Silicon-containing compound-coated inorganic compound particle, and material for electronic component

A method for uniformly coating inorganic compound particles with silicon-containing compounds addresses non-uniformity issues, preserving base material properties and enhancing resin compatibility, suitable for high-frequency electronic components.

JP2024144180APending Publication Date: 2024-10-11SAKAI CHEM IND CO LTD

Patent Information

Application Number
JP2024031420
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for surface treatment of inorganic compound particles with silicon-containing compounds often result in non-uniform coatings, especially for larger particles, leading to impaired base material properties and incomplete coverage, which affects the effectiveness of the surface treatment.

Method used

A method involving mixing inorganic compound particles with a silicon-containing compound in a solvent, followed by solvent removal and hydrothermal treatment in an aqueous solution with a pH of 7 to 14, ensuring a thin and uniform coating layer of silicon-containing compound on the particles.

Benefits of technology

The resulting silicon-containing compound-coated inorganic compound particles maintain the properties of the base material, such as high dielectric constant and refractive index, while improving compatibility with resins and reducing dielectric loss tangent, making them suitable for high-frequency electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144180000003
    Figure 2024144180000003
  • Figure 2024144180000004
    Figure 2024144180000004
  • Figure 2024144180000005
    Figure 2024144180000005
Patent Text Reader

Abstract

To provide an inorganic compound particle having a coated layer (surface-treated layer) by a silicon-containing compound thin and even in thickness.SOLUTION: A silicon-containing compound-coated inorganic compound particle has a coated layer by a silicon-containing compound on a substrate particle surface represented by the following general formula (1): MxOy (in the formula (1), M is Zn, Ti, or Zr, x, y are each independently an integer of 1-3), or the following general formula (2): ATiO3 (in the formula (2), A is represented by Ca, Ba, or St), where the ratio (tA / D) of an average thickness tA of the coated layer to an average particle size D of the substrate particle is 0.02 or less, and the ratio (tmax / tc) of a calculated thickness tc of a coated layer by the silicon-containing compound when evenly coating the substrate particle with the silicon-containing compound and a maximum value tmax of thicknesses of the measured coated layer of the silicon-containing compound is 2.1 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to inorganic compound particles coated with a silicon-containing compound and materials for electronic components. [Background technology]

[0002] Inorganic compound particles are used as functional fillers that change the properties of resins when added to them. For example, inorganic compound particles having a perovskite crystal structure, such as ternary transition metal oxides such as barium titanate, are characterized by their high dielectric constant and refractive index, and are therefore used as functional fillers to increase the dielectric constant and refractive index. When inorganic compound particles are added to a resin, surface modification is generally performed in order to improve compatibility with the resin and dispersibility, and inorganic compound particles with various surface treatments have been reported. For example, there is a dispersion containing core-shell type oxide fine particles in which a metal oxide particle such as zirconium is used as a core particle and the core particle is covered with a shell layer mainly composed of a composite oxide of silicon and aluminum (see Patent Document 1); 2 Fe 17 N 3 Examples of such magnetic powders that have been described include a rare earth magnetic powder having a silica film formed on the particle surface of the magnetic powder by dry mixing with a silica sol obtained by hydrolyzing an alkyl silicate in a basic catalyst (see Patent Document 2); a luster pigment in which a titanium oxide coating formed on the surface of a flaky substrate is peeled off, a coating layer made of a metal oxide is formed on the surface of the titanium oxide coating, and a surface-treated layer of silica or the like is formed on the surface of the coating layer (see Patent Document 3); and barium titanate in which barium titanate seeds are synthesized in a liquid containing tetrahydroxysilane, tetraethoxysilane, or vinyltriethoxysilane, and then hydrothermally treated to form a surface-treated layer of silica (see Patent Document 4). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-143297 A [Patent Document 2] JP 2000-309802 A [Patent Document 3] JP 2004-224964 A [Patent Document 4] JP 2015-13792 A Summary of the Invention [Problem to be solved by the invention]

[0004] It is common to use silicon-containing compounds such as silica for surface coating of inorganic compound particles, and various effects such as imparting acid resistance and weather resistance, improving hydrophilicity, and improving reactivity with silicone-based surface treatment agents can be obtained. On the other hand, when surface treatment is performed with a silicon-containing compound, the surface of the substrate essentially becomes a silicon-containing compound, and when the amount of the silicon-containing compound coated is large, the characteristics of the substrate are weakened, so it is preferable to coat the substrate with as little amount as possible. Here, in surface modification using a silicon-containing compound such as silica, a method of forming a coating layer by precipitating the silicon-containing compound on the substrate surface is common, but if the amount of the silicon-containing compound is reduced in an attempt to reduce the coating thickness of the silicon-containing compound so as not to impair the characteristics of the substrate, the substrate is not uniformly coated over the entire substrate, and the silicon-containing compound is precipitated in an island shape, resulting in exposure of the uncoated substrate and the effect of the surface treatment cannot be fully exerted. In particular, when the particle size of the substrate is large, the surface area per substrate particle becomes large, making it more difficult to coat uniformly, and there is a problem that the amount of coating must be increased.

[0005] In view of the above-mentioned current situation, an object of the present invention is to provide inorganic compound particles having a thin and uniform coating layer (surface treatment layer) made of a silicon-containing compound. [Means for solving the problem]

[0006] The inventors have investigated a method for obtaining inorganic compound particles having a thin and uniform coating layer of a silicon-containing compound, and have succeeded in obtaining inorganic compound particles having a thin and uniform coating layer of a silicon-containing compound by mixing base particles of an inorganic compound and a silicon-containing compound in a solvent to prepare a slurry, removing the solvent from the slurry to obtain inorganic compound particles coated with a silicon-containing compound, and then subjecting the obtained inorganic compound particles to hydrothermal treatment in an aqueous solution of pH 7 to 14, thereby completing the present invention.

[0007] That is, the present invention is as follows. [1] The following general formula (1): M x O y (1) (In formula (1), M represents Zn, Ti or Zr, and x and y each independently represent an integer of 1 to 3), or The following general formula (2): ATiO 3 (2) (In the formula (2), A represents Ca, Ba or Sr.) The surface of the base particle is coated with a silicon-containing compound. The average thickness t of the coating layer of the silicon-containing compound with respect to the average particle diameter D of the base particle A Ratio of (t A / D) is 0.02 or less, The calculated thickness t of the coating layer of the silicon-containing compound when the silicon-containing compound is uniformly coated on the base particle c The largest thickness of the coating layer of the silicon-containing compound measured by observing 10 arbitrary points of the silicon-containing compound by TEM observation is t max Ratio to (t max / t c ) is less than or equal to 2.1 1. A silicon-containing compound coated inorganic particle comprising:

[0008] [2] The silicon-containing compound coated inorganic compound particles according to [1], characterized in that the base particles have an average particle size of 100 nm or more.

[0009] [3] The silicon-containing compound coated inorganic compound particles according to [1] or [2], characterized in that the silicon-containing compound is silica.

[0010] [4] The silicon-containing compound coated inorganic compound particle according to any one of [1] to [3], wherein the inorganic compound represented by the general formula (2) has a perovskite type crystal structure.

[0011] [5] A material for electronic parts, comprising the silicon-containing compound-coated inorganic compound particles according to any one of [1] to [4].

[0012] [6] An electronic component, characterized by using the material for electronic components described in [5].

[0013] [7] A method for producing inorganic compound particles having a coating layer made of a silicon-containing compound, comprising the steps of: The production method includes the following general formula (1): M x O y (1) (In formula (1), M represents Zn, Ti or Zr, and x and y each independently represent an integer of 1 to 3), or The following general formula (2): ATiO 3 (2) (wherein A represents Ca, Ba, or Sr) and a silicon-containing compound are mixed in a solvent to obtain a slurry; a second step of removing the solvent from the slurry to obtain inorganic compound particles having a coating layer of a silicon-containing compound; A method for producing inorganic compound particles having a coating layer made of a silicon-containing compound, comprising: a third step of hydrothermally treating the inorganic compound particles obtained in the second step in an aqueous solution having a pH of 7 to 14.

[0014] [8] The base particles are BaTiO 3 , SrTiO 3 , TiO 2The method for producing inorganic compound particles having a coating layer made of a silicon-containing compound according to [7], characterized in that the coating layer is made of a silicon-containing compound, or ZnO. Effect of the Invention

[0015] The silicon-containing compound-coated inorganic compound particles of the present invention are inorganic compound particles having a thin and uniform coating layer of a silicon-containing compound, and exhibit the effects of improving compatibility with resins due to the silicon-containing compound coating without impairing the properties of the base particle such as high dielectric constant and high refractive index, and can be suitably used as a filler for resin materials used as electronic components. [Brief description of the drawings]

[0016] [Figure 1] 1 is a TEM image of the inorganic compound particles obtained in Example 1. [Diagram 2] 1 is a TEM image of inorganic compound particles obtained in Example 2. [Diagram 3] 1 is a TEM image of inorganic compound particles obtained in Example 3. [Figure 4] 3 is a TEM image of the inorganic compound particles obtained in Comparative Example 1. [Diagram 5] 3 is a TEM image of inorganic compound particles obtained in Comparative Example 2. [Figure 6] 1 is a TEM image of inorganic compound particles obtained in Comparative Example 4. [Figure 7] 1 is a TEM image of inorganic compound particles obtained in Comparative Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] A preferred embodiment of the present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified and applied as appropriate within the scope that does not change the gist of the present invention.

[0018] 1. Silicon-containing compound coated inorganic compound particles The silicon-containing compound-coated inorganic compound particles of the present invention are represented by the following general formula (1): M x O y (1) (In formula (1), M represents Zn, Ti or Zr, and x and y each independently represent an integer of 1 to 3), or The following general formula (2): ATiO 3 (2) (In the formula (2), A represents Ca, Ba or Sr.) The inorganic compound particles have a coating layer of a silicon-containing compound on the surface of the base particle, and the average thickness t of the coating layer of the silicon-containing compound with respect to the average particle diameter D of the base particle is A Ratio of (t A One of its features is that the ratio of the thickness of the sintered body to the thickness of the sintered body is 0.02 or less. The average thickness t of the coating layer of the silicon-containing compound with respect to the average particle diameter D of the substrate particles A Ratio of (t A When the ratio (t / D) is 0.02 or less, it means that the thickness of the coating layer of the silicon-containing compound-coated inorganic compound of the present invention is thin relative to the particle size. A It is preferable that / D is 0.01 or less. The average particle diameter D of the substrate particles and the average thickness t of the coating layer made of the silicon-containing compound A can be measured by the method described in the Examples below.

[0019] Furthermore, the silicon-containing compound-coated inorganic compound particles of the present invention have a calculated thickness t of a coating layer of the silicon-containing compound when the silicon-containing compound is uniformly coated on the base particle. c The largest thickness of the coating layer of the silicon-containing compound measured by observing 10 arbitrary points of the silicon-containing compound by TEM observation is t max Ratio to (t max / t c ) is 2.1 or less. By satisfying this requirement, it can be said that the base particles are uniformly coated with the silicon-containing compound. t max / t c is preferably 1.2 or less, and more preferably 1.1 or less. The thickness of the coating layer of the silicon-containing compound can be measured by TEM observation according to the method described in the Examples below. Calculated thickness of the coating layer of the silicon-containing compound when the silicon-containing compound is uniformly coated on the base particle c can be calculated by the following formula (1).

[0020]

number

[0021] The silicon-containing compound coated inorganic compound particles of the present invention preferably have an average particle size of 100 nm or more of the base particle. As mentioned above, the larger the particle size of the base material, the more difficult it is to form a uniform thin coating on the base particle. Therefore, when the average particle size of the base particle is 100 nm or more, the technical significance of the silicon-containing compound coated inorganic compound particles of the present invention, which have a uniform thin coating on the base particle, is greater. The average particle size of the base particle is more preferably 300 nm or more. More preferably, it is 800 nm or more. There is no particular upper limit to the average particle size of the base particles, but when used as a resin filler, particles having a diameter of 100 μm or less are usually used. The average particle size of the base particles of the silicon-containing compound-coated inorganic compound particles can be measured by the method described in the Examples below.

[0022] In the silicon-containing compound coated inorganic compound particles of the present invention, the silicon-containing compound coating the base particle is not particularly limited as long as it is a compound containing silicon element capable of coating inorganic compound particles, and examples thereof include silica, zeolite, sodium silicate, zinc silicate, magnesium silicate, etc., and one or more of these can be used. Among these, silica is preferred from the viewpoint of acid resistance. Silica is SiO 2There are no particular limitations as long as the compound is represented by the formula (I), and for example, hydrophobic dry process silica, hydrophobic wet process silica, etc. can be used.

[0023] The silicon-containing compound coated inorganic compound particles of the present invention exhibit the effect of improving compatibility with resins by coating with silicon-containing compounds without impairing the characteristics of the base particle such as high dielectric constant and high refractive index.The silicon-containing compound coated inorganic compound particles of the present invention further have a low dielectric loss tangent compared to conventional inorganic compound particles having a coating layer of a surface treatment agent.In recent years, with the progress of information and communication technology, the signal transmission in the high frequency range, which is increasing, has a larger transmission loss than the conventional wavelength, so a material with a low dielectric loss tangent is required.The silicon-containing compound coated inorganic compound particles of the present invention can be suitably used as a material for high frequency electronic components that use such a high frequency range.

[0024] 2. Method for producing inorganic compound particles coated with silicon-containing compound The present invention also provides a method for producing inorganic compound particles having a coating layer made of a silicon-containing compound, the method comprising reacting a silicon-containing compound with a silicon-containing compound having a silicon-containing compound represented by the following general formula (1): M x O y (1) (In formula (1), M represents Zn, Ti or Zr, and x and y each independently represent an integer of 1 to 3), or The following general formula (2): ATiO 3 (2) (in formula (2), A represents Ca, Ba or Sr) and a silicon-containing compound in a solvent to obtain a slurry; a second step of removing the solvent from the slurry to obtain inorganic compound particles having a coating layer of the silicon-containing compound; and a third step of hydrothermally treating the inorganic compound particles obtained in the second step in an aqueous solution having a pH of 7 to 14 (hereinafter, also referred to simply as the production method of the present invention). By using such a manufacturing method, it is possible to produce silicon-containing compound-coated inorganic compound particles in which a uniformly thin coating of a silicon-containing compound is formed on an inorganic compound base particle, even when the average particle diameter of the base particle is large.

[0025] The first step in the production method of the present invention is a step of mixing base particles of an inorganic compound and a silicon-containing compound in a solvent to obtain a slurry. The amount of silicon-containing compound used in the first step can be appropriately adjusted depending on the average particle size and density of the inorganic compound base particles and the type of silicon-containing compound. Specifically, for example, in the case of strontium titanate having an average particle size of 300 nm and silica as the silicon-containing compound, the amount of silicon-containing compound used is preferably 0.1-5.4% by mass, more preferably 1.0-2.0% by mass, based on 100% by mass of strontium titanate. When the barium titanate has an average particle size of 100 nm and the silicon-containing compound is silica, the amount of the silicon-containing compound used is preferably 0.1 to 5.4 mass %, more preferably 2.0 to 4.0 mass %, based on 100 mass % of barium titanate. When the barium titanate has an average particle size of 800 nm and the silicon-containing compound is silica, the amount of the silicon-containing compound used is preferably 0.1 to 4.6 mass %, more preferably 0.5 to 2.0 mass %, based on 100 mass % of barium titanate.

[0026] Examples of the silicon-containing compound used in the first step include silicates such as sodium metasilicate, magnesium metasilicate, and zinc silicate, silica powder, and zeolite, and one or more of these can be used.

[0027] In the first step, the solvent used to prepare the slurry of the base particles of the inorganic compound and the silicon-containing compound is not particularly limited, but may be water.

[0028] The amount of the solvent used in the first step is not particularly limited as long as a slurry of the inorganic compound base particles and the silicon-containing compound is obtained, but is preferably 50 to 10,000 mass % relative to 100 mass % of the inorganic compound particles, and more preferably 200 to 3,000 mass %.

[0029] In the first step, the method for mixing the base particles of the inorganic compound and the silicon-containing compound in the solvent is not particularly limited, and can be performed using a ribbon mixer, a Spartan mixer, a planetary ball mill, a bead mill, etc. Examples of media to be used when using either a planetary ball mill or a bead mill include glass beads, alumina beads, zirconia beads, titania beads, silicon nitride beads, agate beads, tungsten carbide beads, etc.

[0030] In the first step, when a water-soluble silicate such as sodium metasilicate is used as the silicon-containing compound, it is preferable to mix the base material particles and the silicon-containing compound in a solvent to obtain a slurry, and then perform a step of neutralizing the slurry. By neutralizing, a silicic acid-containing compound that is poorly soluble in water is obtained, and the excess solvent can be easily separated by filtration. If the slurry is basic, such as when sodium metasilicate is used as the silicon-containing compound, it can be neutralized with hydrochloric acid, nitric acid, sulfuric acid, acetic acid, or the like.

[0031] In the second step of the manufacturing method of the present invention, the method for removing the solvent from the slurry to obtain inorganic compound particles having a coating layer of a silicon-containing compound is not particularly limited as long as the solvent is removed, but a method in which the slurry is dried to remove the solvent is preferred. The drying temperature when drying the slurry is preferably 80 to 300°C, more preferably 100 to 130°C, from the viewpoint of efficiently removing the solvent and preventing the inorganic compound particles from being altered by heat. The drying time is not particularly limited, but in consideration of sufficient removal of the solvent and production efficiency, it is preferably 1 to 24 hours, and more preferably 3 to 10 hours.

[0032] When the slurry is dried to remove the solvent in the second step, it is preferable to carry out a step of washing the solid content of the slurry before drying. By washing the solid content, it is possible to obtain silicon-containing compound-coated inorganic compound particles with few impurities. The method for washing the solid content of the slurry is not particularly limited, but a method can be used in which the solid content of the slurry is separated by filtration, and then the solid content is washed with a solvent once or twice or more. The solvent for washing can be the same as that used in the first step.

[0033] The third step of the production method of the present invention is a step of hydrothermally treating the inorganic compound particles obtained in the second step in an aqueous solution having a pH of 7-14. The inorganic compound particles obtained in the second step are coated with the silicon-containing compound, but the coating is not sufficiently uniform. In particular, when the particle diameter of the inorganic compound particles is large, the coating tends to be in an island-like state in which there are coated and uncoated parts. When such inorganic compound particles are hydrothermally treated with an aqueous solution of pH 7 to 14, a part of the silicon-containing compound in the coated part dissolves. At that time, the silicic acid-containing compound coats the entire base particle evenly, making the coating layer uniform, and thus it is possible to obtain inorganic compound particles that are uniformly coated even if the coating layer is thin. The hydrothermal treatment of the inorganic compound particles may be carried out in an aqueous solution having a pH of 7 to 14, preferably in an aqueous solution having a pH of 7.5 to 11, and more preferably in an aqueous solution having a pH of 8 to 9.

[0034] The hydrothermal treatment in the third step is not particularly limited, but is usually carried out in a heat-resistant container such as an autoclave. The treatment temperature for the hydrothermal treatment is not particularly limited, but is preferably 80 to 300°C, and more preferably 100 to 200°C. The time for the hydrothermal treatment is not particularly limited, but is preferably 0.5 to 24 hours, and more preferably 4 to 12 hours.

[0035] In the third step, after the hydrothermal treatment, the process of separating the solvent and the solid content (silicon-containing compound coated inorganic compound particles) from the slurry is carried out. The method of separating the solvent and the solid content (silicon-containing compound coated inorganic compound particles) from the slurry after the hydrothermal treatment is not particularly limited, but filtration or centrifugation can be used. In addition, after the step of separating the solid content from the solvent, it is preferable to perform a step of washing the solid content with water. After washing with water, a step of separating the solid content by filtration or centrifugation can be performed to obtain the washed solid content. The washing step and the separation step of the solid content may each be performed once or twice or more.

[0036] In the third step, it is preferable to further carry out a step of separating the solvent and solids from the slurry after the hydrothermal treatment, optionally carrying out a water washing step and a solids separation step, and then carrying out a step of drying the solids. The temperature for drying the solid content is not particularly limited, but is preferably 80 to 300°C, and more preferably 100 to 130°C. The drying time is not particularly limited as long as the solid content is sufficiently dried, but it is preferably 1 to 24 hours, and more preferably 3 to 10 hours.

[0037] The method for producing silicon-containing compound-coated inorganic compound particles of the present invention may include other steps other than the above-mentioned steps. Examples of other steps include a step of pulverizing the solid content after drying obtained in the second step or the third step, and a step of classifying the pulverized solid content.

[0038] 3. Materials for electronic components, electronic components The silicon-containing compound coated inorganic compound particles of the present invention have the characteristics of inorganic compounds, and are surface-treated, so that they have high compatibility with resins, and can be mixed uniformly into resins when mixed into resins.Therefore, the silicon-containing compound coated inorganic compound particles of the present invention can be suitably used as a functional filler that changes the properties of resins by adding them to resins.In particular, inorganic compounds having a perovskite crystal structure have the characteristics of high dielectric constant and refractive index, and low dielectric tangent, so that they can be mixed uniformly into resins while retaining these characteristics. A material for electronic devices containing such inorganic compound particles coated with a silicon-containing compound also constitutes one aspect of the present invention, and an electronic device formed using the material for electronic devices of the present invention also constitutes one aspect of the present invention. EXAMPLES

[0039] In order to explain the present invention in detail, specific examples are given below, but the present invention is not limited to these examples. Unless otherwise specified, "%" and "wt%" mean "weight % (mass %)". The various measurement and calculation methods are as follows.

[0040] <Particle diameter D of base particles> The particle size was calculated based on the specific surface area of ​​the base particles measured with a BET specific surface area measuring device (Macsorb Model HM-1220 manufactured by Mountec Co., Ltd.), assuming that the base particles were spherical. <Silicon-containing compounds (SiO 2 ) SiO in coated particles 2 Percentage of The amount of Ti and Si was measured using a fluorescent X-ray analyzer (Rigaku Corporation, ZSX Primus II) to determine the amount of SiO 2 / BaTiO 3 Or SiO 2 / SrTiO 3 The weight ratio (%) was calculated. <Silicon-containing compounds (SiO 2 ) calculated thickness of the coating layer t c > As shown in the above formula (1), the specific gravity ρ1 of the substrate, the average particle diameter D, and SiO2 Specific gravity ρ2 and SiO 2 SiO in coated particles 2 From the ratio of 2 When covered with SiO 2 Calculate the thickness, calculate thickness t c It was decided. The specific gravity ρ1 of the substrate was the specific gravity of barium titanate (6.02) and the specific gravity of strontium titanate (5.12), and the specific gravity ρ2 of the silicon-containing compound was the specific gravity of silica (2.20). <Silicon-containing compounds (SiO 2 ) the maximum thickness of the coating layer t max > Observation with a TEM (JEM-2100F, manufactured by JEOL Ltd.) revealed that SiO 2 The maximum thickness t max It was decided. <Silicon-containing compounds (SiO 2 ) Average thickness of the coating layer on the coated particles t A > Observation with a TEM (JEM-2100F, manufactured by JEOL Ltd.) revealed that SiO 2 SiO measured by observing 10 randomly selected points on the coated particle 2 The average thickness of the coating layer is the average thickness t A It was decided. <Silicon-containing compounds (SiO 2 ) Powder dielectric properties of coated particles> The powder dielectric properties of the silicon-containing compound coated inorganic compound were determined by measuring the dielectric constant ε and dielectric tangent tanδ of the powder at 1 GHz in TM mode using a cavity resonator ADMS01Nc1 manufactured by AET Corporation and a vector network analyzer P9373A manufactured by Keysight Technologies.

[0041] Example 1 [First step] 25 g of strontium titanate particles (manufactured by Sakai Chemical Industry Co., Ltd.) having a perovskite crystal structure with a particle diameter of 300 nm was repulped with 250 g of ion-exchanged water, and 2.4 g (0.50 g in terms of silica) of sodium metasilicate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd.) was added to prepare a slurry. The obtained slurry was heated with stirring, the liquid temperature was kept between 80°C and 90°C, and 73 g of nitric acid diluted to 2.5% by weight was added over 2 hours. [Second process] The slurry obtained in the first step was cooled to room temperature, filtered, washed with water, and dried at 105° C. for 10 hours to obtain dried particles of silica-coated strontium titanate. [Third step] Sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 250 g of ion-exchanged water to prepare an aqueous solution with a pH of 8.0, and the dried particles of silica-coated strontium titanate obtained in the second step were added, and the entire amount was repulped to prepare a slurry. The prepared repulp slurry was placed in an autoclave and subjected to hydrothermal treatment at 200°C for 12 hours. After cooling the slurry after the hydrothermal treatment to room temperature, it was subjected to solid-liquid separation using a centrifuge, and the precipitate was repulped with ion-exchanged water. The obtained repulp slurry was again subjected to solid-liquid separation using a centrifuge, and the precipitate was washed with ion-exchanged water. Washing was performed a total of five times. The washed precipitate was dried at 105°C for 10 hours to obtain silica-coated strontium titanate particles. When the obtained silica-coated strontium titanate particles were subjected to fluorescent X-ray analysis, the Si / Ti ratio was found to be 0.036, which was converted to 1.18 wt % in terms of silica / strontium titanate.

[0042] Example 2 The same operations as in Example 1 were carried out to obtain silica-coated barium titanate particles, except that in the first step of Example 1, barium titanate particles having a particle diameter of 100 nm (manufactured by Sakai Chemical Industry Co., Ltd.) were used instead of strontium titanate particles having a particle diameter of 300 nm, the amount of sodium metasilicate added was changed to 5.9 g (1.24 g in terms of silica), and in the third step, the pH of the aqueous solution was changed to 7.0. When the obtained silica-coated barium titanate particles were subjected to fluorescent X-ray analysis, the Si / Ti ratio was found to be 0.154, which was converted to 3.97 wt % in terms of silica / barium titanate.

[0043] Example 3 The same operations as in Example 1 were carried out to obtain silica-coated barium titanate particles, except that in the first step of Example 1, barium titanate particles having a particle diameter of 800 nm (manufactured by Sakai Chemical Industry Co., Ltd.) were used instead of strontium titanate particles having a particle diameter of 300 nm, the amount of sodium metasilicate added was changed to 3.0 g (0.63 g in terms of silica), and in the third step, the pH of the aqueous solution was changed to 11.0. When the obtained silica-coated barium titanate particles were subjected to fluorescent X-ray analysis, the Si / Ti ratio was found to be 0.078, which was converted to 2.00 wt % in terms of silica / barium titanate.

[0044] Example 4 The same operations as in Example 1 were carried out to obtain silica-coated titanium oxide particles, except that in the first step of Example 1, titanium oxide particles (manufactured by Sakai Chemical Industry Co., Ltd.) having a particle diameter of 3 μm were used instead of strontium titanate particles having a particle diameter of 300 nm, the amount of sodium metasilicate added was changed to 1.1 g (0.23 g in terms of silica), and the hydrothermal treatment in the third step was carried out at 140°C for 6 hours. When the obtained silica-coated titanium oxide particles were subjected to fluorescent X-ray analysis, the Si / Ti molar ratio was found to be 0.011, which was calculated as 0.80 wt % in terms of silica / titanium oxide.

[0045] Example 5 The same operations as in Example 1 were carried out to obtain silica-coated zinc oxide particles, except that in the first step of Example 1, zinc oxide particles (manufactured by Sakai Chemical Industry Co., Ltd.) having a particle diameter of 2 μm were used instead of strontium titanate particles having a particle diameter of 300 nm, the amount of sodium metasilicate added was changed to 1.2 g (0.25 g in terms of silica), and the hydrothermal treatment in the third step was carried out at 100° C. for 6 hours. When the obtained silica-coated zinc oxide particles were subjected to fluorescent X-ray analysis, the Si / Zn molar ratio was found to be 0.010, which was converted to 0.74 wt % in terms of silica / zinc oxide.

[0046] Example 6 The same operations as in Example 1 were carried out to obtain silica-coated titanium oxide particles, except that in the first step of Example 1, titanium oxide particles (manufactured by Sakai Chemical Industry Co., Ltd.) having a particle diameter of 300 nm were used instead of strontium titanate particles having a particle diameter of 300 nm, the amount of sodium metasilicate added was changed to 4.8 g (1.0 g in terms of silica), and the hydrothermal treatment in the third step was carried out at 200°C for 6 hours. When the obtained silica-coated titanium oxide particles were subjected to fluorescent X-ray analysis, the Si / Ti molar ratio was found to be 0.044, which was converted to 3.34 wt % in terms of silica / titanium oxide.

[0047] Comparative Example 1 The same procedures as in Example 1 up to the second step were carried out, and the resulting dried particles were used as silica-coated strontium titanate of Comparative Example 1. When the obtained silica-coated strontium titanate was analyzed by a fluorescent X-ray analyzer, the Si / Ti ratio was found to be 0.050, which was converted to 1.67 wt % in terms of silica / strontium titanate.

[0048] Comparative Example 2 In the first step of Example 1, except that the amount of sodium metasilicate added was changed to 7.08 g, the process up to the second step was carried out in the same manner as in Example 1, and the obtained dried particles were used as silica-coated strontium titanate of Comparative Example 2. When the obtained silica-coated strontium titanate was analyzed by a fluorescent X-ray analyzer, the Si / Ti ratio was found to be 0.130, which was converted to 4.25 wt % in terms of silica / strontium titanate.

[0049] Comparative Example 3 The strontium titanate particles having a particle diameter of 300 nm used as the substrate in Example 1 (without being coated with silica) were used as the particles in Comparative Example 3.

[0050] Comparative Example 4 The same procedures as in Example 2 were carried out up to the second step, and the resulting dried particles were used as silica-coated barium titanate of Comparative Example 4. When the obtained silica-coated barium titanate was analyzed by a fluorescent X-ray analyzer, the Si / Ti ratio was 0.168, which was equivalent to 4.33 wt % in terms of silica / barium titanate.

[0051] Comparative Example 5 The barium titanate particles having a particle diameter of 100 nm used as the substrate in Example 2 (without being coated with silica) were used as the particles in Comparative Example 5.

[0052] Comparative Example 6 The same procedures as in Example 3 up to the second step were carried out, and the obtained dried particles were used as silica-coated barium titanate of Comparative Example 6. When the obtained silica-coated barium titanate was analyzed by a fluorescent X-ray analyzer, the Si / Ti ratio was found to be 0.083, which was calculated as 2.14 wt% in terms of silica / barium titanate.

[0053] Comparative Example 7 The barium titanate particles having a particle diameter of 800 nm used as the substrate in Example 3 (without being coated with silica) were used as the particles in Comparative Example 7.

[0054] Comparative Example 8 The titanium oxide particles having a particle diameter of 3 μm used as the substrate in Example 4 (without being coated with silica) were used as the particles in Comparative Example 8.

[0055] Comparative Example 9 The zinc oxide particles having a particle diameter of 2 μm used as the substrate in Example 5 (without being coated with silica) were used as the particles in Comparative Example 9.

[0056] Comparative Example 10 The titanium oxide particles having a particle diameter of 300 nm used as the substrate in Example 6 (without being coated with silica) were used as the particles in Comparative Example 10.

[0057] The results of various measurements of the silica-coated strontium titanate, silica-coated barium titanate, silica-coated titanium oxide, and silica-coated zinc oxide obtained in the Examples and Comparative Examples are shown in Table 1. In Table 1, ε 1 , tan δ 1 is the value of silica-coated strontium titanate, silica-coated barium titanate, silica-coated titanium oxide, or silica-coated zinc oxide, and ε 2 , tan δ 2 is the value of the substrate strontium titanate, barium titanate, titanium oxide or zinc oxide. t max / t c The smaller the value of t, the more uniform the silica coating layer is (minimum value is 1.0). A / D is a relative index of the thickness of the silica coating layer, and if this value is large, tan δ deteriorates due to the hydroxyl groups contained in the silica.

[0058] [Table 1]

[0059] From the results of the Examples and Comparative Examples, it was confirmed that strontium titanate, barium titanate, titanium oxide, or zinc oxide having a thin and uniform silica coating layer can be obtained by using the manufacturing method of the present invention. It was also confirmed that the strontium titanate, barium titanate, titanium oxide, or zinc oxide of the Examples having such a coating layer have a lower dielectric tangent (tan δ) and are superior in dielectric properties compared to those of the Comparative Examples.

Claims

1. The following general formula (1): M x O y (1) (In formula (1), M represents Zn, Ti, or Zr, and x and y each independently represent an integer of 1 to 3), or The following general formula (2): ATiO 3 (2) (In the formula (2), A represents Ca, Ba or Sr.) The surface of the base particle is coated with a silicon-containing compound. The average thickness t of the coating layer of the silicon-containing compound relative to the average particle diameter D of the base particle A The ratio (t A / D) is 0.02 or less, The calculated thickness t of the coating layer of the silicon-containing compound when the silicon-containing compound is uniformly coated on the base particle c and the largest thickness of the coating layer of the silicon-containing compound measured by observing 10 arbitrary points of the silicon-containing compound by TEM observation, t max Ratio to (t max / t c ) is 2.1 or less 1. A silicon-containing compound coated inorganic particle comprising:

2. 2. The silicon-containing compound coated inorganic particle according to claim 1, wherein the average particle size of the base particle is 100 nm or more.

3. 2. The silicon-containing compound coated inorganic particle according to claim 1, wherein the silicon-containing compound is silica.

4. 2. The silicon-containing compound coated inorganic compound particle according to claim 1, wherein the inorganic compound represented by the general formula (2) has a perovskite type crystal structure.

5. A material for electronic parts, comprising the silicon-containing compound-coated inorganic compound particles according to any one of claims 1 to 4.

6. An electronic component, comprising the material for electronic components according to claim 5.

7. A method for producing inorganic compound particles having a coating layer made of a silicon-containing compound, comprising the steps of: The production method includes the following general formula (1): M x O y (1) (In formula (1), M represents Zn, Ti, or Zr, and x and y each independently represent an integer of 1 to 3), or The following general formula (2): ATiO 3 (2) (wherein A represents Ca, Ba or Sr) and a silicon-containing compound are mixed in a solvent to obtain a slurry; a second step of removing the solvent from the slurry to obtain inorganic compound particles having a coating layer of a silicon-containing compound; and a third step of hydrothermally treating the inorganic compound particles obtained in the second step in an aqueous solution having a pH of 7 to 14.

8. The base particles are BaTiO 3 , SrTiO 3 , TiO 2 8. The method for producing inorganic compound particles having a coating layer made of a silicon-containing compound according to claim 7, characterized in that the coating layer made of the silicon-containing compound is ZnO.

Citation Information

Patent Citations

  • Rare earth magnetic powder, method for surface treatment of the same and rare earth bond magnet using the same

    JP2000309802A

  • Luster pigment and method for producing the same

    JP2004224964A

  • Production method of barium titanate coated with highly crystalline silicon dioxide, and barium titanate powder coated with highly crystalline silicon dioxide produced by the method

    JP2015013792A

  • Dispersion of core-shell type oxide fine particles, production method of same, and use of same

    JP2015143297A

Cited By

  • Inorganically treated zinc oxide, inorganically treated zinc oxide dispersion, and cosmetic