Method for producing lithium-containing solution

By employing controlled elution steps and a manganese oxidation process with high and low concentration lithium solutions, the method enhances lithium content and reduces solution usage, addressing the cost limitations of existing lithium production methods.

JP2024146087AActive Publication Date: 2024-10-15SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023058800
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing methods for producing lithium-containing solutions require the addition of large amounts of acid to adjust hydrogen ion concentration, limiting the reduction of the amount of solution used after the elution process and increasing manufacturing costs.

Method used

A method involving multiple elution steps with controlled hydrogen ion concentrations, use of high and low concentration lithium elution solutions, and a manganese oxidation step to enhance lithium content and reduce solution usage, including a water washing step to recover discarded lithium.

Benefits of technology

This approach efficiently reduces the amount of acid and eluent solution used, increases lithium content, and lowers manufacturing costs by optimizing elution and oxidation processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146087000001_ABST
    Figure 2024146087000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a lithium-containing solution, which can suppress a production cost for producing lithium, by increasing a lithium content of a solution after an elution step, and reducing a quantity of the solution in a step after the elution step.SOLUTION: The method for producing the lithium-containing solution includes: an adsorption step; an elution step of bringing lithium manganate after the adsorption into contact with an acid-containing solution and obtaining an elution solution; and a manganese oxidation step, which are carried out in this order. The elution step includes: a first elution step in which an H+ concentration of the acid-containing solution is high; and a second elution step in which the H+ concentration of the acid-containing solution is lower than that in the first elution step. The second elution step is performed after the first elution step. According to this constitution, the elution is efficiently performed in the first elution step; the amount of acid added to the acid-containing solution can be reduced because the hydrogen ion concentration of the acid-containing solution does not need to be increased in the second elution step; and the amount of the elution solution to be used in the manganese oxidation step can be reduced.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a lithium-containing solution. More specifically, the present invention relates to a method for producing a lithium-containing solution that can reduce the production cost for lithium production by increasing the lithium content in the solution after an elution step and reducing the amount of the solution used in the step after the elution step. [Background technology]

[0002] Lithium manganese oxide (LiMn2O4, Li 1.33 Mn 1.67 O4, Li 1.6 Mn 1.6 λ-MnO2 (HMn2O4, HO4, etc.) is obtained by contacting mineral acids such as hydrochloric acid with 1.33 Mn 1.67 O4, H 1.6 Mn 1.6 It is known that λ-MnO2 (such as λ-MnO4) selectively adsorbs lithium. When this λ-MnO2 is used for lithium recovery, it has the advantage that the amount of neutralizing agent used in lithium recovery can be significantly reduced because λ-MnO2 does not adsorb impurities. For this reason, commercial use of this method is expected. A method for producing a lithium-containing solution using this λ-MnO2 is disclosed in Patent Document 1.

[0003] In the method for producing a lithium-containing solution of Patent Document 1, an acid-containing solution used in the elution step is added to the total amount of the elution solution obtained in the elution step to adjust the hydrogen ion concentration of the acid-containing solution, thereby reducing the amount of the elution solution used in the steps after the elution step. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 210847 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the acid-containing solution requires the addition of acid to adjust the hydrogen ion concentration to a predetermined value, and if a large amount of acid is added, there is a problem in that the effect of reducing the amount of solution used in the process after the elution solution is limited.

[0006] In view of the above circumstances, an object of the present invention is to provide a method for producing a lithium-containing solution that can reduce the production cost for lithium production by increasing the lithium content in the solution after the elution step and reducing the amount of the solution used in the step after the elution step. [Means for solving the problem]

[0007] The method for producing a lithium-containing solution of the first invention includes an adsorption step of bringing a low-concentration lithium-containing solution into contact with a lithium adsorbent obtained from lithium manganate to obtain an adsorbed lithium manganate, an elution step of bringing the adsorbed lithium manganate into contact with an acid-containing solution to obtain an elution solution, and a manganese oxidation step of adding an oxidizing agent and a pH adjuster to the elution solution to oxidize manganese and obtain a lithium-containing solution with a reduced manganese concentration, in this order, and the elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, and the second elution step is performed after the first elution step. The method for producing a lithium-containing solution of the second invention is characterized in that, in the first invention, the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less. A third aspect of the present invention is a method for producing a lithium-containing solution according to the first aspect of the present invention, characterized in that, in the elution step, the elution solution is separated into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution having a lower lithium concentration than that of the high-concentration lithium elution solution, the acid-containing solution used in the elution step contains the low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step contains the high-concentration lithium elution solution. A fourth aspect of the present invention is a method for producing a lithium-containing solution according to the third aspect of the present invention, wherein the high-concentration lithium elution solution is an elution solution obtained by extracting a predetermined volume of the elution solution obtained through the elution step based on a start of obtaining the elution solution. The manufacturing method of a lithium-containing solution of a fifth invention is characterized in that, in the third invention, the high-concentration lithium elution solution is the elution solution obtained between a predetermined start time and an end time after the start of the elution step. The method for producing a lithium-containing solution of a sixth invention is characterized in that, in the first invention, a water-washing step for washing an eluted lithium adsorbent obtained after the elution step is provided after the elution step, and a post-washing liquid obtained in the water-washing step is added to the acid-containing solution. Effect of the Invention

[0008] According to the first invention, the elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, and the second elution step is performed after the first elution step, so that the elution is efficiently performed in the first elution step, and since it is not necessary to increase the hydrogen ion concentration of the acid-containing solution in the second elution step, the amount of acid added to the acid-containing solution can be reduced, and the amount of elution solution used in the manganese oxidation step can be reduced, thereby reducing the production cost for lithium production. According to the second invention, the hydrogen ion concentration of the acid-containing solution in the first elution step and the hydrogen ion concentration of the acid-containing solution in the second elution step are predetermined values, whereby dissolution of manganese from the lithium adsorbent can be suppressed and the efficiency of elution can be increased. According to the third invention, the high-concentration lithium elution solution is contained in the elution solution used in the manganese oxidation step, so that the lithium content of the elution solution used in the manganese oxidation step can be increased. Also, since only the low-concentration lithium elution solution is added to the acid-containing solution, the hydrogen ion concentration in the acid-containing solution can be increased by adding only a small amount of acid, and as a result, the amount of the acid-containing solution can be further reduced, and the amount of the elution solution used in the manganese oxidation step can be reduced. According to the fourth invention, the high-concentration lithium elution solution is an elution solution obtained by extracting a predetermined volume based on the start of obtaining the elution solution, so that the lithium content of the high-concentration lithium elution solution can be increased. According to the fifth aspect of the present invention, the high-concentration lithium elution solution is an elution solution obtained between a predetermined start time and end time after the start of the elution step, and therefore the high-concentration lithium elution solution can be easily obtained. According to the sixth aspect of the present invention, the post-wash liquid obtained in the water-washing step is added to the acid-containing solution, whereby lithium that would otherwise have to be discarded in the water-washing step can be recovered. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a flow diagram of a method for producing a lithium-containing solution according to a first embodiment of the present invention. [Diagram 2] FIG. 5 is a flow diagram of a method for producing a lithium-containing solution according to a second embodiment of the present invention. [Diagram 3] FIG. 11 is a flow diagram of a method for producing a lithium-containing solution according to a third embodiment of the present invention. [Figure 4] FIG. 11 is a flow diagram of a method for producing a lithium-containing solution according to a fourth embodiment of the present invention. [Diagram 5]3 is a graph showing a lithium concentration for each predetermined volume fraction, based on the start of obtaining an elution solution in the method for producing a lithium-containing solution in FIG. 2. [Figure 6] 4 is a graph showing the lithium concentration for each predetermined volume fraction, based on the start of obtaining the solution after washing with water, in the method for producing the lithium-containing solution in FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, an embodiment of the present invention will be described with reference to the drawings. However, the embodiment described below is merely an example of a method for producing a lithium-containing solution to embody the technical concept of the present invention, and the present invention does not limit the method for producing a lithium-containing solution to the following.

[0011] The method for producing a lithium-containing solution according to the present invention includes an adsorption step of bringing a low-concentration lithium-containing solution into contact with a lithium adsorbent obtained from lithium manganate to obtain an adsorbed lithium manganate, an elution step of bringing the adsorbed lithium manganate into contact with an acid-containing solution to obtain an elution solution, and a manganese oxidation step of adding an oxidizing agent and a pH adjuster to the elution solution to oxidize manganese and obtain a lithium-containing solution with a reduced manganese concentration, in this order, and the elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, and the second elution step is performed after the first elution step.

[0012] The elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step. By carrying out the second elution step after the first elution step, elution is carried out efficiently in the first elution step, and since there is no need to increase the hydrogen ion concentration of the acid-containing solution in the second elution step, the amount of acid added to the acid-containing solution can be reduced, and the amount of elution solution used in the manganese oxidation step can be reduced, thereby reducing the production costs for lithium production.

[0013] It is also preferable that the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less. This embodiment can suppress dissolution of manganese from the lithium adsorbent and can increase the efficiency of elution.

[0014] In addition, the elution solution is separated into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution containing a lower concentration of lithium than the high-concentration lithium elution solution in the elution step, and the acid-containing solution used in the elution step includes the low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step preferably includes the high-concentration lithium elution solution. This embodiment makes it possible to increase the lithium content of the elution solution used in the manganese oxidation step. In addition, since only the low-concentration lithium elution solution is added to the acid-containing solution, the hydrogen ion concentration in the acid-containing solution can be increased by simply adding a small amount of acid, and as a result, the amount of the acid-containing solution can be further reduced, and the amount of the elution solution used in the manganese oxidation step can be reduced.

[0015] In addition, the high-concentration lithium elution solution is preferably an elution solution obtained by extracting a predetermined volume of the elution solution obtained through the elution step based on the start of the elution solution being obtained. This embodiment allows the lithium content of the high-concentration lithium elution solution to be high.

[0016] In addition, the high-concentration lithium elution solution is preferably the elution solution obtained between a predetermined start time and a predetermined end time after the start of the elution step. With this embodiment, the high-concentration lithium elution solution can be easily obtained.

[0017] In addition, it is preferable that a water washing step for washing the eluted lithium adsorbent obtained after the elution step is provided after the elution step, and the post-washing liquid obtained in the water washing step is added to the acid-containing solution. With this embodiment, it is possible to recover lithium that would otherwise have to be discarded in the water washing step.

[0018] (First embodiment) (Pre-adsorption process) In the adsorption step, a low-concentration lithium-containing solution is brought into contact with a lithium adsorbent to obtain lithium manganate after adsorption. A method for obtaining a lithium adsorbent used in this adsorption step will be described. Note that FIG. 1 shows a flow diagram of a method for producing a lithium-containing solution according to a first embodiment of the present invention, and the explanation of the "pre-adsorption step" will be given in the H 1.6 Mn 1.6 This is the stage where O4 is obtained.

[0019] Lithium manganate becomes a lithium adsorbent by acid treatment as shown in formula 1. In formula 1, lithium manganate is Li 1.6 Mn 1.6 Although it is expressed as O4, lithium manganese oxide is not limited to this. For example, Li 1.33 Mn 1.67 O4 can also be used, i.e. lithium manganate is Li 1.6 Mn 1.6 If O4, the lithium adsorbent is H 1.6 Mn 1.6 O4, but lithium manganese oxide, for example, Li 1.33 Mn 1.67 If O4, the lithium adsorbent is H 1.33 Mn 1.67 O4. Although the acid used in the acid treatment is HCl, it is not limited to this. For example, sulfuric acid, nitric acid, etc. can also be used.

[0020] The shape of lithium manganate is determined by considering the adsorption of lithium in the adsorption process. For example, lithium manganate can be in various shapes such as powder, granulated powder, or sprayed onto the fibers of a column. When the acid treatment is performed, for example, H 1.6 Mn 1.6 O4 is obtained. The shape of the lithium adsorbent is the same as that of the lithium manganese oxide before the acid treatment.

[0021] [Number 1] Li 1.6 Mn 1.6 O4+1.6HCl→H 1.6 Mn 1.6 O4+1.6LiCl

[0022] (Adsorption process) 1 shows a flow diagram of a method for producing a lithium-containing solution according to a first embodiment of the present invention. In the adsorption step, a low-concentration lithium-containing solution is brought into contact with a lithium adsorbent to obtain adsorbed lithium manganate by an ion exchange reaction between H and Li shown in Equation 2. In this specification, the lithium manganate obtained in the adsorption step is sometimes referred to as adsorbed lithium manganate.

[0023] [Number 2] H 1.6 Mn 1.6 O4+1.6LiCl→Li 1.6 Mn 1.6 O4+1.6HCl

[0024] The low-concentration lithium-containing solution is, for example, seawater or salt lake brine. For example, seawater contains an average of 0.17 ppm lithium. However, in addition to lithium, elements such as sodium, magnesium, and calcium are dissolved in these low-concentration lithium-containing solutions. According to the method for producing a lithium-containing solution of the present invention, it is possible to selectively recover lithium from the low-concentration lithium-containing solution in which these elements are dissolved. Note that the low-concentration lithium-containing solution means that the amount of lithium per unit volume is smaller, i.e., the lithium concentration is lower, compared to the lithium-containing solution described below.

[0025] In the adsorption process, the contact method between the low-concentration lithium-containing solution and the adsorbent differs depending on the shape of the adsorbent. For example, when the adsorbent is powdery, a predetermined amount of the adsorbent is put into the low-concentration lithium-containing solution and stirred for a predetermined time, so that the low-concentration lithium-containing solution comes into contact with the adsorbent, and lithium is adsorbed to the adsorbent. When the adsorbent is particulate, a particulate adsorbent is sealed in a liquid passage container, and the low-concentration lithium-containing solution is passed through the liquid passage container, so that the low-concentration lithium-containing solution comes into contact with the adsorbent, and lithium is adsorbed to the adsorbent. When the adsorbent is sprayed onto the fibers of the column, the low-concentration lithium-containing solution passes through the column, so that the low-concentration lithium-containing solution comes into contact with the adsorbent, and lithium is adsorbed to the adsorbent. When the low-concentration lithium-containing solution is passed through the column, the low-concentration lithium-containing solution may be passed through repeatedly to ensure the number of times it comes into contact with the adsorbent.

[0026] After the adsorption process, the adsorbent becomes lithium manganese oxide after adsorption. The low-concentration lithium-containing solution becomes a post-adsorption liquid after lithium is adsorbed by the adsorbent. This post-adsorption liquid is discharged into the sea or lake from which the low-concentration lithium-containing solution was collected. At that time, the post-adsorption liquid is discharged after being treated, such as neutralized, to make it suitable for discharge.

[0027] (Elution step) In the elution step, the lithium manganate after adsorption is contacted with an acid-containing solution to obtain an elution solution by the reaction shown in Equation 3. At this time, the lithium manganate after adsorption is Li + and H + Through this exchange reaction between cations, the lithium adsorbent is regenerated as a lithium adsorbent, and this lithium adsorbent is reused in the adsorption step.

[0028] [Number 3] Li 1.6 Mn 1.6 O4+1.6HCl→H 1.6 Mn 1.6 O4+1.6LiCl

[0029] In this embodiment, the acid-containing solution includes a solution of an acid alone such as hydrochloric acid, and an elution solution obtained by adding an acid to the elution solution obtained by one elution step. For example, in this embodiment, the elution step is divided into a plurality of steps such as a first elution step and a second elution step. The first elution step is an elution step in which the hydrogen ion concentration of the acid-containing solution is relatively high, and the second elution step is an elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step. For example, in the initial stage of the first elution step, the acid-containing solution is a solution of an acid alone, and the subsequent one can be made to have a predetermined hydrogen ion concentration by adding an acid to the elution solution obtained in the previous stage. In this case, in the second elution step, the acid is added to the elution solution obtained in the previous stage. Also, the acid-containing solution in the first elution step can be only a solution of an acid alone, and the acid-containing solution in the second elution step can be made to have an acid added to the elution solution obtained in the previous stage.

[0030] The reaction shown in Equation 3 proceeds better as the pH value of the acid-containing solution used in the elution step is smaller. However, when the reaction shown in Equation 3 proceeds to a certain extent, the pH value of the acid-containing solution increases, and the reaction shown in Equation 3 no longer proceeds. In Patent Document 1, International Publication No. 2022 / 210847, in order to prevent this state from being reached, the elution step is divided into multiple stages, and in the second stage of the multiple stages and thereafter, the elution solution obtained in the previous stage was used as the acid-containing solution by adding acid. However, at this time, the acid was supplied so as to have the same pH as the acid-containing solution supplied initially, so that the amount of the elution solution was limited.

[0031] The elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step. By carrying out the second elution step after the first elution step, elution is carried out efficiently in the first elution step, and since there is no need to increase the hydrogen ion concentration of the acid-containing solution in the second elution step, the amount of acid added to the acid-containing solution can be reduced, and the amount of elution solution used in the manganese oxidation step can be reduced, thereby reducing the production costs for lithium production.

[0032] If the lithium content of the elution solution can be increased in this way, the size of the equipment in the subsequent process can be reduced, and the load of the process when obtaining lithium as a solid can be reduced. In other words, if the lithium content is increased, the amount of the lithium-containing solution itself can be reduced, so there is no need to increase the size of the equipment in the subsequent process. In addition, when obtaining lithium as a solid, the time for boiling the solution can be shortened, and the amount of the pH adjuster in the manganese oxidation process described below or the pH adjuster in the neutralization process provided after the manganese oxidation process can be reduced. This neutralization process is provided, for example, to remove magnesium. In addition, the solution containing lithium at a high concentration can be shipped to the customer as it is.

[0033] Although the elution step is divided into a plurality of steps, the elution step is not limited to this form. For example, the elution step may include a case in which an acid is continuously added to the elution solution to form an acid-containing solution.

[0034] In the elution step of this embodiment, i.e., the first elution step and the second elution step, the hydrogen ion concentration of the acid-containing solution that is contacted with the lithium manganate after adsorption is preferably 0.1 mol / L or more and 4.0 mol / L or less.Furthermore, the hydrogen ion concentration is preferably 0.25 mol / L or more and 2.0 mol / L or less.Furthermore, the hydrogen ion concentration is preferably 0.5 mol / L or more and 1.0 mol / L or less.

[0035] In this elution step, the hydrogen ion concentration of the acid-containing solution is 0.1 mol / L or more and 4.0 mol / L or less, so that Li + and H + The efficiency of the exchange reaction between cations can be maintained while suppressing the dissolution of the entire lithium manganate. In other words, the lithium adsorbent can be used repeatedly.

[0036] When the hydrogen ion concentration of the acid-containing solution is less than 0.1 mol / L, the exchange reaction between cations cannot be sufficiently carried out, and the efficiency of this exchange reaction decreases. When the acid-containing solution is more than 4.0 mol / L, the lithium manganate dissolves in its entirety in the acid solution, and the lithium manganate cannot be used again as a lithium adsorbent after adsorption. The acid used in the acid-containing solution is preferably hydrochloric acid, but is not limited thereto. For example, sulfuric acid or acetic acid may be used.

[0037] It is preferable that the hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, and that the hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less.

[0038] By setting the hydrogen ion concentration of the acid-containing solution in the first elution step and the hydrogen ion concentration of the acid-containing solution in the second elution step to predetermined values, dissolution of manganese from the lithium adsorbent can be suppressed and the efficiency of elution can be increased.

[0039] Depending on the shape of the lithium manganate, the form of contact between the adsorbed lithium manganate and the acid solution in the elution step varies. For example, if the lithium manganate is in powder form, one method is to put the powder of the adsorbed lithium manganate into the acid solution and stir it to bring the adsorbed lithium manganate into contact with the acid solution. If the lithium manganate is in particulate form or sprayed onto the fibers of a column, one method is to pass the acid solution through the liquid passage container while the particulate lithium manganate and the column are stored in the liquid passage container to bring the adsorbed lithium manganate into contact with the acid solution.

[0040] (Manganese oxidation process) In the manganese oxidation process, an oxidizing agent and a pH adjuster are added to the elution solution obtained in the elution process to oxidize divalent manganese to tetravalent manganese, resulting in a lithium-containing solution with a reduced manganese concentration. Tetravalent manganese is poorly soluble, so it precipitates in the solution. This makes it possible to reduce the concentration of manganese in the elution solution. Furthermore, the precipitated manganese can be reused as a raw material for lithium adsorbents.

[0041] In order to oxidize divalent manganese to tetravalent manganese, an oxidizing agent and a pH adjuster are added to the elution solution. When the oxidizing agent and the pH adjuster are added, it is preferable to adjust the pH to a range of 3 to 7 and the redox potential to 600 mV to 1100 mV using a silver-silver chloride electrode. That is, the pH and the redox potential are measured simultaneously, and the oxidizing agent and the pH adjuster are added simultaneously or alternately so that they are within the above range. As the oxidizing agent, for example, sodium hypochlorite, sodium chlorite, ozone, permanganate, etc. can be used. However, the oxidizing agent is not limited to these, and there is no problem as long as the redox potential can be adjusted. As the pH adjuster, for example, an alkaline neutralizing agent such as sodium hydroxide or slaked lime can be used. However, the oxidizing agent is not limited to these, and there is no problem as long as the pH can be adjusted.

[0042] (Post-manganese oxidation process) In the lithium-containing solution obtained in the manganese oxidation step, lithium exists in the form of lithium chloride (LiCl) in this embodiment, so that lithium can be obtained in the form of, for example, lithium carbonate by adding an alkali to this solution or by concentrating it by superheating.

[0043] After the adsorption, the lithium manganate is converted into a lithium adsorbent by the acid solution, and this lithium adsorbent is reused in the adsorption step.

[0044] Second embodiment 2 shows a flow diagram of the method for producing a lithium-containing solution according to the second embodiment of the present invention. The difference between the method for producing a lithium-containing solution according to the second embodiment and the method for producing a lithium-containing solution according to the first embodiment is that in the elution step, the elution solution is separated into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution having a lower lithium concentration than the high-concentration lithium elution solution, the acid-containing solution contains a low-concentration lithium elution solution to which an acid has been added, and the elution solution used in the manganese oxidation step contains a high-concentration lithium elution solution, and the other points are the same as those of the first embodiment. Therefore, the above differences will be described below.

[0045] (Elution step in the second embodiment) In the present embodiment, the elution solution is separated into a high-concentration lithium elution solution and a low-concentration lithium elution solution in the elution step. The high-concentration lithium elution solution is an elution solution containing lithium at a high concentration, and the low-concentration lithium elution solution is an elution solution having a lower lithium concentration than the high-concentration lithium elution solution.

[0046] In this embodiment, the acid-containing solution in the elution step includes a solution of a simple acid such as hydrochloric acid, and a solution in which an acid has been added to a low-concentration lithium elution solution.

[0047] The high-concentration lithium elution solution is an elution solution containing lithium at a high concentration, and is therefore used in a process carried out after the elution process, such as a manganese oxidation process.

[0048] By including the high-concentration lithium elution solution in the elution solution used in the manganese oxidation step, the lithium content of the elution solution used in the manganese oxidation step can be increased. Also, since only the low-concentration lithium elution solution is added to the acid-containing solution, the hydrogen ion concentration in the acid-containing solution can be increased by adding only a small amount of acid, and as a result, the amount of the acid-containing solution can be reduced, and the amount of the elution solution used in the manganese oxidation step can be reduced. This allows the production cost for lithium production to be reduced.

[0049] For example, when the elution step is performed by batch processing, the separation of the high-concentration lithium elution solution and the low-concentration lithium elution solution can be performed by extracting a predetermined volume of the elution solution based on the start of obtaining the elution solution by adding the acid-containing solution, and the remaining solution can be used as the low-concentration lithium elution solution. For example, when it is possible to predict the type of low-concentration lithium-containing solution and the amount of lithium eluted from the lithium adsorbent, the elution solution with a volume that is a predetermined multiple of the volume of the lithium adsorbent can be used as the high-concentration lithium elution solution, and the subsequent elution solution can be used as the low-concentration lithium elution solution.

[0050] 5 shows a graph showing the lithium concentration for each predetermined volume based on the start of obtaining the elution solution in this embodiment. The horizontal axis is BV (Bed Volume: a unit showing how many times the volume of the lithium adsorbent in the column) and the vertical axis shows the lithium concentration contained in the elution solution obtained after the elution step. For example, in the case shown in FIG. 3, BV2 and BV3 that exceed the second horizontal line from the top can be extracted as "predetermined volumes based on the start of obtaining the elution solution" and separated into a high-concentration lithium elution solution, BV1, and BV4 to BV9 as low-concentration lithium elution solutions.

[0051] The high-concentration lithium elution solution is an elution solution obtained by extracting a predetermined volume based on the start of obtaining the elution solution, so that the lithium content of the high-concentration lithium elution solution can be increased.

[0052] In this embodiment, BV2 and BV3 are extracted to form the high-concentration lithium elution solution, but this is not limited to this. For example, it is also possible to extract a predetermined volume from the beginning of the elution solution, that is, BV1 to BV4 are used as the high-concentration lithium elution solution. It is also possible to use only BV3 as the high-concentration lithium elution solution.

[0053] In addition, for example, when the elution step is performed by batch processing and the flow rate of the acid-containing solution used in the elution step is a predetermined rate, the high-concentration lithium elution solution and the low-concentration lithium elution solution can be separated by using the elution solution obtained between a predetermined start time and end time after the elution step begins as the high-concentration lithium elution solution, and the elution solution obtained thereafter as the low-concentration lithium elution solution. The flow rate is generally expressed as SV (Space Velocity: the amount of liquid passing per unit time (1 hour) BV), and when this SV is constant, the high-concentration lithium elution solution can be the elution solution obtained between a predetermined start time and end time after the elution step begins. The start of the elution step can be predetermined, such as when the acid-containing solution begins to be injected or when the elution solution begins to be collected.

[0054] The high-concentration lithium elution solution is an elution solution obtained within a predetermined period of time after the start of the elution step, so that the high-concentration lithium elution solution can be easily obtained.

[0055] Third embodiment 3 shows a flow diagram of the method for producing a lithium-containing solution according to the third embodiment of the present invention. The difference between the method for producing a lithium-containing solution according to the third embodiment and the method for producing a lithium-containing solution according to the first embodiment is that a water washing step for washing the eluted lithium adsorbent obtained through the elution step is provided after the elution step, and that the post-washing liquid obtained in the water washing step is added to the acid-containing solution. The other points are the same as those in the first embodiment. Therefore, the above differences will be described below.

[0056] (Water washing process) In the elution step in the second embodiment, an eluted lithium adsorbent is obtained. This eluted lithium adsorbent is washed in a water washing step. In the water washing step, for example, pure water is used, or industrial water is used in consideration of cost. The eluted lithium adsorbent washed in the water washing step is regenerated as a lithium adsorbent, and this lithium adsorbent is used again in the adsorption step.

[0057] The post-washing liquid obtained after washing the lithium adsorbent after elution in the water washing step may contain lithium. For example, the post-washing liquid obtained immediately after starting washing has a relatively high lithium concentration. In this embodiment, this post-washing liquid is added to the acid-containing solution. The post-washing liquid to be added to the acid-containing solution may be the whole of the post-washing liquid or a part of it. However, since the post-washing liquid obtained immediately after starting washing has a high lithium concentration, it is preferable that a predetermined amount of the post-washing liquid is added to the acid-containing solution after starting washing.

[0058] 6 is a graph showing the lithium concentration for each predetermined volume fraction based on the start of obtaining the post-rinsing liquid in this embodiment. The horizontal axis indicates the BV of the post-rinsing liquid, and the vertical axis indicates the lithium concentration contained in the post-rinsing liquid obtained after the water washing process. For example, in this embodiment, it is preferable to use the post-rinsing liquid of BV1, i.e., the start of obtaining the post-rinsing liquid, as the base, and repeat the post-rinsing liquid of only BV1 from the start of obtaining it into the acid-containing solution.

[0059] The post-rinsing liquid obtained in the water-rinsing step is added to the acid-containing solution, whereby lithium that would otherwise have to be discarded in the water-rinsing step can be recovered.

[0060] (Fourth embodiment) FIG. 4 shows a flow diagram of the method for producing a lithium-containing solution according to the fourth embodiment of the present invention. The difference between the method for producing a lithium-containing solution according to the fourth embodiment and the method for producing a lithium-containing solution according to the second embodiment is that a water washing step for washing the eluted lithium adsorbent obtained through the elution step is provided after the elution step, and the post-washing liquid obtained in the water washing step is added to the acid-containing solution. The other points are the same as those of the second embodiment. In addition, a detailed description of the water washing step is included in the description of the third embodiment. Therefore, a detailed description of the water washing step is omitted. EXAMPLES

[0061] Hereinafter, specific examples of the method for producing a lithium-containing solution according to the present invention will be described, but the present invention is not limited to these examples.

[0062] <Example 1> (Adsorption process) Powdered lithium adsorbent H 1.6 Mn 1.6 10 ml of O4 was held in a glass column with a diameter of 20 mm. A solution containing lithium dissolved therein, simulating salt lake brine, a low-concentration lithium-containing solution, was passed through the column to adsorb the lithium adsorbent and then the lithium manganate Li 1.6 Mn 1.6 The lithium concentration of the low-concentration lithium-containing solution was 0.7 g / L. In the adsorption process, the solution was passed through SV15, and the low-concentration lithium-containing solution was passed through only BV30.

[0063] (Elution step) The lithium manganate after adsorption in the glass column was contacted with an acid-containing solution. In the first elution step, an acid-containing solution consisting of only 1 mol / L hydrochloric acid was passed through the acid-containing solution for BV2. In the next second elution step, the acid-containing solution was 0.5 mol / L obtained by repeating the elution solution that had been through the first elution step and adding hydrochloric acid to it. The amount of liquid passed at that time was BV10, and the liquid passing speed was SV15. That is, all of the steps from BV3 to BV12 were second elution steps, and all of the acid-containing solutions were 0.5 mol / L. The solution that flowed out of the column was separated into a high-concentration lithium elution solution containing lithium at a high concentration at the initial stage of the elution, and a low-concentration lithium elution solution that was later than the initial stage and had a lower lithium concentration than the high-concentration lithium elution solution. In this example, the concentration of the high-concentration lithium elution solution was 6.5 g / L. The amount of the elution solution was 120 mL because only BV12 was passed through. The manganese concentration of the elution solution was 0.02 g / L.

[0064] (Manganese oxidation process) The manganese oxidation step was carried out using the eluted solution obtained in the elution step. An oxidizing agent and a pH adjuster were used in this step, and a lithium-containing solution was obtained. The manganese concentration in this step was 0.0 g / L.

[0065] <Comparative Example 1> In Comparative Example 1, the hydrogen ion concentration of the acid-containing solution in the elution step was all 0.5 mol / L (initially 0.5 mol / L using only hydrochloric acid, and then 0.5 mol / L was obtained by adding hydrochloric acid to the elution solution that had been through the elution step once). The parameters were the same as in Example 1. The concentration of the high-concentration lithium elution solution in Comparative Example 1 was 3.4 g / L. The volume of the elution solution at this time was 120 ml, the same as in Example 1. The manganese concentration of the elution solution at this time was 0.02 g / L.

[0066] <Comparative Example 2> In Comparative Example 2, the hydrogen ion concentration of the acid-containing solution in the elution step was all 1.0 mol / L (initially, 1.0 mol / L using only hydrochloric acid, and then 1.0 mol / L was obtained by adding hydrochloric acid to the elution solution that had been through the elution step once). The parameters were the same as in Example 1. The concentration of the high-concentration lithium elution solution in Comparative Example 2 was 5.2 g / L. The volume of the elution solution was 120 ml, the same as in Example 1. The manganese concentration of the elution solution was 0.06 g / L.

[0067] (summary) Regarding the high-concentration lithium elution solution, in Example 1, the lithium concentration was 6.5 g / L, which is 6.0 g / L or more, and the lithium concentration was maintained high, whereas in Comparative Example 1, the lithium concentration was 3.4 g / L, and in Comparative Example 2, the lithium concentration was 5.2 g / L, which is less than 6.0 g / L, and it was found that the lithium concentration of the high-concentration lithium elution solution was low. As described above, since the lithium concentration of the high-concentration lithium elution solution is high in the examples, it was found that when the amount of lithium finally obtained is constant, the total amount of the elution solution can be suppressed. In addition, in Example 1, the manganese concentration can also be suppressed to a low level compared to Comparative Example 2, and it was found that the deterioration of the lithium adsorbent can be suppressed.

Claims

1. an adsorption step of contacting a low-concentration lithium-containing solution with a lithium adsorbent obtained from lithium manganate to obtain lithium manganate after adsorption; an elution step of contacting the lithium manganate after the adsorption with an acid-containing solution to obtain an elution solution; a manganese oxidation step of adding an oxidizing agent and a pH adjuster to the elution solution to oxidize manganese and obtain a lithium-containing solution having a reduced manganese concentration; Execute in this order, The elution step includes a first elution step and a second elution step in which the hydrogen ion concentration of the acid-containing solution is lower than that of the first elution step, The second elution step is carried out after the first elution step.

2. The method for producing a lithium-containing solution comprising the steps of:

2. The hydrogen ion concentration of the acid-containing solution in the first elution step is 1.0 mol / L or more and 4.0 mol / L or less, The hydrogen ion concentration of the acid-containing solution in the second elution step is 0.1 mol / L or more and 0.5 mol / L or less. The method for producing a lithium-containing solution according to claim 1 .

3. In the elution step, the elution solution is separated into a high-concentration lithium elution solution containing lithium at a high concentration and a low-concentration lithium elution solution having a lower lithium concentration than the high-concentration lithium elution solution; The acid-containing solution used in the elution step includes the low-concentration lithium elution solution to which an acid has been added, The elution solution used in the manganese oxidation step includes the high-concentration lithium elution solution. The method for producing a lithium-containing solution according to claim 1 .

4. The high-concentration lithium elution solution is The elution solution is obtained by extracting a predetermined volume of the elution solution obtained through the elution step based on the start of the elution solution being obtained. The method for producing a lithium-containing solution according to claim 3 .

5. The high-concentration lithium elution solution is The elution solution obtained between a predetermined start time and end time after the elution step has begun. The method for producing a lithium-containing solution according to claim 3 .

6. A water washing step for washing the eluted lithium adsorbent obtained after the elution step is provided after the elution step, The post-washing liquid obtained in the water-washing step is added to the acid-containing solution. The method for producing a lithium-containing solution according to claim 1 .

Citation Information

Patent Citations

  • Lithium-containing solution production method