Water-soluble polymer composition

A water-soluble polymer composition with phenolic antioxidants, sulfur-containing amine compounds, and inorganic salts addresses viscosity issues in industrial solutions with iron and oxidizing agents, ensuring stable paper production.

JP2024144241APending Publication Date: 2024-10-11SUMITOMO SEIKA CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024043902
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Water-soluble polymer aqueous solutions used in industrial applications, such as papermaking, experience viscosity decreases due to the presence of iron ions and oxidizing agents, leading to issues like non-uniform dispersion and sedimentation.

Method used

A water-soluble polymer composition comprising a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt, excluding transition metal salts, is formulated to maintain viscosity stability even in the presence of iron ions and oxidizing agents.

Benefits of technology

The composition effectively prevents viscosity reduction and maintains stability over time, ensuring uniform dispersion and sedimentation control in papermaking processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144241000001
    Figure 2024144241000001
Patent Text Reader

Abstract

To provide a water-soluble polymer aqueous solution capable of preparing an aqueous solution unlikely to cause viscosity decrease and capable of suppressing occurrence of temporal viscosity decrease even when water in which iron ion and acidic chemical are present is used, a paper making agent, water solution and a producing method thereof, and methods of producing industrial chemical, a kit, and paper.SOLUTION: A water-soluble polymer composition of the present invention includes a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt excluding transition metal salts. According to the water-soluble polymer composition of the present invention, a water-soluble polymer aqueous solution in which a decrease in viscosity is unlikely to occur even if water in which an iron ion and an oxidizing agent are present is used, and the occurrence of a decrease in viscosity over time is suppressed, can be prepared.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-soluble polymer composition, a papermaking tackifier, an aqueous solution and a method for producing the same, an industrial chemical, a kit, and a method for producing paper. [Background technology]

[0002] Water-soluble polymers such as polyalkylene oxides are widely used as industrial chemicals (e.g., thickeners for papermaking, flocculants, dispersants, sedimentation promoters, etc.) in various industrial applications such as papermaking, mining, cement, and dyeing (see Patent Document 1). In these fields, water-soluble polymers are often used as aqueous solutions of, for example, about 1 ppm to 15%.

[0003] In general, the water used to prepare the above-mentioned aqueous water-soluble polymer solution may contain iron ions. Such iron ions may be mixed into the water due to, for example, iron rust in piping. When the aqueous water-soluble polymer solution contains iron ions, there is a problem that the viscosity decreases over time. Such a decrease in the viscosity of the aqueous water-soluble polymer solution may be detrimental to the expression of the functions of the water-soluble polymer. For example, in papermaking applications, the aqueous water-soluble polymer solution is used as a papermaking thickener for paper stock, and a decrease in the viscosity of the aqueous solution may hinder the uniform dispersion of the paper stock and cause sedimentation, which may hinder uniform papermaking.

[0004] From this viewpoint, for example, Patent Document 2 discloses a technique for suppressing the decrease in viscosity of an aqueous solution of a water-soluble polymer over time by using a phenolic antioxidant and an inorganic salt in combination at a predetermined ratio. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2017 / 104496 [Patent Document 2] International Publication No. 2021 / 241662 Summary of the Invention [Problem to be solved by the invention]

[0006] However, industrial water used for preparing the aqueous solution of water-soluble polymers often contains not only iron ions as described above, but also oxidizing agents such as bactericides and slime control agents for the purpose of improving water quality.In this regard, the present inventors have found that even if the viscosity reduction of the aqueous solution of water-soluble polymers using water containing iron ions can be suppressed, the viscosity reduction of the aqueous solution of water-soluble polymers using water containing oxidizing agents in addition to iron ions cannot necessarily be suppressed.Since industrial water is likely to contain oxidizing agents in addition to iron ions, it is important in various industrial chemical applications to suppress the occurrence of viscosity reduction of the aqueous solution of water-soluble polymers obtained using water containing both iron ions and oxidizing agents, and particularly in the above-mentioned papermaking application, it is extremely important for uniform papermaking.

[0007] The present invention has been made in view of the above, and has an object to provide a water-soluble polymer composition, a papermaking thickener, an aqueous solution, an industrial chemical, and a kit capable of preparing a water-soluble polymer aqueous solution that is resistant to viscosity reduction and can suppress viscosity reduction over time, even when water containing iron ions and an oxidizing agent is used, as well as a method for producing such an aqueous solution and a method for producing paper. [Means for solving the problem]

[0008] That is, the present invention includes, for example, the subject matter described in the following sections.

[0009] Item 1 A water-soluble polymer composition comprising a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt excluding transition metal salts. Section 2 the content of the inorganic salt is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer, Item 2. The water-soluble polymer composition according to item 1, wherein the content of the sulfur-containing amine compound is 0.001 to 10 parts by mass based on 100 parts by mass of the water-soluble polymer. Section 3 Item 3. The water-soluble polymer composition according to item 1 or 2, wherein the water-soluble polymer is at least one polymer selected from the group consisting of a homopolymer of (meth)acrylamide, a neutralized product of a (meth)acrylamide-(meth)acrylic acid copolymer, polyethylene oxide, polypropylene oxide, and an ethylene oxide-propylene oxide copolymer. Section 4 4. The water-soluble polymer composition according to any one of items 1 to 3, wherein the inorganic salt is neutral or alkaline in an aqueous solution state. Section 5 Item 5. The water-soluble polymer composition according to any one of items 1 to 4, wherein the content of the phenol-based antioxidant is 0.001 to 5 parts by mass based on 100 parts by mass of the water-soluble polymer. Section 6 6. The water-soluble polymer composition according to any one of items 1 to 5, wherein the inorganic salt is contained in an amount of 20 to 10,000 parts by mass per 100 parts by mass of the phenol-based antioxidant. Section 7 7. The water-soluble polymer composition according to any one of items 1 to 6, wherein the sulfur-containing amine compound is contained in an amount of 20 to 10,000 parts by mass based on 100 parts by mass of the phenol-based antioxidant. Section 8 8. An aqueous solution comprising the water-soluble polymer composition according to any one of items 1 to 7 and water. Section 9 Item 9. The aqueous solution according to item 8, comprising iron ions and an oxidizing agent. Section 10 Item 8. An industrial chemical comprising the water-soluble polymer composition according to any one of items 1 to 7. Item 10´ Item 9. An industrial chemical containing the aqueous solution according to item 8. Section 11 Item 8. A papermaking adhesive comprising the water-soluble polymer composition according to any one of items 1 to 7. Item 11´ Item 9. A papermaking adhesive comprising the aqueous solution according to item 8. Section 12 Item 8 or 9, a method for producing an aqueous solution comprising the steps of: A method of manufacturing comprising the step of mixing the water-soluble polymer composition with water containing iron ions and an oxidizing agent. Section 13 A first agent including a water-soluble polymer and a phenol-based antioxidant; a second agent containing an inorganic salt excluding transition metal salts; A third agent containing a sulfur-containing amine compound is provided, The kit, wherein the content of the inorganic salt in the second agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent, and the content of the sulfur-containing amine compound in the third agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent. Section 14 Item 14. A method for producing an aqueous solution using the kit according to item 13, A step of mixing the second agent, the third agent, and water containing iron ions and an oxidizing agent to obtain a mixed solution; mixing the mixture with the first agent; The method for producing an aqueous solution comprises the steps of: Section 15 Item 14. A method for producing an aqueous solution using the kit according to item 13, A step of mixing water containing iron ions and an oxidizing agent with the first agent to obtain a mixed solution, and a step of mixing the mixed solution with the second agent and the third agent; The method for producing an aqueous solution comprises the steps of: Item 16 Item 8 or 9. A step of preparing an aqueous dispersion of the paper stock by mixing the aqueous solution according to item 8 or 9 with the paper stock; A step of making paper from the aqueous dispersion of the paper stock; A method for producing paper comprising the steps of: Item 17 Item 8. A viscosity reduction inhibitor comprising the water-soluble polymer composition according to any one of items 1 to 7. Section 18 8. A method for suppressing a decrease in viscosity of an aqueous solution, comprising the step of preparing an aqueous solution of the water-soluble polymer composition according to any one of items 1 to 7. Section 19 Item 8. Use of the water-soluble polymer composition according to any one of items 1 to 7 in an aqueous solution. Section 20 Item 8. Use of the water-soluble polymer composition according to any one of items 1 to 7 as a papermaking adhesive. Effect of the Invention

[0010] According to the water-soluble polymer composition of the present invention, even if water containing iron ions and an oxidizing agent is used, it is possible to prepare an aqueous water-soluble polymer solution that is resistant to viscosity reduction and can also suppress the occurrence of viscosity reduction over time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".

[0012] In the numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range can be arbitrarily combined with the upper or lower limit of another numerical range. In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in an example or a value that can be unambiguously derived from an example. In addition, in this specification, a numerical value connected with "~" means a numerical range that includes the numerical values ​​before and after "~" as the lower and upper limits.

[0013] 1. Water-soluble polymer composition The water-soluble polymer composition of the present invention contains a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt. Here, the inorganic salt does not include transition metal salts. With such a water-soluble polymer composition, even if water containing iron ions and an oxidizing agent is used, it is possible to prepare an aqueous water-soluble polymer solution that is unlikely to cause a decrease in viscosity and that can suppress the occurrence of a decrease in viscosity over time. Therefore, the polymer composition of the present invention can be suitably used in various industrial chemicals, and can contribute to the uniform dispersion of paper material and the prevention of sedimentation during the papermaking process in papermaking, etc., thereby contributing to the stable production of paper.

[0014] (Water-soluble polymer) The water-soluble polymer contained in the water-soluble polymer composition of the present invention is not particularly limited, and examples thereof include a wide range of known polymers having water solubility.

[0015] Specific examples of the water-soluble polymer include water-soluble polyalkylene oxides such as polyethylene oxide, polypropylene oxide, and ethylene oxide-propylene oxide copolymers; neutralized (meth)acrylamide-(meth)acrylic acid copolymers; (meth)acrylamide homopolymers; polyvinyl alcohol; polyamino acids; celluloses such as carboxymethyl cellulose or a salt thereof; etc. The copolymer may be a block copolymer or a random copolymer.

[0016] In this specification, "(meth)acrylic" means "acrylic" or "methacrylic", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)allyl" means "allyl" or "methallyl".

[0017] Among them, the water-soluble polymer is preferably at least one polymer selected from the group consisting of a homopolymer of (meth)acrylamide, a neutralized product of a (meth)acrylamide-(meth)acrylic acid copolymer, polyethylene oxide, polypropylene oxide, and an ethylene oxide-propylene oxide copolymer. In this case, even if water containing iron ions and an oxidizing agent is used, it becomes easy to prepare an aqueous solution of the water-soluble polymer that is less likely to reduce in viscosity.

[0018] The method for producing the water-soluble polyalkylene oxide is not particularly limited, and for example, known methods can be widely adopted. A specific example is a method for producing a water-soluble polyalkylene oxide by polymerizing an alkylene oxide in the presence of an alkali or metal catalyst. Water-soluble polyalkylene oxides can also be obtained from commercial products, such as the "PEO" series from Sumitomo Seika Chemicals Co., Ltd., the "POLYOX" series from Dow Chemical Company, Ltd., the "Alkox" series from Meisei Chemical Industry Co., Ltd., or the "ZEOSPAN" series from Zeon Corporation.

[0019] When the water-soluble polyalkylene oxide is polypropylene oxide, the propylene oxide constituting the polypropylene oxide can usually have units derived from 1,2-propylene oxide or 1,3-propylene oxide, or can have both.

[0020] When the water-soluble polymer is a neutralized product of a (meth)acrylamide-(meth)acrylic acid copolymer, the degree of neutralization is not particularly limited, and is preferably 20 to 100%, and more preferably 40 to 100%.

[0021] The molecular weight of the water-soluble polymer is not particularly limited, and can be selected from an appropriate range depending on the purpose of use. For example, the viscosity average molecular weight of the water-soluble polymer is preferably 100,000 to 22,000,000, more preferably 200,000 to 15,000,000. In this case, even if water containing iron ions and oxidizing agents is used, it becomes easy to prepare an aqueous solution of the water-soluble polymer that is less likely to cause a decrease in viscosity, and it can be suitably used, for example, as a papermaking adhesive in papermaking applications.

[0022] In the present invention, the viscosity average molecular weight of a water-soluble polymer (excluding (meth)acrylamide homopolymers and neutralized (meth)acrylamide-(meth)acrylic acid copolymers) is calculated from the limiting viscosity measured using an Ostwald viscometer using the Staudinger formula. Specifically, the viscosity average molecular weight [M] of the water-soluble polymer is calculated from the limiting viscosity [η] measured using an Ostwald viscometer using the following Staudinger formula. [η]=6.4×10 -5 ×M 0.82 When calculating using the above formula, the solvent is set to pure water and the measurement temperature is set to 35°C.

[0023] When the water-soluble polymer is a homopolymer of (meth)acrylamide or a neutralized copolymer of (meth)acrylamide-(meth)acrylic acid, its viscosity average molecular weight (Mw) is calculated by dissolving the homopolymer of (meth)acrylamide or the neutralized copolymer of (meth)acrylamide-(meth)acrylic acid in a 1N aqueous solution of sodium nitrate, determining the intrinsic viscosity [η] at 30°C, and applying the following conversion formula: Intrinsic viscosity formula: [η]=3.73×10 -4 ×(Mw)×0.66 It is calculated using:

[0024] The viscosity of the water-soluble polymer aqueous solution is not particularly limited, and can be selected from an appropriate range depending on the purpose of use. For example, the viscosity of a 0.5% by mass aqueous solution of the water-soluble polymer at 25°C can be 10 to 4000 mPa·s, and the viscosity of a 5% by mass aqueous solution at 25°C can be 50 to 80,000 mPa.s. In these cases, even if water containing iron ions and oxidizing agents is used, it becomes easy to prepare a water-soluble polymer aqueous solution that is less likely to experience a decrease in viscosity, and the water-soluble polymer aqueous solution can be suitably used, for example, as a papermaking adhesive in papermaking applications.

[0025] In the present invention, the viscosity of a water-soluble polymer aqueous solution of a given concentration is measured using a B-type rotational viscometer. The measurement is performed by immersing a beaker containing a water-soluble polymer aqueous solution of a given concentration in a thermostatic bath at 25°C for at least 30 minutes, and then setting the viscometer rotation speed to 12 r / min and the measurement time to 3 minutes. The rotor to be used is rotor No. 1 when the viscosity of the measurement target is less than 500 mPa·s, rotor No. 2 when the viscosity of the measurement target is 500 mPa·s or more and less than 2,500 mPa·s, and rotor No. 3 when the viscosity of the measurement target is 2,500 mPa·s or more and less than 10,000 mPa·s.

[0026] The water-soluble polymer contained in the water-soluble polymer composition of the present invention may be one type or two or more types.

[0027] (Phenol-based antioxidant) The type of phenol-based antioxidant is not particularly limited, and for example, a wide variety of known phenol-based antioxidants can be used.

[0028] Specific examples of phenol-based antioxidants include dibutylhydroxytoluene (BHT), tocopherol (vitamin E), dibutylhydroxyanisole (BHA), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl ]-4,6-di-tert-pentylphenyl acrylate, 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, 3,9-bis[2-(3-(3-tert-butyl-4-hydroxy-5-methylphenyl)-propionyloxy)-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, etc. Other examples of phenolic antioxidants include various phenolic compounds sold under the product name "ADEKA STAB AO" series by ADEKA Corporation and various compounds sold under the product name "IRGANOX" series by BASF, which correspond to phenolic compounds.

[0029] Among them, the phenol-based antioxidant is preferably dibutylhydroxytoluene (BHT), tocopherol (vitamin E), etc. In this case, even if water containing iron ions and an oxidizing agent is used, it becomes easy to prepare an aqueous water-soluble polymer solution in which the viscosity is less likely to decrease.

[0030] The phenol-based antioxidant can be obtained, for example, by a known production method, and can also be obtained from commercial products.

[0031] The phenol-based antioxidant contained in the water-soluble polymer composition of the present invention may be one type or two or more types.

[0032] (Sulfur-containing amine compounds) The sulfur-containing amine compound is not particularly limited as long as it is an amine compound containing one or more sulfurs (S) in the molecule, and for example, a wide variety of known sulfur-containing amine compounds can be used.

[0033] Specific examples of the sulfur-containing amine compound include mercaptobenzimidazoles such as 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, 4-mercaptomethylbenzimidazole, 5-mercaptomethylbenzimidazole, and salts thereof (e.g., zinc salts, etc.); thiazoles such as 2-mercaptobenzothiazole, 2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole sodium salt, and 2-(4-morpholinyldithio)benzothiazole; thioureas such as ethylenethiourea, diethylthiourea, dibutylthiourea, dilaurylthiourea, diphenylthiourea, and trimethylthiourea; and tetramethylthiuramdithiourea. thiurams such as zinc sulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, dipentamethylenethiuram tetrasulfide, and tetramethylthiuram monosulfide; dithiocarbamate salts such as zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc ethylphenyldithiocarbamate, pentamethylenedithiocarbamic acid piperidine salt, diethyldithiocarbamate tellurium, dimethyldithiocarbamate sodium, diethyldithiocarbamate sodium, dibutyldithiocarbamate sodium, dibutyldithiocarbamate nickel, and N,N-diethyldithiocarbamate sodium trihydrate; isothiazoles, thiamine, mercaptobenzoxazole, and 1-phenyl-5-mercapto-1H-tetrazole.

[0034] Among them, the sulfur-containing amine compounds are preferably mercaptobenzimidazoles, thioureas, thiurams, dithiocarbamates and thiazoles, more preferably mercaptobenzimidazoles, thioureas and thiazoles, and even more preferably 2-mercaptobenzimidazole and 2-mercaptobenzothiazole. In these cases, even if water containing iron ions and oxidizing agents is used, it becomes easy to prepare a water-soluble polymer aqueous solution that is less likely to cause a decrease in viscosity, and it can be suitably used, for example, as a papermaking adhesive in papermaking applications.

[0035] The sulfur-containing amine compound can be obtained, for example, by a known production method, or can be obtained from a commercial product, etc. Examples of commercial products include the "Noccela" and "Nocrac" series of products manufactured by Ouchi Shinko Chemical Co., Ltd., the "Accel" and "Antage" series of products manufactured by Kawaguchi Chemical Industry Co., Ltd., and the "Suncera" series of products manufactured by Sanshin Chemical Industry Co., Ltd.

[0036] The sulfur-containing amine compound contained in the water-soluble polymer composition of the present invention may be one type or two or more types.

[0037] (Inorganic salts) The inorganic salt is not particularly limited as long as it is an inorganic salt other than a transition metal salt, and for example, a wide variety of known inorganic salts can be used. In addition, it is also preferable that the inorganic salt is an inorganic salt other than a hypochlorite.

[0038] The inorganic salt preferably exhibits neutrality or alkalinity in its aqueous solution state. Specifically, when the inorganic salt is prepared into a 4 mg / L aqueous solution, the aqueous solution preferably exhibits a pH of 7 or more (for example, 7 to 13). The pH is measured by the glass electrode method.

[0039] Specific examples of inorganic salts include carbonates such as potassium carbonate, lithium carbonate, sodium carbonate, magnesium carbonate, and sodium bicarbonate; silicates such as sodium silicate; phosphates such as trisodium phosphate; sulfates such as magnesium sulfate and sodium sulfate; sulfites such as sodium sulfite; thiosulfates such as sodium thiosulfate; chlorides such as calcium chloride and lithium chloride; bromides such as lithium bromide; iodides such as sodium iodide; sulfides such as sodium sulfide; hydrogen sulfides such as sodium hydrogen sulfide; nitrates such as sodium nitrate; and nitrites such as sodium nitrite.

[0040] Among these, the inorganic salt is preferably a carbonate salt. In this case, even if water containing iron ions and an oxidizing agent is used, it becomes easier to prepare an aqueous water-soluble polymer solution in which the occurrence of a decrease in viscosity over time is particularly likely to be suppressed.

[0041] The inorganic salt contained in the water-soluble polymer composition of the present invention may be of one type or of two or more types.

[0042] (Water-soluble polymer composition) As described above, the water-soluble polymer composition of the present invention contains at least a water-soluble polymer, a phenol-based antioxidant, a sulfur-containing amine compound, and an inorganic salt other than transition metal salts (sometimes simply referred to as "inorganic salt"). In particular, the water-soluble polymer composition of the present invention contains both a sulfur-containing amine compound and an inorganic salt, so that even if water containing iron ions and an oxidizing agent is used, the viscosity reduction is even less likely to occur, and furthermore, it is possible to prepare an aqueous water-soluble polymer solution in which the occurrence of viscosity reduction over time is particularly easily suppressed.

[0043] In the water-soluble polymer composition of the present invention, the content ratio of the water-soluble polymer, the phenolic antioxidant, the sulfur-containing amine compound and the inorganic salt can be selected within appropriate ranges depending on the purpose of the water-soluble polymer composition.

[0044] In particular, in the water-soluble polymer composition of the present invention, the content of the inorganic salt is preferably 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer, and the content of the sulfur-containing amine compound is preferably 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer. In this case, even if water containing iron ions and an oxidizing agent is used, viscosity reduction is particularly unlikely to occur, and further, it becomes easy to prepare an aqueous water-soluble polymer solution in which the occurrence of viscosity reduction over time is particularly likely to be suppressed.

[0045] In the water-soluble polymer composition of the present invention, the content of the inorganic salt is, relative to 100 parts by mass of the water-soluble polymer, preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.15 parts by mass or more, particularly preferably 0.2 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 2 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.5 parts by mass or less.

[0046] In the water-soluble polymer composition of the present invention, the content of the sulfur-containing amine compound is, relative to 100 parts by mass of the water-soluble polymer, preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.08 parts by mass or more, particularly preferably 0.09 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 2 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.5 parts by mass or less.

[0047] In the water-soluble polymer composition of the present invention, the content of the phenol-based antioxidant is preferably 0.001 to 5 parts by mass relative to 100 parts by mass of the water-soluble polymer. In the water-soluble polymer composition of the present invention, the content of the phenol-based antioxidant is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, even more preferably 0.08 parts by mass or more, particularly preferably 0.09 parts by mass or more, and preferably 5 parts by mass or less, more preferably 2 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.5 parts by mass or less, relative to 100 parts by mass of the water-soluble polymer.

[0048] In the water-soluble polymer composition of the present invention, the content ratio of the inorganic salt and the phenol-based antioxidant is not particularly limited. For example, the inorganic salt is preferably contained in an amount of 20 to 10,000 parts by mass, more preferably 40 to 1,000 parts by mass, further preferably 60 to 500 parts by mass, and particularly preferably 80 to 300 parts by mass, relative to 100 parts by mass of the phenol-based antioxidant.

[0049] In the water-soluble polymer composition of the present invention, the content ratio of the sulfur-containing amine compound and the phenol-based antioxidant is not particularly limited. For example, the sulfur-containing amine compound is preferably contained in an amount of 20 to 10,000 parts by mass, more preferably 40 to 1,000 parts by mass, further preferably 60 to 500 parts by mass, and particularly preferably 80 to 300 parts by mass, relative to 100 parts by mass of the phenol-based antioxidant.

[0050] In the water-soluble polymer composition of the present invention, the content (mixture) of the water-soluble polymer can be, for example, 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. In addition, in the water-soluble polymer composition of the present invention, the content (mixture) of the water-soluble polymer can be, for example, 99.99% by mass or less.

[0051] The water-soluble polymer composition of the present invention may also contain other ingredients so long as it contains a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt.

[0052] The other components can be selected from an appropriate range depending on the intended use of the water-soluble polymer composition, and examples thereof include antioxidants other than phenol-based antioxidants, ultraviolet absorbers, fillers, colorants (e.g., pigments and dyes), preservatives, rust inhibitors, surfactants, solvents (e.g., organic solvents), flow improvers (e.g., silica), viscosity modifiers (e.g., hydrophilic silica and water-soluble polymers), and electrolytes.The other components preferably do not contain transition metals, and preferably do not contain hypochlorite.The other components contained in the water-soluble polymer composition may be one type or two or more types.

[0053] When the water-soluble polymer composition contains other components, the content ratio of the other components (excluding the water-based solvent described below) is not particularly limited.For example, based on the total mass of the water-soluble polymer, the phenolic antioxidant, the sulfur-containing amine compound and the inorganic salt, it is 50 mass% or less, preferably 30 mass% or less, more preferably 10 mass% or less, further preferably 5 mass% or less, and particularly preferably 1 mass% or less.

[0054] The water-soluble polymer composition may be in a solid state or in a liquid state. When the water-soluble polymer composition is in a solid state, it may be in a powder, lump, granule, fiber, or the like, and when it is in a liquid state, it may be in the form of an aqueous solution, a dispersion, a paste, or the like, as described below. When the water-soluble polymer composition is in a liquid state other than an aqueous solution, for example, the type of solvent for dissolving or dispersing is not particularly limited, and an appropriate solvent can be selected according to the purpose.

[0055] The method of preparing the water-soluble polymer composition of the present invention is not particularly limited, and can be obtained by mixing a predetermined amount of water-soluble polymer, phenolic antioxidant, sulfur-containing amine compound, inorganic salt, and other components added as necessary.The mixing method is not particularly limited, and can be, for example, dry blending.In addition, as described later, when the water-soluble polymer composition is an aqueous solution, the water-soluble polymer composition of the present invention can also be prepared by using a predetermined kit.

[0056] The water-soluble polymer composition of the present invention contains at least a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt other than transition metal salts, so that even if water containing iron ions and oxidizing agents is used, the viscosity is less likely to decrease, and the viscosity decrease over time can be easily suppressed.For example, industrial water contains iron ions caused by iron rust on pipes, etc., and may also contain oxidizing agents such as bactericides and slime control agents for the purpose of improving water quality.Even if the aqueous solution of the water-soluble polymer composition of the present invention is prepared using such industrial water as a medium, the viscosity of the aqueous solution is less likely to decrease, and the viscosity decrease over time can be suppressed.

[0057] Therefore, the water-soluble polymer composition of the present invention is suitable for use in aqueous water-soluble polymer solutions, and is particularly suitable as a raw material for preparing aqueous water-soluble polymer solutions.

[0058] In addition, the water-soluble polymer composition of the present invention can be suitably used in various applications requiring a water-soluble polymer aqueous solution with suppressed viscosity reduction over time, specifically, it can be used as an industrial chemical in various industrial applications such as papermaking, mining, cement, and dyeing. Examples of industrial chemicals include papermaking thickeners, flocculants, dispersants, and sedimentation promoters, and among them, the water-soluble polymer composition of the present invention is particularly suitable for use as a papermaking thickener. Since the papermaking thickener or industrial chemical contains the water-soluble polymer composition of the present invention, viscosity reduction is even less likely to occur even when the thickener is prepared using water containing iron ions and an oxidizing agent.

[0059] When paper is produced using a papermaking adhesive containing the water-soluble polymer composition of the present invention, for example, the water-soluble polymer composition of the present invention is made into a powdery or granular form, which is mixed with water when used to prepare an aqueous solution of the water-soluble polymer, and the concentration is further adjusted so that when the paper stock is subjected to papermaking, the concentration of the water-soluble polymer in the aqueous dispersion containing the paper stock is, for example, about 1 to 5,000 ppm by mass.

[0060] 2.Aqueous solution An aqueous solution can be prepared using the water-soluble polymer composition of the present invention. Since such an aqueous solution contains the water-soluble polymer composition of the present invention and water, the viscosity is unlikely to decrease immediately after mixing the water-soluble polymer composition with water, and the occurrence of viscosity decrease over time is also suppressed. Hereinafter, the aqueous solution containing the water-soluble polymer composition of the present invention and water will be referred to as the "aqueous solution of the present invention."

[0061] In the aqueous solution of the present invention, various aqueous solvents can be used as the medium, including water and a mixed solvent of water and a lower alcohol compound. The lower alcohol compound is, for example, an alcohol compound having 1 to 3 carbon atoms. As the water, industrial water can be used, and various types of water such as distilled water, tap water, ion-exchanged water, deionized water, pure water, and electrolytic water can also be used.

[0062] The concentration of the water-soluble polymer in the aqueous solution of the present invention is not particularly limited. For example, the concentration of the water-soluble polymer based on the total mass of the aqueous solution can be 1 ppm by mass or more and 20% by mass or less.

[0063] As an embodiment of the aqueous solution of the present invention, for example, the aqueous solution of the present invention can further contain iron ions and an oxidizing agent. That is, as an embodiment of the aqueous solution of the present invention, an aqueous solution containing a water-soluble polymer composition, iron ions, an oxidizing agent, and water can be mentioned. The content of iron ions in such an aqueous solution is, for example, preferably 10 ppm by mass or less, more preferably 5 ppm by mass or less, further preferably 2 ppm by mass or less, and particularly preferably 1 ppm by mass or less, based on the total mass of the aqueous solution. The lower limit of the content of iron ions is not particularly limited, and can be, for example, 0.1 ppm by mass.

[0064] The oxidizing agent is not particularly limited, and examples thereof include hypochlorites such as sodium hypochlorite, potassium hypochlorite, calcium hypochlorite, and barium hypochlorite, chlorine dioxide, chlorinated isocyanuric acid, and combined chlorine type compounds. Examples of combined chlorine compounds include, but are not limited to, slime control agents such as the Crykiller series, Fuzzicide series, and Clinox series (Kurita Water Industries Ltd.), Somacide series, Curecide series (Somar Co., Ltd.), Tower Clear series (Kankyo Koken Co., Ltd.), Molnon series, SLC series (Katayama Nalco Co., Ltd.), Statect series, High Clean series (Nissin Chemical Research Institute Co., Ltd.), Bio Hope series, Biodan series, and Bio Ace series (Keiai Chemical Co., Ltd.), Neosintol series (Sumika Environmental Science Co., Ltd.), Amolden series (Daiwa Chemical Industry Co., Ltd.), Fineside series (Tokyo Fine Chemical Co., Ltd.), Slaclin series (Hakuto Co., Ltd.), Permakem series, Topside series (Permakem Asia Co., Ltd.), and Powerside series (Fuji Sangyo Co., Ltd.), which provide drug persistence and strong bactericidal properties. The oxidizing agent may be used alone or in combination of two or more kinds as long as the effect of the present invention is not impaired. The oxidizing agent may be added all at once, may be added in several portions, or may be added continuously.

[0065] When the aqueous solution of the present invention contains the oxidizing agent, the content of the oxidizing agent in the aqueous solution is, for example, preferably 10,000 mass ppm or less, more preferably 1,000 mass ppm or less, even more preferably 500 mass ppm or less, and particularly preferably 100 mass ppm or less, based on the total mass of the aqueous solution. The lower limit of the content of the oxidizing agent is not particularly limited, and can be, for example, 1 mass ppm.

[0066] The aqueous solution containing the water-soluble polymer composition, iron ions, an oxidizing agent, and water can be produced, for example, by a production method including a step of mixing the water-soluble polymer composition of the present invention with water containing iron ions and an oxidizing agent. The mixing method is not particularly limited, and for example, any known mixing means can be widely adopted.

[0067] The aqueous solution containing the water-soluble polymer composition, iron ions, an oxidizing agent, and water can also be produced using a kit. Such a kit can include, for example, a first agent containing a water-soluble polymer, a second agent containing an inorganic salt other than transition metal salts, and a third agent containing a sulfur-containing amine compound, and the content of the inorganic salt in the second agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent, and the content of the sulfur-containing amine compound in the third agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent.

[0068] The phenol-based antioxidant may be contained in any of the first agent, the second agent, and the third agent, and may be contained in the first agent, for example. In this case, the kit (hereinafter referred to as "kit A") includes a first agent containing a water-soluble polymer and a phenol-based antioxidant, a second agent containing an inorganic salt excluding transition metal salts, and a third agent containing a sulfur-containing amine compound. In this kit A as well, the content of the inorganic salt in the second agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent, and the content of the sulfur-containing amine compound in the third agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent.

[0069] The above-mentioned "aqueous solution containing a water-soluble polymer composition, iron ions, an oxidizing agent, and water" can be produced by using the kit A. For example, the aqueous solution can be produced by a production method (hereinafter referred to as production method 1) including a step of mixing the second agent, the third agent, and water containing iron ions and an oxidizing agent to obtain a mixed solution, and a step of mixing the mixed solution with the first agent.

[0070] In the production method 1, the mixing conditions in each step are not particularly limited, and the mixing means are also not particularly limited. For example, any known mixing means can be widely adopted.

[0071] Alternatively, the aqueous solution can be produced by a production method (hereinafter referred to as production method 2) including a step of mixing water containing iron ions and an oxidizing agent with the first agent to obtain a mixed solution, and a step of mixing the mixed solution, the second agent, and the third agent.

[0072] In the production method 2, the time from the start of mixing the water containing iron ions and an oxidizing agent with the first agent to the addition of the second agent and / or the third agent is preferably 0 to 120 minutes, more preferably 0 to 30 minutes. In this case, even if water containing iron ions and an oxidizing agent is used, a water-soluble polymer aqueous solution in which viscosity reduction is further unlikely to occur and the occurrence of viscosity reduction over time is particularly likely to be suppressed is easily obtained. In the production method 2, other mixing conditions are not particularly limited, and the mixing means is also not particularly limited, and for example, known mixing means can be widely adopted.

[0073] For example, paper can be produced using the aqueous solution of the present invention. Specifically, paper can be produced by a production method including a step of preparing an aqueous dispersion of the paper stock by mixing the aqueous solution of the present invention with a paper stock, and a step of making paper from the aqueous dispersion of the paper stock. The type of paper stock is not particularly limited, and for example, a wide range of known paper stocks can be exemplified. The papermaking method is also not particularly limited, and for example, a wide range of known papermaking means can be adopted.

[0074] In specifying the invention included in the present disclosure, the configurations (properties, structures, functions, etc.) described in each embodiment of the present disclosure may be combined in any manner. In other words, the present disclosure includes all subject matter consisting of all combinations of the configurations that can be combined as described in this specification. EXAMPLES

[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0076] (Preparation Example 1) 999.976 g of ion-exchanged water and 23.2 mg of iron(II) chloride (Strohm Chemicals, purity 98%) were placed in a 1000 mL plastic beaker and stirred with a magnetic stirrer for 1 hour, thereby obtaining 1000 g of an aqueous solution with an iron(II) ion concentration of 10 ppm by mass.

[0077] (Preparation Example 2) 99.047 g of ion-exchanged water and 0.953 g of sodium hypochlorite (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) with an effective chlorine concentration of 10.39% by mass as an oxidizing agent were placed in a 100 mL measuring flask and shaken well to obtain 100 g of an aqueous solution with a hypochlorite ion concentration of 1000 ppm by mass.

[0078] (Reference example 1) 0.999 g of polyethylene oxide having a viscosity average molecular weight of 8 million and 0.001 g of dibutylhydroxytoluene (BHT) as a phenolic antioxidant were dry-blended to obtain polymer raw material (1). Next, 499,000 g of ion-exchanged water was placed in a 1000 mL plastic beaker, and 1,000 g of the polymer raw material (1) was added while stirring with a flat plate (width 80 mm, length 25 mm) at a tip peripheral speed of 1.0 m / s, and stirring was continued for 3 hours under the same stirring conditions. In this way, a test aqueous solution (1) was produced.

[0079] (Reference example 2) 0.999 g of polyacrylamide and 0.001 g of BHT were dry-blended to obtain polymer raw material (2). Next, 499,000 g of ion-exchanged water was placed in a 1000 mL plastic beaker, and 1,000 g of polymer raw material (2) was added while stirring with a flat plate (width 80 mm, length 25 mm) at a tip speed of 1.0 m / s, and stirring was continued for 3 hours under the same stirring conditions. In this way, test aqueous solution (2) was produced.

[0080] (Reference example 3) A mixture of 0.4995 g of polyethylene oxide and 0.4995 g of polyacrylamide, each having a viscosity average molecular weight of 8,000,000, was dry-blended with 0.001 g of BHT to obtain polymer raw material (3). Next, 499,000 g of ion-exchanged water was placed in a 1000 mL plastic beaker, and 1,000 g of the polymer raw material (3) was added while stirring with a flat plate (width 80 mm, length 25 mm) at a tip peripheral speed of 1.0 m / s, and stirring was continued for 3 hours under the same stirring conditions. Thus, a test aqueous solution (3) was produced.

[0081] Example 1 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT as a phenolic antioxidant, 0.002 g of lithium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzimidazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (1). Separately, an aqueous medium was prepared by mixing 447,000 g of ion-exchanged water, 50,000 g of the aqueous solution obtained in Preparation Example 1, and 2,000 g of the aqueous solution obtained in Preparation Example 2 in a 1000 mL plastic beaker. While stirring this aqueous medium with a flat plate (width 80 mm, length 25 mm) at a tip peripheral speed of 1.0 m / s, 1,000 g of the water-soluble polymer composition (1) was added, and stirring was continued for 3 hours under the same stirring conditions. In this way, a water-soluble polymer aqueous solution was produced. Such a water-soluble polymer aqueous solution was designated as water-soluble polymer aqueous solution (1).

[0082] Example 2 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT as a phenolic antioxidant, 0.002 g of sodium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzothiazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (2). Except for using this water-soluble polymer composition (2) instead of the water-soluble polymer composition (1), an aqueous water-soluble polymer solution was produced under the same conditions as in Example 1. Such an aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (2).

[0083] Example 3 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT as a phenolic antioxidant, 0.002 g of lithium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzothiazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (3). Except for using this water-soluble polymer composition (3) instead of the water-soluble polymer composition (1), an aqueous water-soluble polymer solution was produced under the same conditions as in Example 1. Such an aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (3).

[0084] Example 4 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT as a phenolic antioxidant, 0.002 g of sodium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzimidazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (4). Except for using this water-soluble polymer composition (4) instead of the water-soluble polymer composition (1), an aqueous water-soluble polymer solution was produced under the same conditions as in Example 1. Such an aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (4).

[0085] Example 5 Mixture (5) was prepared by dry blending 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000 and 0.001 g of BHT as a phenolic antioxidant. Separately, 447.000 g of ion-exchanged water, 50.000 g of the aqueous solution obtained in Preparation Example 1, and 2.000 g of the aqueous solution obtained in Preparation Example 2 were mixed in a 1000 mL plastic beaker to prepare an aqueous medium. This aqueous medium was stirred with a flat plate (width 80 mm, length 25 mm) at a tip speed of 1.0 m / s, while adding 0.002 g of lithium carbonate as an inorganic salt and 0.001 g of 2-mercaptobenzimidazole as a sulfur-containing amine compound and stirring for 30 minutes, and further adding 0.997 g of the mixture (5) obtained above and continuing stirring for 3 hours under the same stirring conditions to produce an aqueous water-soluble polymer solution. This aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (5).

[0086] Example 6 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of tocopherol as a phenolic antioxidant, 0.002 g of lithium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzimidazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (6). Except for using this water-soluble polymer composition (6) instead of the water-soluble polymer composition (1), an aqueous water-soluble polymer solution was produced under the same conditions as in Example 1. Such an aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (6).

[0087] Example 7 0.996 g of polyacrylamide, 0.001 g of BHT as a phenolic antioxidant, 0.002 g of lithium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzimidazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (7). Except for using this water-soluble polymer composition (7) instead of the water-soluble polymer composition (1), an aqueous water-soluble polymer solution was produced under the same conditions as in Example 1. Such an aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (7).

[0088] Example 8 0.498 g of polyethylene oxide having a viscosity average molecular weight of 8 million, 0.498 g of polyacrylamide, 0.001 g of BHT as a phenolic antioxidant, 0.002 g of lithium carbonate as an inorganic salt, and 0.001 g of 2-mercaptobenzothiazole as a sulfur-containing amine compound were dry-blended to produce a water-soluble polymer composition (8). Except for using this water-soluble polymer composition (8) instead of the water-soluble polymer composition (1), an aqueous water-soluble polymer solution was produced under the same conditions as in Example 1. This aqueous water-soluble polymer solution was designated as aqueous water-soluble polymer solution (8).

[0089] Example 9 Mixture (9) was produced by dry blending 0.996 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000 and 0.001 g of BHT as a phenolic antioxidant. Separately, 447.000 g of ion-exchanged water, 50.000 g of the aqueous solution obtained in Preparation Example 1, and 2.000 g of the aqueous solution obtained in Preparation Example 2 were mixed in a 1000 mL plastic beaker to prepare an aqueous medium. While stirring this aqueous medium using a flat plate (width 80 mm, length 25 mm) at a tip peripheral speed of 1.0 m / s, 0.997 g of the mixture (9) obtained above was added, and stirring was continued for 30 minutes under the same stirring conditions. Thereafter, 0.002 g of lithium carbonate as an inorganic salt and 0.001 g of 2-mercaptobenzothiazole as a sulfur-containing amine compound were added and stirred for 1 hour to produce an aqueous water-soluble polymer solution. This aqueous water-soluble polymer solution was designated as the aqueous water-soluble polymer solution (9).

[0090] Comparative Example 1 0.999 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000 and 0.001 g of BHT were dry blended to produce a mixture (1a). An aqueous water-soluble polymer solution was produced under the same conditions as in Example 1, except that this mixture (1a) was used in place of the water-soluble polymer composition (1).

[0091] Comparative Example 2 0.997 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT, and 0.002 g of lithium carbonate were dry blended to produce a mixture (2a). Separately, an aqueous medium was prepared by mixing 497,000 g of ion-exchanged water and 2,000 g of the aqueous solution obtained in Preparation Example 2 in a 1000 mL plastic beaker. While stirring this aqueous medium using a flat plate (width 80 mm, length 25 mm) at a tip speed of 1.0 m / s, 1,000 g of mixture (2a) was added, and stirring was continued for 3 hours under the same stirring conditions. This produced an aqueous water-soluble polymer solution.

[0092] Comparative Example 3 0.997 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT, and 0.002 g of sodium carbonate were dry blended to produce a mixture (3a). An aqueous water-soluble polymer solution was produced under the same conditions as in Comparative Example 2, except that this mixture (3a) was used in place of mixture (2a).

[0093] Comparative Example 4 0.997 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT, and 0.002 g of lithium carbonate were dry blended to produce a mixture (4a). An aqueous water-soluble polymer solution was produced under the same conditions as in Example 1, except that this mixture (4a) was used in place of the water-soluble polymer composition (1).

[0094] Comparative Example 5 0.997 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT, and 0.002 g of sodium carbonate were dry blended to produce a mixture (5a). An aqueous water-soluble polymer solution was produced under the same conditions as in Example 1, except that this mixture (5a) was used in place of the water-soluble polymer composition (1).

[0095] Comparative Example 6 0.998 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT, and 0.001 g of 2-mercaptobenzimidazole were dry blended to produce a mixture (6a). An aqueous water-soluble polymer solution was produced under the same conditions as in Example 1, except that this mixture (6a) was used in place of the water-soluble polymer composition (1).

[0096] Comparative Example 7 0.998 g of polyethylene oxide having a viscosity average molecular weight of 8,000,000, 0.001 g of BHT, and 0.001 g of 2-mercaptobenzothiazole were dry blended to produce a mixture (7a). An aqueous water-soluble polymer solution was produced under the same conditions as in Example 1, except that this mixture (7a) was used in place of the water-soluble polymer composition (1).

[0097] (Method for measuring the viscosity of aqueous solution immediately after production) The viscosity of the aqueous solutions obtained in each of the Examples, Comparative Examples, and Reference Examples immediately after production was measured using a B-type rotational viscometer (manufactured by Tokimec Corporation, rotor No. 1, measurement conditions: rotation speed 30 rpm, 3 minutes) (however, rotor No. 2 was used in Reference Examples 2 and 3 and Examples 7 and 9). Specifically, 150 g of the aqueous solution immediately after production was placed in a 200 mL glass container and kept in a sealed state in a thermostatic water bath (manufactured by Thomas Chemical Instruments, T-23Z) in an environment of 25°C for 15 minutes, and then the viscosity of the aqueous solution was measured.

[0098] (Method for measuring aqueous solution viscosity after 3 hours) 150 g of the aqueous solution obtained in each of the Examples, Comparative Examples, and Reference Examples immediately after production was stored in a sealed state for 3 hours at 25° C. The viscosity of the aqueous solution was measured in the same manner as that of the aqueous solution immediately after production, except that the aqueous solution after storage for 3 hours was used.

[0099] (Method for measuring aqueous solution viscosity after 24 hours) 150 g of the aqueous solution obtained in each of the Examples, Comparative Examples, and Reference Examples immediately after production was stored in a sealed state for 24 hours at 25° C. The viscosity of the aqueous solution was measured in the same manner as that of the aqueous solution immediately after production, except that the aqueous solution after storage for 24 hours was used.

[0100] (Method 1 for calculating viscosity retention rate) For Examples 1 to 6 and 9 and Comparative Examples 1 to 7 in which polyethylene oxide was used as the water-soluble polymer, the viscosity retention rate (%) was calculated based on the viscosity of the test aqueous solution (1) produced in Reference Example 1. That is, the viscosity retention rate (%) was calculated using the following formula (A1): S(%)=(X / Ya)×100 (A1) (Here, S is the viscosity retention rate, Ya is the viscosity [mPa s] of the test aqueous solution (1) obtained in Reference Example 1, and X is the viscosity [mPa s] of the aqueous solutions obtained in the Examples and Comparative Examples immediately after production, after storage for 3 hours, or after storage for 24 hours.) The calculation was made as follows.

[0101] (Method 2 for calculating viscosity retention rate) For Example 7 in which polyacrylamide was used as the water-soluble polymer, the viscosity retention rate (%) was calculated based on the viscosity of the test aqueous solution (2) produced in Reference Example 2. That is, the viscosity retention rate (%) was calculated according to the following formula (A2): S(%)=(X / Yb)×100 (A2) (Here, S is the viscosity retention rate, Yb is the viscosity [mPa s] of the test aqueous solution (2) obtained in Reference Example 2, and X is the viscosity [mPa s] of the aqueous solution obtained in the Examples immediately after production, after storage for 3 hours, or after storage for 24 hours.) The calculation was made as follows.

[0102] (Method 3 for calculating viscosity retention rate) For Example 8, in which a mixture of polyethylene oxide and polyacrylamide was used as the water-soluble polymer, the viscosity retention rate (%) was calculated based on the viscosity of the test aqueous solution (3) produced in Reference Example 3. That is, the viscosity retention rate (%) was calculated using the following formula (A3): S(%)=(X / Yc)×100 (A3) (Here, S is the viscosity retention rate, Yc is the viscosity [mPa s] of the test aqueous solution (3) obtained in Reference Example 3, and X is the viscosity [mPa s] of the aqueous solution obtained in the Examples immediately after production, after storage for 3 hours, or after storage for 24 hours.) The calculation was made as follows.

[0103] As can be seen from formulas (A1), (A2), and (A3) in the above viscosity retention calculation methods 1 to 3, the larger the viscosity retention value, the less likely the viscosity to decrease, and the larger the viscosity retention value after storage for 3 hours or after storage for 24 hours, the less likely the viscosity to decrease over time.

[0104] [Table 1]

[0105] Table 1 shows the aqueous solution viscosity and viscosity retention immediately after production, after 3 hours storage, and after 24 hours storage of the aqueous solutions obtained in each of the Examples, Comparative Examples, and Reference Examples. In Table 1, "0h" means immediately after production, "3h" means after 3 hours storage, and "24h" means after 24 hours storage.

[0106] From Table 1, it is demonstrated that the water-soluble polymer composition containing a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt other than a transition metal salt suppresses a decrease in viscosity even when water containing iron ions and hypochlorite ions is used, and furthermore, the occurrence of a decrease in viscosity over time is also suppressed.

[0107] As can be seen from Reference Examples 1 to 3, the viscosity of the water-soluble polymer aqueous solution does not decrease even when water containing no iron ions and / or hypochlorite ions is used, which indicates that the viscosity decrease observed in the water-soluble polymer aqueous solution of the Comparative Example is caused by iron ions and / or hypochlorite ions. [Industrial Applicability]

[0108] According to the water-soluble polymer composition of the present invention, it is possible to prepare a water-soluble polymer aqueous solution which is unlikely to cause a decrease in viscosity even when water containing iron ions and oxidizing agents is used, and which is also capable of suppressing the occurrence of a decrease in viscosity over time. The water-soluble polymer aqueous solution thus obtained is considered to be capable of contributing to the improvement of the efficiency of the manufacturing process and the reduction of the environmental load in various industrial chemical applications, such as easily producing uniform paper in papermaking applications.

Claims

1. A water-soluble polymer composition comprising a water-soluble polymer, a phenolic antioxidant, a sulfur-containing amine compound, and an inorganic salt excluding transition metal salts.

2. the content of the inorganic salt is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer, 2. The water-soluble polymer composition according to claim 1, wherein the content of the sulfur-containing amine compound is 0.001 to 10 parts by mass based on 100 parts by mass of the water-soluble polymer.

3. The water-soluble polymer composition according to claim 1, wherein the water-soluble polymer is at least one polymer selected from the group consisting of a homopolymer of (meth)acrylamide, a neutralized product of a (meth)acrylamide-(meth)acrylic acid copolymer, polyethylene oxide, polypropylene oxide, and an ethylene oxide-propylene oxide copolymer.

4. The water-soluble polymer composition according to claim 1 , wherein the inorganic salt is neutral or alkaline in its aqueous solution.

5. 2. The water-soluble polymer composition according to claim 1, wherein the content of the phenol-based antioxidant is 0.001 to 5 parts by mass based on 100 parts by mass of the water-soluble polymer.

6. 2. The water-soluble polymer composition according to claim 1, wherein the inorganic salt is contained in an amount of 20 to 10,000 parts by mass based on 100 parts by mass of the phenol-based antioxidant.

7. 2. The water-soluble polymer composition according to claim 1, wherein the sulfur-containing amine compound is contained in an amount of 20 to 10,000 parts by mass based on 100 parts by mass of the phenol-based antioxidant.

8. An aqueous solution comprising the water-soluble polymer composition according to any one of claims 1 to 7 and water.

9. 9. The aqueous solution according to claim 8, comprising iron ions and an oxidizing agent.

10. An industrial chemical comprising the water-soluble polymer composition according to any one of claims 1 to 7.

11. A papermaking adhesive comprising the water-soluble polymer composition according to any one of claims 1 to 7.

12. A method for producing the aqueous solution according to claim 9, comprising the steps of: A method of manufacturing comprising the step of mixing the water-soluble polymer composition with water containing iron ions and an oxidizing agent.

13. a first agent including a water-soluble polymer and a phenol-based antioxidant; a second agent containing an inorganic salt excluding transition metal salts; A third agent containing a sulfur-containing amine compound is provided, the content of the inorganic salt in the second agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent, and the content of the sulfur-containing amine compound in the third agent is 0.001 to 10 parts by mass relative to 100 parts by mass of the water-soluble polymer in the first agent.

14. A method for producing an aqueous solution using the kit according to claim 13, comprising the steps of: A step of mixing the second agent, the third agent, and water containing iron ions and an oxidizing agent to obtain a mixed solution; mixing the mixed solution with the first agent; The method for producing an aqueous solution comprises the steps of:

15. A method for producing an aqueous solution using the kit according to claim 13, comprising the steps of: A step of mixing water containing iron ions and an oxidizing agent with the first agent to obtain a mixed solution, and a step of mixing the mixed solution with the second agent and the third agent; The method for producing an aqueous solution comprises the steps of:

16. A step of preparing an aqueous dispersion of the paper stock by mixing the aqueous solution according to claim 8 with the paper stock; A step of making paper from the aqueous dispersion of the paper stock; A method for producing paper comprising the steps of:

Citation Information

Patent Citations

  • Polyalkylene oxide composition

    WO2017104496A1

  • Water-soluble polymer composition

    WO2021241662A1