Powder film deposition apparatus and powder film deposition method

The apparatus and method integrate film formation and crushing under vacuum conditions, addressing inefficiencies and contamination issues by controlling temperature transitions, enhancing film forming efficiency and safety for powder materials.

JP2024147416AActive Publication Date: 2024-10-16DENSO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023060421
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-16
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

Conventional film forming methods for powder materials face challenges in disintegrating aggregates under vacuum conditions, particularly due to the incompatibility of crushing processes with high-temperature vacuum environments, leading to contamination and inefficiencies.

Method used

A powder film forming apparatus and method that allows for film formation and crushing of powder particles under vacuum conditions by using a crushing unit that operates at a temperature lower than the film forming temperature, with a controlled temperature transition to prevent unnecessary film formation on the crushing mechanism.

Benefits of technology

Enables efficient and safe film formation on powder materials with smaller particle sizes by integrating crushing within the vacuum environment, reducing equipment space and cost, and improving film forming efficiency while minimizing contamination and energy waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147416000001_ABST
    Figure 2024147416000001_ABST
Patent Text Reader

Abstract

To provide a powder film deposition apparatus capable of cracking a powder inside the powder film deposition apparatus.SOLUTION: In a powder film deposition apparatus 100, a film deposition step of depositing a film by reacting a surface of a powder with a raw material gas introduced under a vacuum condition heated in a predetermined film deposition temperature range, and a cracking step of cracking an aggregate of a powder particle at a temperature lower than the film deposition temperature range are performed. A chamber 50 is arranged in a vacuum chamber 200, and the raw material gas flows upward in a vertical direction through a powder storage part 55 in the film deposition step. An exhaust block 40 exhausts the raw material gas from an exhaust port 41 arranged on a side wall. A cracking unit 30 is configured such that the cracking unit is raised in the film deposition step and is retracted upward in the chamber 50, and is lowered in the cracking step and a crushing head 36 goes into the powder storage part 55. A control part 80 heats the chamber 50 to the film deposition temperature range in the film deposition step, lifts the cracking unit 30, cools the chamber 50 to a cracking possible temperature in the cracking step, and lowers the cracking unit 30.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder film forming apparatus and a powder film forming method. [Background technology]

[0002] Conventionally, there are known film-forming apparatuses and film-forming methods for forming a film on the surface of a processing object by reacting a source gas under vacuum conditions. For example, Patent Document 1 discloses a vacuum film-forming apparatus and film-forming method for forming a film on the surface of a substrate by the ALD (atomic layer deposition) method in which two types of source gases are alternately introduced and reacted. Patent Document 2 discloses a powder film-forming apparatus and film-forming method for forming a film on the surface of powder by the plasma CVD method. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-184482 A [Patent Document 2] Patent Publication No. 2022-008248 Summary of the Invention [Problem to be solved by the invention]

[0004] When performing ALD film formation on powder materials, the film is formed by supplying gas into a chamber that confines the powder. Here, the action of breaking down the agglomerates of powder particles is called "disintegration." By repeating the process of exposing the agglomerated parts of the powder after film formation by disintegration and then performing film formation again, it becomes possible to form films on powder materials with smaller particle sizes. However, since a typical disintegration process is performed in the atmosphere, it is not suitable for combination with ALD film formation, which is performed in a vacuum.

[0005] Furthermore, ALD film formation is performed under high-temperature vacuum conditions, for example, heated to a film formation temperature range of about 300°C. If the source gas comes into contact with the structure of the crushing mechanism heated to the film formation temperature range, unnecessary film formation processing will also occur on the surface of the structure, resulting in problems such as loss of source gas and by-products being mixed into the powder material. For this reason, it has been difficult to crush powder inside a powder film formation device under high-temperature vacuum conditions.

[0006] The present invention has been made in view of the above points, and an object of the present invention is to provide a powder film-forming apparatus and a powder film-forming method that are capable of crushing powder inside the powder film-forming apparatus. [Means for solving the problem]

[0007] The powder film-forming apparatus of the present invention carries out a film-forming process in which one or more types of raw material gases introduced from vertically below are reacted with the surface of the powder under vacuum conditions heated to a predetermined film-forming temperature range to form a film, and a crushing process in which agglomerates of powder particles are broken down at a temperature lower than the film-forming temperature range.

[0008] This powder film formation apparatus includes a vacuum chamber housing (20), a chamber (50), a heater (51), an exhaust block (40), a crushing unit (30), a unit lifting mechanism (25), an expandable member (24), and a control unit (80).

[0009] The vacuum chamber housing forms a vacuum chamber (200) therein, and has a source gas inlet (56) at the bottom. The chamber (50) is disposed in the vacuum chamber, and has a powder reservoir (55) that contains the powder to be processed, and the source gas introduced from the inlet in the film forming process flows vertically upward through the powder reservoir. The heater (51) heats the chamber.

[0010] The exhaust block (40) is connected to the top of the chamber, and the source gas is exhausted from an exhaust port (41) provided in the side wall.

[0011] The crushing unit (30) has a crushing head (36) at its lower end, which rotates to crush the powder. The crushing unit is configured to rise and retreat above the chamber during the film-forming process, and to descend during the crushing process, so that the crushing head enters the powder storage section.

[0012] The unit lifting mechanism 25 lifts and lowers the crushing unit. One end of a cylindrical expandable member 24 is fixed to the crushing unit, and expands and contracts in response to the elevation and lowering of the crushing unit while maintaining a vacuum inside.

[0013] The control unit (80) controls the temperature of the chamber, the lifting and lowering operation of the unit lifting mechanism, and the crushing operation of the crushing unit. Preferably, during the film-forming process, the control unit raises the temperature of the chamber to a film-forming temperature range and raises the crushing unit. Also, during the crushing process, the control unit lowers the temperature of the chamber to a crushing-enabling temperature that is lower than the film-forming temperature range and at which film formation on the crushing head is suppressed, and lowers the crushing unit.

[0014] In the powder film forming apparatus of the present invention, the chamber temperature in the crushing step is lowered to the crushing temperature, so the temperature of the crushing head that enters the powder is kept below the crushing temperature due to heat transfer. Even if the raw material gas comes into contact with the crushing head that has retreated to the upper part of the chamber in the subsequent film forming step, film formation on the crushing head is suppressed. Therefore, powder crushing can be realized inside the powder film forming apparatus.

[0015] The powder coating method of the present invention is a method in which a coating process in which one or more types of raw material gases introduced from vertically below are reacted with the surface of the powder to form a coating under vacuum conditions heated to a predetermined coating temperature range, and a crushing process in which agglomerates of powder particles are broken down at a temperature lower than the coating temperature range, are carried out inside a single powder coating apparatus (100).

[0016] In the powder film forming device, a crushing unit (30) having a crushing head (36) for crushing powder at its lower end can be raised and lowered by a unit lifting mechanism (25). In addition, a cylindrical expandable member (24) having one end fixed to the crushing unit is configured to expand and contract in response to the raising and lowering of the crushing unit while maintaining a vacuum inside.

[0017] In the film formation process, a chamber (50) having a powder storage section (55) for storing the powder to be processed, which is disposed in a vacuum chamber (20), is heated to a temperature within the film formation temperature range, and the crushing unit is raised and retreated to the upper part of the chamber. The raw material gas introduced from an inlet (56) flows vertically upward through the powder storage section and is exhausted from an exhaust port (41) provided in a side wall of an exhaust block (40) connected to the upper part of the chamber.

[0018] In the crushing step, the temperature of the chamber is lowered to a crushing temperature that is lower than the film-forming temperature range and suppresses film formation on the crushing head. The crushing unit is lowered, and the crushing head enters the powder storage section and rotates to crush the powder.

[0019] The powder film forming method of the present invention can provide the same effects as the powder film forming apparatus described above. This powder film forming method is synonymous with the "manufacturing method of a powder film formed," and the use, transfer, etc. of the powder film formed is included in the practice of the invention. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a schematic diagram showing a configuration of an original position of a powder film forming apparatus according to an embodiment. [Diagram 2] 2 is a schematic diagram showing an operation of the powder film-forming apparatus in FIG. 1 in a film-forming process. FIG. [Diagram 3] 2 is a schematic diagram showing an operation in a crushing process of the powder deposition apparatus in FIG. 1. [Figure 4] Schematic diagram of the powder storage section of the chamber during (a) the film formation process and (b) the crushing process. [Diagram 5] (a) Front view and (b) bottom view of the crushing head. [Figure 6]5A to 5C are diagrams illustrating changes in the state of powder particles caused by repeating a film-forming step and a crushing step. [Figure 7] 3 is a time chart of a powder film forming method according to an embodiment. [Figure 8] 1 is a flowchart of a powder deposition method according to an embodiment. [Figure 9] 4 is a time chart of a powder film forming method according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A powder film forming apparatus and a powder film forming method according to an embodiment of the present invention will be described with reference to the drawings. This powder film forming apparatus is an apparatus for forming a film by reacting one or more types of source gases on the surface of powder under vacuum conditions heated to a predetermined film forming temperature range. In this embodiment, an example is shown in which the powder is applied to an ALD (atomic layer deposition) method in which two types of precursors are introduced alternately as source gases. For example, the powder in the ALD method is carbon or silica, and the precursor is a metal oxide such as alumina. In batch processing, one batch of powder is set in the powder film forming apparatus.

[0022] Conventionally, it has been difficult to perform "disintegration" to break up aggregates of powder particles inside a powder deposition apparatus under high temperature vacuum conditions. Therefore, in this embodiment, an object is to provide a powder deposition apparatus 100 that can perform both the deposition process and the disintegration process inside a single apparatus. The disintegration process is performed at a temperature lower than the deposition temperature range. By integrating a disintegration mechanism into the vacuum deposition apparatus, the space and cost of the equipment can be reduced.

[0023] The configuration of a powder film forming apparatus 100 according to an embodiment will be described with reference to Figs. 1 to 3. Fig. 1 shows the apparatus configuration in situ. Fig. 2 shows the film forming process, and Fig. 3 shows the operation in the crushing process. The up-down direction of the paper surface of Figs. 1 to 3 is the vertical direction. In the following description, "upper" and "lower" mean "vertically upper" and "vertically lower". In the film forming process, the source gas introduced into the chamber 50 from below flows upward.

[0024] The powder film forming apparatus 100 includes a vacuum chamber housing 20, a chamber 50, a heater 51, a reflector 52, an exhaust block 40, a crushing unit 30, a unit lifting mechanism 25, an expandable member 24, a control unit 80, and the like.

[0025] First, the configuration related to the film formation process will be described. The vacuum chamber housing 20 is a housing surrounded by a bottom plate 21, a top plate 22, and a side plate 23, and a vacuum chamber 200 is formed inside. The vacuum chamber 200 communicates with a vacuum pump (not shown) via an exhaust passage. When an exhaust valve provided in the exhaust passage is opened, the pressure in the vacuum chamber 200 is reduced from atmospheric pressure to vacuum. For convenience, the low pressure state of the vacuum degree according to the film formation conditions is referred to as "vacuum". An inlet 56 for the source gas and the purge gas (N2, etc.) is provided at the bottom of the vacuum chamber housing 20. Hereinafter, the reference to the purge gas may be omitted as appropriate.

[0026] The chamber 50 is disposed in a vacuum chamber 200. Within the vacuum chamber housing 20, the inside of the chamber 50 through which the source gas for the film formation process passes is maintained at a higher degree of vacuum than the outside of the chamber 50. If the outside of the chamber 50 is considered to be a "low vacuum", the inside of the chamber 50 corresponds to a "medium vacuum". The chamber 50 is cylindrical with the diameter of the upper part being larger than the diameter of the lower part.

[0027] The chamber 50 has a powder reservoir 55 in the lower portion, which contains a batch of powder to be processed, and constitutes a fluidized bed type ALD film formation apparatus. As shown in Fig. 2, in the film formation process, a source gas (and a purge gas) introduced from an inlet 56 flows upward through the powder reservoir 55. Details will be described later with reference to Fig. 4.

[0028] The heater 51 is provided so as to surround the radial outside of the chamber 50, and heats the chamber 50. For example, the heater 51 is configured by laying a sheath heater on a plate. The reflector 52 is provided on the radial outside of the heater 51, and reflects the radiant heat from the heater 51 toward the chamber 50, as shown by the dashed arrow. This prevents parts other than the chamber 50, such as the crushing mechanism, from being unnecessarily overheated by the radiant heat from the heater 51. A temperature sensor 53, such as a thermocouple, detects the temperature of the chamber 50.

[0029] The exhaust block 40 is formed in a cylindrical shape and is connected to the upper part of the chamber 50. The source gas is exhausted from an exhaust port 41 provided on a side wall of the exhaust block 40. Although one exhaust port 41 is shown in FIG. 1 and the like, two exhaust ports may be provided so that two types of precursors are separately collected by a switching valve. As shown in FIG. 2, in the film formation process, the source gas flows to the upper part of the chamber 50, then changes direction horizontally within the exhaust block 40 and heads toward the exhaust port 41.

[0030] A thermal expansion absorbing member 44 made of, for example, a bellows is provided between the top plate 22 of the vacuum chamber housing 20 and the upper end of the exhaust block 40. The thermal expansion absorbing member 44 absorbs thermal expansion caused by temperature rises in the chamber 50 and the exhaust block 40 while isolating the internal space of the chamber 50 and the exhaust block 40 through which the source gas passes from the external space. Also, by not having the exhaust block 40 in direct contact with the top plate 22 of the vacuum chamber housing 20, heat transfer from the chamber 50 to the top plate 22 is inhibited.

[0031] Next, the configuration of the crushing mechanism installed under high temperature vacuum conditions will be described. The crushing unit 30 has a crushing head 36 at its lower end, which rotates to crush the powder. The crushing head 36 has a pin mill type structure, and will be described in detail later with reference to FIG. 5. As shown in FIG. 2 and FIG. 3, the crushing unit 30 is configured to rise and retreat above the chamber 50 in the film forming process, and to fall in the crushing process so that the crushing head 36 enters the powder storage section 55.

[0032] Preferably, when the crushing unit 30 is raised, the crushing head 36 is disposed above the height of the exhaust port 41 so as to avoid the exhaust path of the raw material gas. As described later, in addition to lowering the chamber temperature in the crushing step to a temperature at which crushing is possible, by making it difficult for the raw material gas to come into contact with the crushing head 36, it is more advantageous to suppress unnecessary film formation processing on the surface of the crushing head 36.

[0033] A cylindrical isolation case 38 is provided at the top of the disintegration unit 30 to isolate an atmosphere-side space Ra that is open to the atmosphere and a vacuum-side space Rv that communicates with the vacuum chamber 200. The unit lifting mechanism 25 lifts and lowers the disintegration unit 30 by, for example, rotating a ball screw 252 with a motor 251 to move the upper end position of the isolation case 38.

[0034] One end of the cylindrical expandable member 24 is fixed to the crushing unit 30, and expands and contracts in response to the elevation of the crushing unit 30 while maintaining a vacuum inside. In this embodiment, the expandable member 24 is composed of a bellows whose lower end is fixed to the top plate 22 of the vacuum chamber housing 20 and whose upper end is fixed to the isolation case 38. The space inside the isolation case 38 becomes the atmosphere-side space Ra, and the annular space between the outer wall of the isolation case 38 and the expandable member 24 becomes the vacuum-side space Rv. The volume of the vacuum-side space Rv changes as the expandable member 24 expands and contracts.

[0035] The crushing unit 30 includes the crushing head 36 and the isolation case 38, as well as a crushing motor 31, a coupling 32, a shaft 34, a bearing 35, a magnetic seal 33, and the like, which are provided along the rotation axis Z. The crushing motor 31 is disposed in the atmosphere side space Ra inside the isolation case 38, and outputs rotational power. The coupling 32 connects the output shaft of the crushing motor 31 to the shaft 34. The shaft 34 is disposed in the vacuum side space Rv, and rotates by the rotational power of the crushing motor 31 being transmitted thereto. As a result, the crushing head 36 fixed to the tip of the shaft 34 rotates to crush the powder. The bearing 35 rotatably supports the shaft 34.

[0036] Here, if air leaks from the atmosphere side space Ra to the vacuum side space Rv through the radial clearance in the rotation support part of the shaft 34, the degree of vacuum in the vacuum chamber 200 will decrease. In this embodiment, as a means for ensuring airtightness, a magnetic seal 33 is provided that seals the radial clearance with a magnetic fluid. The magnetic fluid is held in the gap between the rotating shaft and the pole piece along the magnetic flux lines formed by the magnet, thereby obtaining a seal. The heat resistance temperature of commercially available magnetic seals is about 130°C, which is the lowest heat resistance among the parts of the disintegration mechanism. Therefore, cooling water may be run around the magnetic seal 33 to prevent overheating.

[0037] In this embodiment, at least the control unit 80 controls the energization of the heater 51, the lifting operation of the unit lifting mechanism 25, and the disintegration operation of the disintegration unit 30. Regarding the temperature control of the chamber 50, the control unit 80 in this embodiment controls the energization of the heater 51 by PID control or the like so that the temperature detected by the temperature sensor 53, which is fed back, approaches a target value, and after reaching the target value, the detected temperature maintains the target value. In addition, the same control unit 80 may control the opening and closing of the exhaust valve, the timing of introduction of the purge gas and raw material gas in the film formation process, and the like, or a different control unit may share the function.

[0038] During the film formation process, the control unit 80 energizes the heater 51 to heat the chamber 50 to a film formation temperature range (for example, a target value of 300°C) and raises the crushing unit 30 using the unit lifting mechanism 25. During the crushing process, the control unit 80 stops energizing the heater 51 to lower the temperature of the chamber 50 to a crushing possible temperature (for example, 100°C) and lowers the crushing unit 30 using the unit lifting mechanism 25. The crushing possible temperature is set to a temperature that is lower than the film formation temperature range and suppresses film formation on the crushing head 36.

[0039] Here, even if the temperature of the crushing head 36 is within the film formation temperature range, the crushing operation itself is possible. However, for example, if the crushing head 36 enters the powder storage section 55 heated to 300°C to perform crushing, the crushing head 36 may receive heat from the powder and frictional heat, and the temperature may rise to nearly 300°C. The same applies to the lower part of the shaft 34 connected to the crushing head 36, and the same will be interpreted below. When the crushing unit 30 is raised and the crushing head 36 is evacuated above the chamber 50 in the subsequent film formation process, if the exhausted raw material gas comes into contact with the high-temperature crushing head 36, an unnecessary film formation process will be performed on the surface of the crushing head 36.

[0040] Therefore, the control unit 80 of this embodiment reduces the chamber temperature in the crushing process to a crushing temperature, thereby suppressing the temperature of the crushing head 36, which receives heat from heat transfer and friction from the powder during the crushing operation, to a temperature below the crushing temperature. Therefore, unnecessary film formation processing on the surface of the crushing head 36 is suppressed.

[0041] Next, referring to Figs. 4 to 6, the mechanism of the film forming process on the powder surface and the powder particle crushing process will be described. Fig. 4 shows a fluidized bed type film forming apparatus with a simplified shape of the chamber 50. In the film forming process shown in Fig. 4(a), the raw material gas (precursor) and the purge gas are introduced from the lower inlet 56, pass through the powder storage section 55 in which the powder particles P are accommodated, and flow out to the upper part of the chamber 50. For each cycle of "purge → precursor A introduction → purge → precursor B introduction", one atomic layer or molecular layer is formed on the surface of the powder particles P. The gas flowing out of the chamber 50 is exhausted to the side, not toward the upper part where the crushing head 36 is retracted.

[0042] In the crushing step shown in Fig. 4(b), the crushing head 36 enters the powder storage section 55 and rotates to break down agglomerates of powder particles P. Here, as shown in Fig. 5, the crushing head 36 has a plurality of pins 362 erected on the upper and lower surfaces of a disk 361. When the disk 361 rotates about the rotation axis Z, the impact of the plurality of pins 362 colliding with the powder particles P causes the powder particles P to be crushed.

[0043] With reference to FIG. 6, the change in the state of the powder particles P due to the repetition of the film-forming process and the crushing process will be described. In the first film-forming process, a first layer of film F1 is formed on the surface of the agglomerates of the powder particles P. In the subsequent crushing process, the agglomerates are dispersed, and the uncoated portions are exposed. The dispersed powder particles P re-aggregate due to intermolecular forces (van der Waals forces). In the second film-forming process, a second layer of film F2 is formed on the surface of the regorged agglomerates. At this time, a film is formed on the entire surface of the powder particles P, including the overlapping portions of the first layer of film F1 and the second layer of film F2 and the portions where only the second layer of film F2 is formed.

[0044] By repeating the film formation process and the crushing process in this way, the ratio of exposed uncoated parts can be reduced, and the film formation efficiency (coverage rate) for powders with small particle diameters can be improved. As will be described later as a comparative example, it is theoretically possible to repeat the film formation process in a vacuum film formation device and the crushing process in the external atmosphere, but this is inefficient in terms of time and energy, and there are also safety issues. In contrast, in this embodiment, the crushing mechanism is installed under high-temperature vacuum conditions by using the crushing unit 30, unit lifting mechanism 25, and expansion member 24, etc., so that the film formation process and the crushing process can be efficiently and safely repeated inside one powder film formation device 100.

[0045] A powder film formation method using the powder film formation apparatus 100 of this embodiment will be described with reference to the time chart of Fig. 7 and the flowchart of Fig. 8. In the explanation of the flowchart, the symbol "S" means a step. Here, an example is shown in which the method is applied to an ALD film formation method using two types of precursors A and B as source gases.

[0046] In the preparation stage, one batch of powder for batch processing is set in the chamber 50. Then, at time t01, the exhaust valve is opened, and at time t02, the vacuum chamber pressure is reduced from atmospheric pressure to vacuum. In S1 of the flowchart, the vacuum chamber pressure is reduced to vacuum.

[0047] At time t02, the control unit 80 starts energizing the heater 51 to heat the chamber 50. The temperature of the chamber 50 is then increased from room temperature (e.g., 20°C) to a target value (e.g., 300°C) in the film formation temperature range. At time t10, the chamber temperature reaches the target value in the film formation temperature range. In this manner, in S2, the control unit 80 increases the temperature of the chamber 50 to the film formation temperature range.

[0048] The first film formation process (S3) is performed from time t10 to t14. In one film formation process, the following four steps are repeated M cycles (M=4 in the illustrated example). For example, one purge takes 20 seconds, and one precursor introduction takes 10 seconds. [1] N2 purge [2] Precursor A introduction [3] N2 purge [4] Precursor B introduction

[0049] After passing through times t11, t12, and t13 when the first to third cycles end, N2 purging is finally performed after the fourth cycle, and one film formation process (S3) ends at time t14. In S4, it is determined whether the film formation process has reached a set number of times N (for example, N=3). If the answer is NO in S4, the process proceeds to S5 to S8, which include the disintegration process and the processes before and after it.

[0050] When the first film formation process is completed at time t14, the control unit 80 stops the power supply to the heater 51 and reduces the temperature of the chamber 50 to a temperature at which disintegration is possible (e.g., 100°C) (S5). When the temperature of the chamber 50 is reduced to the temperature at which disintegration is possible, the control unit 80 lowers the disintegration unit 30 at time t15 and rotates the disintegration motor 31 at time t16 to perform the first disintegration process (S6).

[0051] When the crushing process for a predetermined time is completed, the control unit 80 stops the rotation of the crushing motor 31 at time t17 and raises the crushing unit 30 (S7). When the crushing unit 30 has been raised, the control unit 80 energizes the heater 51 at time t18 and raises the temperature of the chamber 50 again to the film formation temperature range (S8).

[0052] The second film formation process (S3) is performed from time t20 to t24, and the second disintegration process and the processes before and after (S5 to S8) are performed from time t24 to t28. Furthermore, the third film formation process (S3) is performed from time t30 to t34. The operations at each time t20 to t34 are the same as the operations at each time t10 to t18 in the first film formation process and disintegration process, so the explanation will be omitted.

[0053] After the third film formation process, it is determined in S4 that the film formation process has reached the set number of times N, and the process proceeds to S9. At time t34, the control unit 80 stops the power supply to the heater 51, and the temperature of the chamber 50 is lowered to room temperature (S9). When the temperature of the chamber 50 is lowered to room temperature, the exhaust valve is closed at time t99, and the vacuum chamber pressure is returned to atmospheric pressure (S10). Then, the processed batch of powder is removed from the powder film formation apparatus 100.

[0054] As described above, in the powder film-forming method of the present embodiment, the film-forming process and the crushing process are alternately repeated multiple times under vacuum conditions for one batch of powder in the batch processing, thereby improving the film-forming efficiency (coverage rate) for powder with a small particle size.

[0055] The effects of this embodiment will be described in comparison with a powder film formation method of a comparative example shown in Figure 9. In the comparative example, a powder film formation apparatus that performs only the vacuum film formation process is used, and the crushing process is performed in the atmosphere outside the apparatus. In Figure 9, the symbols of time corresponding to Figure 7 are used. The conditions of the film formation process from t10 to t14 and t20 to t24 are the same as in this embodiment. If the time axis is expressed on the same scale as Figure 7, the third film formation process in the comparative example frames out of the page.

[0056] In the comparative example, when the first film formation process is completed at time t14, power to the heater 51 is stopped and the temperature of the chamber 50 is decreased. When the temperature of the chamber 50 is decreased to room temperature at time t15z, the exhaust valve is closed and the vacuum chamber pressure is returned to atmospheric pressure. The powder batch after film formation is removed from the apparatus, and the first crushing process (times t16 to t17) is carried out in the atmosphere outside the apparatus.

[0057] The powder batch after crushing is set back into the powder film forming apparatus, the exhaust valve is opened, and the vacuum chamber pressure becomes a vacuum. At time t18z, the chamber 50 is heated again from room temperature to the film forming temperature range, and the second film forming process is started at time t20. When the second film forming process is completed at time t24, the powder batch is removed from the apparatus in a similar procedure, and a second crushing process (times t26 to t27) is carried out in the atmosphere outside the apparatus. The powder batch after crushing is set back into the apparatus, and the third film forming process is started in a similar procedure.

[0058] In this way, in the comparative example, it takes time to repeatedly lower and raise the temperature from the film formation temperature range to room temperature every time the film formation process and the crushing process are switched over. It also takes time to stabilize the pressure every time the vacuum chamber 200 is depressurized. It takes a huge amount of time, including the time to remove and set the powder batch, and there is a large waste of energy. In addition, it is not preferable to perform the crushing process of highly active powder material such as metallic aluminum in an air atmosphere from the viewpoint of work safety.

[0059] In contrast, in this embodiment, it is sufficient to repeat the temperature drop and rise from the film formation temperature range to the crushing possible temperature every time the film formation process and the crushing process are switched. From this viewpoint, it is preferable that the crushing possible temperature is set as high as possible within a range that can suppress unnecessary film formation processing on the crushing head 36. In some cases, it is possible to accept the disadvantage of some film formation processing on the crushing head 36 and set the optimal crushing possible temperature by trading off with the shortening of the temperature drop time and temperature rise time.

[0060] In addition, in this embodiment, the vacuum chamber 200 is maintained at a vacuum throughout the entire process, so the time required for pressure stabilization during the second and subsequent depressurizations of the vacuum chamber can be shortened compared to the comparative example. In addition, the time required for removing and resetting the powder batch can be shortened, and no work space is required for the external crushing process. Furthermore, energy loss associated with the temperature drop and rise of the chamber and the pressure increase and decrease of the vacuum chamber is also reduced. In addition, safety is improved because the crushing process of highly active powder materials is not performed in the air.

[0061] (Other embodiments) (a) The powder deposition apparatus of the present invention is not limited to use in an ALD method in which two types of precursors are alternately introduced as source gases, but may also be used in a CVD method in which one type of source gas is introduced and deposited on the powder surface.

[0062] (b) The configuration for ensuring airtightness between the atmosphere-side space Ra and the vacuum-side space Rv in the rotational power transmission section of the disintegration unit 30 is not limited to using the magnetic seal 33. For example, the output shaft of the disintegration motor 31 in the atmosphere-side space Ra and the shaft 34 in the vacuum-side section Rv may be mechanically separated via a partition wall, and the rotational power may be transmitted in a non-contact manner by a magnetic coupling. Note that magnetic couplings are known as functional components that transmit torque without liquid leakage in liquid pumps, etc.

[0063] (c) The crushing unit 30 is not limited to a configuration in which the atmosphere side space and the vacuum side space are separated by the separation case 38. If the crushing motor 31 can be arranged in the vacuum side space, the crushing unit 30 may be configured only in the vacuum side space.

[0064] (d) The expandable member 24 is not limited to a bellows, but may be configured with, for example, a multi-cylinder structure, etc. The unit lifting mechanism 25 is not limited to the ball screw structure exemplified in FIG. 1, etc., but may be configured with a cylinder that moves a rod forward and backward, etc.

[0065] (e) In the powder coating method of the above embodiment, the coating process and the crushing process are alternately repeated multiple times under vacuum conditions for one batch of powder in the batch processing, thereby improving the coating efficiency (coverage rate) for powder with a small particle size. However, the crushing process may be performed only once, such as "first coating process - crushing process - second coating process".

[0066] (f) The temperature control of the chamber 50 by the control unit 80 is not limited to the method of controlling the power supply to the heater 51 by feeding back the temperature detected by the temperature sensor 53 installed in the chamber 50. For example, the temperature detected at another location correlated with the chamber temperature may be fed back, or feedforward control may be performed based on the amount of heat generated by the heater 51 and the power supply time.

[0067] As described above, the present invention is not limited to the above-described embodiment, and can be embodied in various forms without departing from the spirit of the present invention. [Explanation of symbols]

[0068] 100...Powder film forming equipment, 200 ··· Vacuum chamber, 20 ··· Vacuum chamber housing, 24....Expandable member; 25....Unit lifting mechanism; 30....Crushing unit, 36....Crushing head, 40... Exhaust block, 41... Exhaust port, 50: chamber; 51: heater; 55...powder storage section, 56...inlet, 80...control section.

Claims

1. A powder film-forming apparatus which performs a film-forming step of forming a film by reacting one or more kinds of raw material gases introduced from below in a vertical direction with the surface of powder under vacuum conditions heated to a predetermined film-forming temperature range, and a disintegration step of disintegrating aggregates of powder particles at a temperature lower than the film-forming temperature range, A vacuum chamber housing (20) having a vacuum chamber (200) formed therein and an inlet (56) for a raw material gas provided at the bottom thereof; a chamber (50) disposed in the vacuum chamber, the chamber having a powder storage section (55) in which a powder to be treated is accommodated, and a source gas introduced from the inlet in a film forming process flows vertically upward through the powder storage section; A heater (51) for heating the chamber; an exhaust block (40) connected to the upper portion of the chamber and through which a source gas is exhausted from an exhaust port (41) provided in a side wall; a crushing unit (30) having a crushing head (36) at a lower end thereof for crushing powder by rotation, the crushing unit (30) being configured to rise and retreat above the chamber in a film forming process and to fall in a crushing process so that the crushing head enters the powder storage section; A unit lifting mechanism (25) for lifting and lowering the crushing unit; a cylindrical expandable member (24) having one end fixed to the crushing unit and expanding and contracting in response to the elevation and lowering of the crushing unit while maintaining a vacuum inside; a control unit (80) for controlling the temperature of the chamber, the lifting and lowering operation of the unit lifting mechanism, and the crushing operation of the crushing unit; A powder deposition apparatus comprising:

2. The control unit is During the film formation process, the chamber is heated to the film formation temperature range, and the crushing unit is raised; 2. The powder film-forming apparatus according to claim 1, wherein, in the crushing step, the temperature of the chamber is lowered to a crushing-enabling temperature that is lower than the film-forming temperature range and suppresses film formation on the crushing head, and the crushing unit is lowered.

3. The crushing unit includes: an isolation case (38) for isolating an atmosphere-side space that is open to the atmosphere from a vacuum-side space that is in communication with the vacuum chamber; A crushing motor (31) disposed in the atmospheric space and outputting rotational power; A shaft (34) is disposed in the vacuum side space and rotates by the rotational power of the disintegration motor being transmitted thereto; The crushing head (36) fixed to the tip of the shaft; The powder deposition apparatus according to claim 2 ,

4. The crushing unit includes:

4. The powder deposition apparatus according to claim 3, further comprising a magnetic seal (33) for sealing a radial clearance at a rotation support portion of the shaft with a magnetic fluid.

5. The heater is provided so as to surround the radial outside of the chamber, 5. The powder deposition apparatus according to claim 2, further comprising a reflector (52) disposed radially outward of the heater for reflecting radiant heat from the heater toward the chamber.

6. A powder film-forming method in which a film-forming step of forming a film by reacting one or more kinds of raw material gases introduced from below in a vertical direction with a surface of powder under vacuum conditions heated to a predetermined film-forming temperature range, and a disintegration step of disintegrating agglomerates of powder particles at a temperature lower than the film-forming temperature range, are performed inside one powder film-forming apparatus (100), The powder deposition apparatus includes: A crushing unit (30) having a crushing head (36) for crushing powder at its lower end can be raised and lowered by a unit lifting mechanism (25); A cylindrical expandable member (24) having one end fixed to the crushing unit is configured to expand and contract in response to the elevation and lowering of the crushing unit while maintaining a vacuum inside, In the film forming step, A chamber (50) that is disposed in a vacuum chamber (20) and has a powder storage section (55) that contains powder to be treated is heated to the film formation temperature range, and the crushing unit is raised and retreated to above the chamber, A raw material gas introduced from an inlet (56) flows vertically upward through the powder storage section and is exhausted from an exhaust port (41) provided in a side wall of an exhaust block (40) connected to an upper portion of the chamber; In the crushing step, A powder coating method in which the temperature of the chamber is lowered to a crushing temperature that is lower than the coating temperature range and suppresses coating formation on the crushing head, the crushing unit is lowered, and the crushing head enters the powder storage section and rotates to crush the powder.

7. The powder film-forming method according to claim 6 , wherein the film-forming step and the crushing step are alternately repeated a plurality of times under vacuum conditions for one batch of powder in the batch processing.

Citation Information

Patent Citations

  • Method for stirring fine particles, and surface modification method for abrasive grain using it

    JP2005281765A

  • Apparatus and method for forming fine particle

    JP2011132591A

  • Vacuum film forming apparatus and film forming method

    JP2012184482A

  • Powder film deposition apparatus and powder film deposition method

    JP2022008248A