

[0070] In Comparative Examples 3 and 9, the hydrogen concentration in the annealing furnace was very low. As a result, the amount of surface oxidation in the surface layer was excessive, and the oxygen and Si of the GDOES in the surface layer were The difference between the maximum Mn depth and the maximum Mn depth was not large. This allowed the formation of a sufficient decarburized layer. The alloying suppression layer cannot be formed sufficiently at the interface between the coating layer and the base steel, and LME cracks are generated. The standard is not met, and surface quality deteriorates due to non-plating on the surface, and SBT peeling occurs, resulting in plating failure. The adhesion deteriorated.

[0071] In Comparative Examples 1 and 6, the coiling temperature during the hot rolling process did not satisfy the range proposed by the present invention. In Comparative Example 1, the hot rolling coiling temperature was lower than the range proposed by the present invention, and the internal oxidation that occurred during hot rolling was The amount of Si or M was insufficient, so the maximum oxygen concentration depth in the surface layer measured by GDOES was The difference between the maximum depth of n concentration and the maximum depth of n concentration exceeds 0.5 μm, and as a result, the LME crack is Comparative Example 6 was produced at a hot rolling coiling temperature exceeding that proposed by the present invention. The amount of internal oxidation generated during the hot rolling process was sufficient and the LME characteristics were good, but the hot rolling scale If excessive scale is generated, it cannot be completely removed during pickling, resulting in unplated areas and poor surface quality. During the flaking evaluation, peeling of the coating occurred, and the hot rolling coiling temperature was too high. The hot-rolled material softened and could not recover even after annealing, resulting in deterioration of the material.

[0072] In Comparative Example 12, the dew point in the furnace during annealing was controlled to be lower than the range proposed by the present invention. Even if a sufficient internal oxide layer is generated over the entire width during the hot rolling heating process, the internal oxide layer is not generated during the annealing process after cold rolling. In the case of the sewage, the dew point is not high enough to allow for sufficient internal oxidation, and the oxygen concentration at the surface layer by GDOES is The smaller of the difference between the maximum depth and the maximum depth of the Si or Mn concentration is 0.5 μm. The degree of surface decarburization is insufficient, and the LME crack length of the spot weld is poor. there were.

[0073] In Comparative Example 8, the dew point in the annealing furnace exceeded the range proposed by the present invention. By increasing the temperature, internal oxidation was sufficiently generated and the LME crack length was good, but Excessive internal oxidation can cause material deterioration and failure to meet tensile strength standards, and excessive dew points can cause surface oxidation. The amount of oxides generated also increased, and as a result of SBT, plating peeling occurred.

[0074] Comparative Example 10 is a case where the steel sheet passing speed in the annealing furnace was higher than the range proposed by the present invention. There is not enough time for the decarburization reaction between the steam in the annealing furnace and the steel sheet, resulting in annealing failure. The internal oxidation of the steel surface layer after the treatment was not sufficiently formed, and the maximum oxygen concentration depth measured by GDOES was and the depth of the maximum point of Si or Mn concentration is 0.5 μm or more, and the spot weld The LME crack evaluation criteria were exceeded and the product was defective.

[0075] In Comparative Example 2, the steel sheet passing speed in the annealing chamber is lower than the range proposed by the present invention. The decarburization reaction time during which the steam in the annealing furnace reacts with the steel sheet is excessive, causing the internal oxide of Si to form. The maximum oxygen concentration depth and Si concentration in the surface layer were measured by GDOES. The difference between the maximum depth of Mn concentration and the maximum depth of Mn concentration is 0.5 μm or more. Although the rack met the criteria for evaluation, the material quality was not satisfactory due to excessive decarburization.

[0076] In Comparative Example 5, the temperature of the soaking zone in the annealing furnace exceeded the range proposed by the present invention. The amount of external oxidation increases due to excessive blunting temperature, and internal oxidation is not sufficient, resulting in the GDO in the surface layer. The difference between the maximum depth of oxygen concentration and the maximum depth of Si or Mn concentration of ES is 0.5μm. m, resulting in LME cracks not meeting the standard and poor spot weldability. In addition, excessive austenite formation and growth in the soaking zone can cause material properties such as tensile strength to degrade. I couldn't satisfy it.

[0077] In Comparative Example 11, the temperature of the soaking zone in the annealing furnace was controlled lower than the range proposed by the present invention. The annealing temperature is low and the oxidation reaction between the steam and the steel sheet is insufficient, so internal oxidation occurs. As a result, the maximum depth of the oxygen and Si or Mn values ​​of GDOES in the surface layer The difference between the values ​​exceeds 0.5 μm, so the LME crack does not meet the criteria and the The weldability was poor. Also, recrystallization did not occur sufficiently during annealing, resulting in the target The microstructure required for the SBT is not formed, and the material quality, such as tensile strength, does not meet the standards. As a result of the evaluation, peeling occurred.

[0078] In Comparative Example 7, the reduction ratio during cold rolling exceeded the standard set forth in the present invention. The internal oxide layer formed in the steel becomes thinner near the surface due to excessive cold rolling. The maximum points are formed deep inside, the difference between the maximum points is 0.5 μm or more, and it is an LME crack. However, it did not meet the standards and was deemed defective.

[0079] In Comparative Example 4, the hydrogen concentration in the annealing furnace was less than 5% by volume, and the reducing atmosphere composition in the annealing furnace was In some cases, the increase in dew point is sufficient to cause internal oxidation and decarburization, resulting in the formation of The difference in maximum depth met the criteria of the present invention, and the LME crack length met the criteria, but The formation of surface oxides on the surface leads to unplated areas, which deteriorates the surface quality and causes the SBT plating to peel off. occurred.

[0080] From the above, the advantageous effects of the present invention were confirmed.

Claims

1. Base steel sheet, and A zinc-based plating layer formed on the surface of the base steel sheet A galvanized steel sheet comprising: One of oxygen, silicon, and manganese measured in the depth direction from the surface of the base steel sheet or the two concentration profiles have a form in which a maximum point appears in a depth direction from the surface, The depth at which the maximum point of the oxygen concentration profile is formed and the silicon and manganese The absolute difference in depth at which one of the concentration profiles forms a maximum point is 0.5 μm or less. There is galvanized steel sheet.

2. A depth at which the maximum point of the oxygen concentration profile is formed is 4 to 15 μm.

2. The zinc-plated steel sheet according to claim 1.

3. 3. The galvanized steel sheet according to claim 2, wherein the oxygen concentration at the maximum point is 0.3% by weight or more. .

4. The depth at which the maximum point of the oxygen concentration profile is formed is is smaller than the depth at which the maximum points of one or two of the concentration profiles are formed. The galvanized steel sheet according to claim 1.

5. 2. The zinc-plated coating of claim 1, wherein the concentration profile is measured by GDOES. Steel plate.

6. The coating weight of the zinc-based plating layer is 30 to 70 g / m 2 The subtilisin according to claim 1, Lead-plated steel sheet.

7. The steel plate has C: 0.05 to 1.5%, Si: 2.0% or less, Mn: 1.0 to 30%, S-Al (acid-soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or less, B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less, A composition comprising Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less, 7. The zinc-plated steel sheet according to any one of claims 6 to 6.

8. heating the steel slab at a temperature of 950-1350°C; hot rolling the steel slab to obtain a hot rolled steel sheet; coiling the hot-rolled steel sheet at a temperature of 590 to 750° C. to obtain a hot-rolled steel sheet; pickling the hot-rolled steel sheet at a threading speed of 180 to 250 mpm; cold rolling the hot rolled steel sheet at a rolling reduction of 35 to 60% to obtain a cold rolled steel sheet; The cold-rolled steel sheet is subjected to recrystallization annealing in an atmosphere having a dew point of 650 to 900°C and -10 to 30°C. Stages, and hot dip galvanizing the annealed cold rolled steel sheet A method for producing a galvanized steel sheet, comprising:

9. The recrystallization annealing step is carried out using hydrogen (H 2 The test was performed in a moist nitrogen gas atmosphere containing 5 to 10% by volume of The method for producing a galvanized steel sheet according to claim 8,

10. The galvanized steel sheet according to claim 9, wherein the sheet passing speed during the recrystallization annealing is 40 to 130 mpm. A method for manufacturing steel plates.

11. The hot dip galvanizing is performed at a steel sheet drawing temperature of 420 to 500°C and an Al concentration of 0.1 to 0 10. The galvanized steel sheet according to claim 8, wherein the galvanization is performed by immersing the steel sheet in a hot dip galvanizing bath having a galvanizing temperature of 0.25 wt.%. Manufacturing method.

12. Claim 1 further comprises a step of alloying at a temperature of 480-560°C after hot dip galvanizing.

2. A method for producing a galvanized steel sheet according to claim 1.

13. The steel slab comprises C: 0.05 to 1.5%, Si: 2.0% or less, Mn: 1.0 to 30 %, S-Al (acid soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or more Bottom, B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less The composition includes Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less.

13. The method for producing a galvanized steel sheet according to any one of claims 8 to 12.

Citation Information

Patent Citations

  • Pickling method for hot rolled steel sheet

    JP1986279311A

  • Method for pickling hot rolled steel sheet

    JP1987063687A

  • High strength galvanized steel sheet and method for manufacturing the same

    JP2014009399A

  • High strength steel sheet excellent in acid resistance and manufacturing method therefor

    JP2014122379A

  • Low-density hot-dip galvanized steel and its manufacturing method

    JP2019521257A