Phase shift blankmask and photomask for extreme ultraviolet lithography

The use of a phase shift film with ruthenium (Ru) and an etching stopper film of tantalum (Ta) and antimony (Sb) in EUV lithography masks addresses the challenge of achieving high extinction coefficient (k) and low refractive index (n), resulting in improved resolution, NILS, and reduced DtC for enhanced semiconductor manufacturing.

JP2024147477AActive Publication Date: 2024-10-16S & S TECH

Patent Information

Application Number
JP2023137275
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-27
Filing Date
2023-08-25
Publication Date
2024-10-16
Estimated Expiration
2043-08-25

AI Technical Summary

Technical Problem

Existing phase shift blank masks for EUV lithography face challenges in achieving high extinction coefficient (k) and low refractive index (n) simultaneously, leading to issues with DtC, NILS, and pattern precision due to the use of ruthenium (Ru) in the phase shift film and tantalum (Ta) in the etching stopper film, which do not satisfy both requirements effectively.

Method used

A blank mask structure is introduced with a phase shift film containing ruthenium (Ru) and an etching stopper film composed of tantalum (Ta) and antimony (Sb), along with specific ratios and additional elements like nitrogen (N) and oxygen (O), to enhance the extinction coefficient (k) and lower the refractive index (n), ensuring a thin thickness, low relative reflectance, and improved NILS.

Benefits of technology

The proposed structure achieves excellent resolution and NILS during wafer printing, reduces DtC, and enhances pattern precision by optimizing the extinction coefficient (k) and refractive index (n) of the laminated films, thereby improving semiconductor productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147477000001_ABST
    Figure 2024147477000001_ABST
Patent Text Reader

Abstract

To provide a solution for achieving a thin thickness, a low relative reflectivity, a low DtC, and a high NILS of a blankmask having a phase shift film containing ruthenium (Ru), by increasing the extinction coefficient (k) and reducing the refractive index (n) in an entire stack structure of an etch stop film and the phase shift film.SOLUTION: A blankmask for EUV lithography has a reflective film formed on a substrate, a capping film containing ruthenium (Ru), an etch stop film containing tantalum (Ta) and antimony (Sb), and a phase shift film containing ruthenium (Ru). The etch stop film has a composition ratio of tantalum (Ta):antimony (Sb) between 3:7 and 7:3. The stack structure of the phase shift film containing ruthenium (Ru) and the etch stop film containing tantalum (Ta) and antimony (Sb) ensures a high extinction coefficient (k) and a low refractive index (n).SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a blank mask and a photomask, and more particularly to a phase shift blank mask for extreme ultraviolet lithography having a phase shift film that shifts the phase of EUV exposure light to realize excellent resolution during wafer printing, and a photomask manufactured using the same. [Background technology]

[0002] A blank mask used in EUV lithography generally comprises two types of thin films on a substrate: a reflective film that reflects EUV light and an absorbing film that absorbs EUV light. Recently, attempts have been made to develop a phase-shift blank mask that can realize a higher resolution than a binary blank mask having such an absorbing film. A phase-shift blank mask has a higher NILS (Normalized Image Log Slope) than a binary blank mask, and therefore can reduce stochastic defects caused by the shot noise effect during wafer printing. In addition, a phase-shift blank mask can realize a low DtC (Dose to Clear), thereby increasing semiconductor productivity.

[0003] In phase shift blank masks for EUV lithography, it is preferable that the phase shift film is made of a material that is easy to manufacture as a photomask and has excellent performance when printing on a wafer. Considering these points, ruthenium (Ru) is being researched as a material for the phase shift film.

[0004] Fig. 1 is a diagram showing the structure of a phase shift blank mask for extreme ultraviolet lithography having a phase shift film containing ruthenium (Ru). The structure in Fig. 1 shows the applicant's prior art compared to the present invention in order to explain the technical features of the present invention, and does not mean that the structure in Fig. 1 described below was publicly known before the filing of the present invention.

[0005] The phase shift blank mask for extreme ultraviolet lithography includes a substrate 102, a reflective film 104 formed on the substrate 102, a capping film 105 formed on the reflective film 104, an etch stop film 107 formed on the capping film 105, a phase shift film 108 formed on the etch stop film 107, a hard mask film 109 formed on the phase shift film 108, and a resist film 110 formed on the hard mask film 109.

[0006] The capping film 105 is made of a material containing ruthenium (Ru), and the phase shift film 108 is also made of a material containing ruthenium (Ru), specifically, RuON.

[0007] The etch stop layer 107 has a two-layer structure, that is, a first layer 107a on the capping layer 105 and a second layer 107b on the first layer 107a. The first layer 107a is made of TaBN, and the second layer 107b is made of TaBO.

[0008] The hard mask film 109 is made of TaBO.

[0009] To manufacture a photomask using the blank mask configured as above, first, a pattern of the resist film 110 is formed by a development process after e-beam writing, and the hard mask film 109 of TaBO is etched using the resist film pattern as an etching mask to form a hard mask film pattern. At this time, a fluorine (F)-based gas is used as an etching gas. After that, the resist film pattern is removed, and the phase shift film 108 is etched with a chlorine (Cl2)-based gas containing oxygen (O2) using the hard mask film pattern as an etching mask.

[0010] Meanwhile, tantalum (Ta) is etched by a chlorine-based gas, but when oxygen (O) is added to tantalum (Ta), it is etched by a fluorine (F)-based gas. Therefore, in the etching process of the etching stopper film 107, the second layer 107b of TaBO is first etched by a fluorine-based gas, and at this time, the pattern of the hard mask film 109 is also etched and removed. Then, the first layer 107a of the etching stopper film 107 is etched using a chlorine (Cl2)-based gas that does not contain oxygen (O2). This completes the manufacture of the phase shift photomask.

[0011] In the phase shift blank mask having the above structure, the phase shift film 108 containing ruthenium (Ru) is etched using chlorine (Cl2)-based gas. At this time, if only chlorine (Cl2) gas is used for etching, the etching speed is very slow, so in order to secure a certain etching speed or higher, chlorine (Cl2)-based gas containing oxygen (O2) is used. However, in the structure of FIG. 1, the capping film 105 and the phase shift film 108 both contain ruthenium (Ru). Therefore, if the etching stop film 107 is not provided, the capping film 105 would be damaged by oxygen (O2) contained in the etching gas during etching for patterning the phase shift film 108, and the reflectance of the capping film 105 would decrease. The etching stop film 107 has a function of preventing the capping film 105 from being damaged by preventing the chlorine (Cl2)-based gas containing oxygen (O2) from coming into contact with the capping film 105.

[0012] However, when forming the phase shift film 108 containing Ru, it is preferable that the etching stop film 107 is formed in a two-layer structure as described above. If the etching stop film 107 is made of a single layer of TaBN, TaBN is vulnerable to oxidation, so that oxidation occurs on the surface of the etching stop film 107 due to oxygen (O2) during etching of the RuON phase shift film 108. Since such oxidation is distributed randomly, it induces defects on the surface of the etching stop film 107, and furthermore, it causes a decrease in the etching rate during etching using chlorine (Cl2)-based gas. Furthermore, etching using chlorine (Cl2)-based gas is mainly chemical etching, and etching using fluorine (F)-based gas is mainly physical etching. Therefore, if the etching stop film 107 is made of a single layer of TaBO, the capping film 105 will be physically damaged during etching using fluorine (F)-based gas. From this point of view, by forming the first layer 107a from TaBN and the second layer 107b from TaBO, the capping film 105 is prevented from being damaged by oxygen (O2) and fluorine (F)-based gases.

[0013] In the process of exposing a wafer using a photomask manufactured using the blank mask as described above, in order to improve productivity, it is necessary to further reduce DtC, and in order to improve the CD of the pattern, it is necessary to further increase NILS. In order to reduce DtC, it is preferable that the phase shift film 108 has a high extinction coefficient (k). Specifically, in order to prevent the sidelobe phenomenon in the exposure process, it is preferable that the relative reflectance of the phase shift film 108 is 15% or less, and in order to reduce the thickness of the phase shift film 108 while reducing the relative reflectance, it is preferable that the extinction coefficient (k) is high. In order to increase the NILS, it is preferable that the phase shift film 108 has a low refractive index (n). However, ruthenium (Ru) has a low refractive index (n) and a low extinction coefficient (k), so it is not possible to simultaneously satisfy these two requirements.

[0014] The etching stop layer 107 under the phase shift layer 108 performs a phase shift function together with the phase shift layer 108. Therefore, if the etching stop layer 107 has a high extinction coefficient (k), the extinction coefficient (k) of the entire thin film that actually functions as a phase shift layer, i.e., the entire stacked structure of the etching stop layer 107 and the phase shift layer 108, becomes high. However, since the etching stop layer 107 in FIG. 1 contains tantalum (Ta) whose extinction coefficient (k) for the EUV wavelength is about 0.04, the entire thin films 107 and 108 performing the phase shift function cannot have a high extinction coefficient (k). This problem can be solved by increasing the thickness of the etching stop layer 107, but in this case, the thickness of the entire thin films 107 and 108 performing the phase shift function increases, which deteriorates the DtC and increases the 3D effect. Summary of the Invention [Problem to be solved by the invention]

[0015] The objective of the present invention is to provide a method for realizing thin thickness, low relative reflectance, low DtC, and high NILS in a blank mask having a phase shifting film containing ruthenium (Ru) by increasing the extinction coefficient (k) and decreasing the refractive index (n) in the entire stacked structure including an etch stop film and a phase shifting film. [Means for solving the problem]

[0016] The blank mask for EUV lithography according to the present invention includes a substrate, a reflective film formed on the substrate, a capping film formed on the reflective film and including ruthenium (Ru), an etching stop film formed on the capping film and including tantalum (Ta) and antimony (Sb), and a phase shift film formed on the etching stop film and including ruthenium (Ru).

[0017] The etching stop layer has a content ratio of tantalum (Ta):antimony (Sb)=3:7 to 7:3.

[0018] The etch stop layer may be configured such that the antimony (Sb) content is greater than the tantalum (Ta) content.

[0019] The etching stop layer may further contain nitrogen (N). The etching stop layer contains 1 to 10 at % of nitrogen (N).

[0020] The etch stop layer may include a first layer formed on the capping layer and further including nitrogen (N), and a second layer formed on the first layer and further including oxygen (O), wherein the first layer includes 1 to 10 at % of nitrogen (N), and the second layer includes 1 to 10 at % of oxygen (O).

[0021] The etch stop film has a thickness of 2 to 20 nm.

[0022] The phase shift film may further contain nitrogen (N). The phase shift film contains 70 to 99 at % of ruthenium (Ru) and 1 to 30 at % of nitrogen (N).

[0023] The phase shift film may further contain oxygen (O). The phase shift film contains 70 to 99 at % of ruthenium (Ru) and 1 to 30 at % of oxygen (O).

[0024] The phase shift film may further contain nitrogen (N) and oxygen (O). The phase shift film contains 40 to 98 at % ruthenium (Ru), 1 to 30 at % nitrogen (N), and 1 to 30 at % oxygen (O).

[0025] The phase shift film has a thickness of 25 to 40 nm.

[0026] A hard mask layer may be formed on the phase shift layer.

[0027] The hard mask film may include tantalum (Ta) and oxygen (O).

[0028] The hard mask film may include a lower layer formed on the phase shift film and containing tantalum (Ta) and nitrogen (N), and an upper layer formed on the lower layer and containing tantalum (Ta) and oxygen (O). The lower layer contains 70 to 99 at% tantalum (Ta) and 1 to 30 at% nitrogen (N), and the upper layer contains 70 to 99 at% tantalum (Ta) and 1 to 30 at% oxygen (O).

[0029] The hard mask film may further contain boron (B).

[0030] The hard mask film may include chromium (Cr) and niobium (Nb), and the hard mask film may include chromium (Cr):niobium (Nb)=3:7 to 6:4.

[0031] The hard mask film may further include at least one of carbon (C), oxygen (O), and nitrogen (N).

[0032] The hard mask film has a thickness of 2 to 4 nm.

[0033] According to another aspect of the present invention, there is provided a photomask for extreme ultraviolet lithography manufactured using the blank mask having the above-mentioned structure. Effect of the Invention

[0034] According to the present invention, a high extinction coefficient (k) and a low refractive index (n) are ensured by a laminated structure of a phase shifting film containing ruthenium (Ru) and an etching stopper film containing tantalum (Ta) and antimony (Sb). Therefore, it is possible to realize the characteristics required for an EUV phase shifting blank mask, that is, excellent resolution and NILS (Normalized Image Log Slop) during wafer printing, and low DtC (Dose to Clear). [Brief description of the drawings]

[0035] [Figure 1]FIG. 1 shows the structure of a phase shift blank mask for extreme ultraviolet lithography. [Diagram 2] FIG. 1 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a first embodiment of the present invention. [Diagram 3] FIG. 13 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a second embodiment of the present invention. [Figure 4] FIG. 13 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a third embodiment of the present invention. [Diagram 5] FIG. 13 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a fourth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] The invention will now be described in more detail with reference to the drawings.

[0037] FIG. 2 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a first embodiment of the present invention.

[0038] The phase shift blank mask for extreme ultraviolet lithography according to the present invention comprises a substrate 202, a reflective film 204 formed on the substrate 202, a capping film 205 formed on the reflective film 204, an etching stop film 207 formed on the capping film 205, a phase shift film 208 formed on the etching stop film 207, and a resist film 210 formed on the phase shift film 208.

[0039] The substrate 202 is made of a glass substrate having a thickness of 0±1.0×10 in order to prevent deformation and stress of the pattern due to heat during exposure so as to be suitable as a glass substrate for a reflective blank mask using EUV exposure light. -7 / °C, preferably 0±0.3×10 -7The substrate 202 is made of a low thermal expansion material (LTEM) substrate having a low thermal expansion coefficient within the range of 100 / ° C. The substrate 202 may be made of SiO2-TiO2 glass, multi-component glass ceramics, or the like.

[0040] The reflective film 204 has a function of reflecting EUV exposure light, and has a multi-layer structure in which each layer has a different refractive index. Specifically, the reflective film 204 is formed by alternately stacking 40 to 60 layers of Mo material and Si material layers.

[0041] The capping film 205 prevents the formation of an oxide film on the reflective film 204, thereby maintaining the reflectance of the reflective film 204 to EUV exposure light, and prevents the reflective film 204 from being etched when the etching stop film 207 is patterned. In general, the capping film 205 is made of a material containing ruthenium (Ru). The capping film 205 is formed to a thickness of 2 to 5 nm. If the thickness of the capping film 205 is 2 nm or less, it is difficult for the capping film 205 to function properly, and if it is 5 nm or more, there is a problem that the reflectance to EUV exposure light decreases.

[0042] The etch stop layer 207 protects the capping layer 205 when etching the phase shift layer 208. After etching the hard mask layer 209 and the phase shift layer 208, the etch stop layer 207 is etched using the pattern of the hard mask layer 209 and the pattern of the phase shift layer 208 as an etching mask. At this time, in order to prevent damage to the capping layer 205, the etch stop layer 207 must be etched using a gas that does not contain oxygen (O2).

[0043] The etching stop film 207 also performs a phase shift function for EUV exposure light together with the phase shift film 208. Therefore, from a functional aspect, the entire laminated structure of the etching stop film 207 and the phase shift film 208 has a phase shift function. Hereinafter, the entire laminated structure of the etching stop film 207 and the phase shift film 208 will be referred to as the "entire phase shift film 207, 208."

[0044] Since the etching stop layer 207 functions as a part of the entire phase shifting layer 207, 208, it is preferable that the etching stop layer 207 is made of a material having a high extinction coefficient (k) in order to increase the extinction coefficient (k) of the entire phase shifting layer 207, 208. In the present invention, the etching stop layer 207 contains tantalum (Ta) and antimony (Sb). Tantalum (Ta) and antimony (Sb) have a higher extinction coefficient (k) with respect to EUV exposure light than ruthenium (Ru), which is the main constituent material of the phase shifting layer 208. Therefore, the extinction coefficient (k) of the entire phase shifting layer 207, 208 can be increased by the etching stop layer 207 containing tantalum (Ta) and antimony (Sb). The content ratio of tantalum (Ta) and antimony (Sb) may be 3:7 to 7:3.

[0045] The etching stop layer 207 is configured to have an extinction coefficient (k) of 0.05 or more, preferably 0.06 or more. Since the extinction coefficient (k) of antimony (Sb) is higher than that of tantalum (Ta), in order to ensure such an extinction coefficient (k), it is preferable that the content of antimony (Sb) is higher than that of tantalum (Ta).

[0046] The etch stop layer 207 may further contain nitrogen (N). When nitrogen (N) is further contained, the extinction coefficient (k) and refractive index (n) of the etch stop layer 207 can be adjusted by adjusting the nitrogen (N) content. At this time, the nitrogen (N) content is preferably 1 to 10 at %. The etch stop layer 207 made of TaSbN is etched by a chlorine (Cl2)-based etching gas that does not contain oxygen (O2).

[0047] The etching stopper film 207 has a thickness of 2 to 20 nm.

[0048] The phase shift film 208 inverts the phase of the exposure light and reflects it, thereby causing destructive interference of the exposure light reflected by the reflective film 204. The phase shift film 208 contains ruthenium (Ru). The phase shift film 208 is etched with a chlorine (Cl2)-based gas, and in particular, in order to ensure an etching speed, it is etched with a chlorine (Cl2)-based gas containing oxygen (O2).

[0049] The phase shift film 208 may further contain nitrogen (N). When nitrogen (N) is contained, the refractive index (n) of the phase shift film 208 is easily controlled, so that the required amount of phase shift can be easily realized. This improves NILS and allows the thickness of the phase shift film 208 to be reduced while realizing the required amount of phase shift. When nitrogen (N) is contained, the refractive index (n) of the phase shift film 208 increases, so the content of nitrogen (N) must be appropriately selected. When the phase shift film 208 is made of RuN, the content of nitrogen (N) is preferably 30 at % or less. Specifically, the phase shift film 208 contains 70 to 99 at % of ruthenium (Ru) and 1 to 30 at % of nitrogen (N).

[0050] The phase shift film 208 may further contain oxygen (O). When oxygen (O) is contained, the reflectance of the phase shift film 208 at DUV wavelengths is reduced, and the phase shift film 208 can be effectively inspected using DUV inspection light. When the phase shift film 208 is made of RuO, the content of oxygen (O) is preferably 30 at% or less. Specifically, the phase shift film 208 contains 70 to 99 at% ruthenium (Ru) and 1 to 30 at% oxygen (O).

[0051] The phase shift film 208 may further contain nitrogen (N) and oxygen (O). When both nitrogen (N) and oxygen (O) are contained, the above-mentioned effects of containing nitrogen (N) and oxygen (O) can be obtained by adjusting the content ratio. When the phase shift film 208 is made of RuON, the contents of nitrogen (N) and oxygen (O) are preferably 30 at% or less each. Specifically, the phase shift film 208 contains 40 to 98 at% ruthenium (Ru), 1 to 30 at% nitrogen (N), and 1 to 30 at% oxygen (O).

[0052] The phase shift film 208 has a thickness of 25 to 40 nm.

[0053] The relative reflectance of the entire phase shifting films 207, 208 is 6 to 15% for exposure light with a wavelength of 13.5 nm. Here, the relative reflectance means the ratio of the reflectance of the entire phase shifting films 207, 208 to the reflectance of the laminated structure of the reflective film 204 and the capping film 205. The entire phase shifting films 207, 208 have a phase shift amount of 180 to 220°, preferably 185 to 220°.

[0054] The hard mask layer 209 is used as an etching mask when etching the phase shift layer 208 . For this reason, the hard mask layer 209 is made of a material having an etching selectivity with respect to the phase shift layer 208 .

[0055] When the hard mask film 209 is composed of a single layer, the hard mask film 209 may contain tantalum (Ta) and oxygen (O). When the hard mask film 209 containing tantalum (Ta) further contains oxygen (O), it is etched by a fluorine (F)-based etching gas, and when it does not contain oxygen (O), it is etched by a chlorine (Cl2)-based etching gas. Therefore, the single-layer hard mask film 209 containing tantalum (Ta) and oxygen (O) is etched by a fluorine (F)-based etching gas.

[0056] The hard mask film 209 may have a two-layer structure as shown in FIG. 2. Specifically, the hard mask film 209 includes a lower layer 209a formed on the phase shift film 208 and an upper layer 209b formed on the lower layer 209a. The lower layer 209a further includes nitrogen (N), and the upper layer 209b further includes oxygen (O). Therefore, the lower layer 209a is etched by a chlorine (Cl2)-based etching gas, and the upper layer 209b is etched by a fluorine (F)-based etching gas. The lower layer 209a includes tantalum (Ta) 70-99 at% and nitrogen (N) 1-30 at% and the upper layer 209b includes tantalum (Ta) 70-99 at% and oxygen (O) 1-30 at%. If the hard mask film 209 were made of a single layer containing tantalum (Ta) and oxygen (O) and was etched with a fluorine (F)-based etching gas, the fluorine (F) gas would damage the phase shift film 208 during the etching process. However, by forming the hard mask film 209 in such a two-layer structure, the upper layer 209b is etched with a fluorine (F)-based gas, and then the lower layer 209a is etched with a chlorine (Cl2)-based gas not containing oxygen (O2), thereby preventing the above-mentioned damage.

[0057] The hard mask film 209 may further contain boron (B). The boron (B) content of the hard mask film 209 is 20 at % or less, preferably 15 at % or less. In this case, the lower layer 207a is made of TaBN, and the upper layer 207b is made of TaBO.

[0058] The hard mask film 209 has a thickness of 5 nm or less, preferably 2 to 4 nm. When the hard mask film 209 has a two-layer structure, the upper layer 209b and the lower layer 209a each preferably have a thickness of 3 nm or less.

[0059] The resist film 210 is made of a chemically amplified resist (CAR). The resist film 210 has a thickness of 40 to 100 nm, and preferably 40 to 80 nm.

[0060] In the blank mask of the present invention, the etch stop layer 207 has a high extinction coefficient (k), so the extinction coefficient (k) of the entire phase shift layer 207, 208 is high. Also, the refractive index (n) of the entire phase shift layer 207, 208 is low, so the required amount of phase shift can be secured even with a small thickness of 40 nm or less. Therefore, the productivity can be increased by lowering DtC, and the precision of the pattern can be improved by increasing NILS.

[0061] The process for manufacturing a photomask using the blank mask having the above-mentioned structure is as follows.

[0062] First, a pattern of the resist film 210 is formed by an e-beam writing and developing process, and then the hard mask film 209 is etched using the resist film pattern as an etching mask. A fluorine (F)-based etching gas is used to etch the hard mask film 209 having a single-layer structure of TaBO. When etching the hard mask film 209 having a two-layer structure of TaBO / TaBN, the upper layer 209b is etched using a fluorine (F)-based etching gas, and then the lower layer 209a is etched using a chlorine (Cl2)-based etching gas that does not contain oxygen (O2).

[0063] The resist film pattern is removed, and the pattern of the hard mask film 209 is used as an etching mask to etch the phase shift film 208. To etch the phase shift film 208, a chlorine (Cl2)-based etching gas containing oxygen (O2) is used.

[0064] The etch stop layer 207 is etched using the pattern of the hard mask layer 209 and the pattern of the phase shift layer 208 as an etching mask. An oxygen (O2)-free chlorine (Cl2)-based etching gas is used to etch the etch stop layer 207. Specifically, the end point of etching the phase shift layer 208 with the oxygen (O2)-containing chlorine (Cl2)-based gas is confirmed using an EPD (End Point Detection) device, and then the etch stop layer 207 is etched using the oxygen (O2)-free chlorine (Cl2)-based gas.

[0065] When the hard mask film 209 is composed of a single layer of TaBO, the hard mask film 209 is etched and removed by a fluorine (F)-based etching gas after the etching of the etching stop film 207. When the hard mask film 209 has an upper layer 209b of TaBO and a lower layer 209a of TaBN, the upper layer 209b is etched and removed by a fluorine (F)-based etching gas, and then the lower layer 209a is etched and removed by a chlorine (Cl2)-based etching gas not containing oxygen (O2). At this time, the etching process of the etching stop film 207 and the removal process of the lower layer 209a of the hard mask film 209 may be performed simultaneously. To achieve this, the removal process of the upper layer 209b of the hard mask film 209 must be performed prior to the etching process of the etching stop film 207.

[0066] 3 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a second embodiment of the present invention. Compared with the first embodiment of FIG. 2, the blank mask of the second embodiment of FIG. 3 is the same in structure except for the etching stop film 207. In the following description and drawings of the embodiment, the same reference numerals are used to designate components corresponding to those of the above-mentioned embodiment for the convenience of illustration and description.

[0067] In the second embodiment, the etch stop layer 207 includes a first layer 207a formed on the capping layer 205, and a second layer 207b formed on the first layer 207a. The first layer 207a further includes nitrogen (N), and the second layer 207b further includes oxygen (O). Thus, the first layer 207a is made of TaSbN, and the second layer 207b is made of TaSbO. The first layer 207a includes 1-30 at % of nitrogen (N), and the second layer 207b includes 1-30 at % of oxygen (O).

[0068] The second layer 207b is etched by a fluorine (F)-based etching gas, and the first layer 207a is etched by a chlorine (Cl2)-based etching gas not containing oxygen (O2). Therefore, according to the configuration of the second embodiment, while the second layer 207b of the etching stop film 207 is being etched, the upper layer 209b of the hard mask film 209 is also etched and removed, and while the first layer 207a of the etching stop film 207 is being etched, the lower layer 209a of the hard mask film 209 is also etched and removed. Therefore, a separate process for removing the hard mask film 209 is not required.

[0069] 4 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a third embodiment of the present invention. Compared with the first embodiment of FIG. 2, the blank mask of the third embodiment of FIG. 4 is different only in the hard mask film 209, and the remaining configuration is the same.

[0070] The hard mask film 209 contains chromium (Cr) and niobium (Nb). Such a hard mask film 209 is etched by a chlorine (Cl2)-based etching gas, and in particular, by a chlorine (Cl2)-based etching gas that does not contain oxygen (O2). The hard mask film 209 is preferably configured to contain Cr:Nb at an at% ratio of 3:7 to 6:4. If the content of Nb is lower than this ratio, the etching speed by a chlorine (Cl2)-based gas that does not contain oxygen (O2) is relatively slow, making it difficult to thin the resist film 210, and if the content of Nb is higher than this ratio, there is a problem that the adhesive strength with the resist film 210 decreases.

[0071] The hard mask film 209 may further include one or more light element substances selected from carbon (C), oxygen (O), and nitrogen (N). In this case, the light element substance preferably has a content of 1 to 30 at%. Specifically, the hard mask film 209 has a composition of Cr 30 to 60 at%, Nb 20 to 40 at%, C 0 to 10 at%, O 0 to 30 at%, and N 0 to 30 at%.

[0072] In the first and second embodiments described above, the hard mask film 209 has a two-layer structure. Such a two-layer structure has a function of reducing damage to the phase shift film 208 caused by fluorine (F)-based etching gas when etching the hard mask film 209 having a single layer structure of TaBO. However, in the hard mask film 209 having such a two-layer structure, when the lower layer 209a is overetched, the lower layer 209a is etched deeper laterally than the upper layer 209b, and the pattern profile of the lower layer 209a and the upper layer 209b becomes poor. Therefore, a problem of reduced CD reproducibility may occur. However, in this embodiment, since the hard mask film 209 is composed of a single layer, such a problem does not occur.

[0073] In addition, according to this embodiment, since chlorine (Cl2)-based gas not containing oxygen (O2) is used when etching the hard mask film 209, damage due to oxygen (O2) does not occur to the underlying phase shift film 208. Furthermore, since the hard mask film 209 is etched and removed together with the etch stop film 207 by chlorine (Cl2)-based gas not containing oxygen (O2), the manufacturing process of the photomask is simplified.

[0074] 5 is a diagram showing a phase shift blank mask for extreme ultraviolet lithography according to a fourth embodiment of the present invention. Compared to the third embodiment of FIG. 4, the blank mask of the fourth embodiment of FIG. 5 is the same in structure as the third embodiment of FIG. 4 except for the etching stop layer 207. The structure of the etching stop layer 207 is the same as that of the second embodiment of FIG. 3.

[0075] In this embodiment, while the first layer 207a of the etch stop layer 207 is being etched, the hard mask layer 209 is also etched and removed.

[0076] The present invention has been described in detail above using the embodiments of the present invention with reference to the drawings, but the embodiments are merely provided for the purpose of illustrating and explaining the present invention, and are not intended to limit the meaning or the scope of the present invention described in the claims. Therefore, a person having ordinary skill in the art of the present invention will understand that various modifications and equivalent other embodiments are possible from the embodiments. Therefore, the true scope of protection of the present invention should be determined by the technical matters of the claims. [Explanation of symbols]

[0077] 102 Substrate 104 Reflective film 105 Capping Membrane 107 Etching stop film 107a 1st layer 107b 2nd layer 108 Phase inversion film 109 Hard mask film 110 Resist film 202 Substrate 204 Reflective film 205 Capping Membrane 207 Etching stop film 207a 1st layer, lower layer 207b 2nd layer, upper layer 208 Phase Inversion Film 209 Hard mask film 209a Lower layer 209b upper layer 210 Resist film

Claims

1. A substrate; A reflective film formed on the substrate; a capping film formed on the reflective film and including ruthenium (Ru); an etch stop layer formed on the capping layer and including tantalum (Ta) and antimony (Sb); a phase shift layer formed on the etching stop layer and including ruthenium (Ru); 1. A blank mask for extreme ultraviolet lithography comprising:

2. 2. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the etching stop layer has a content ratio of tantalum (Ta):antimony (Sb)=3:7 to 7:

3.

3. 2. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the etching stop layer has a higher antimony (Sb) content than a tantalum (Ta) content.

4. 4. The blank mask for extreme ultraviolet lithography according to claim 3, wherein the etching stop layer further contains nitrogen (N) at 1 to 10 at %.

5. The etching stop film is a first layer formed on the capping film and further including nitrogen (N); a second layer formed on the first layer and further containing oxygen (O); 4. The extreme ultraviolet lithography blank mask of claim 3, comprising:

6. The first layer contains 1 to 10 at % nitrogen (N), 6. The blank mask for extreme ultraviolet lithography according to claim 5, wherein the second layer contains 1 to 10 at % of oxygen (O).

7. 4. The blank mask for extreme ultraviolet lithography according to claim 3, wherein the etching stop film has a thickness of 2 to 20 nm.

8. The blank mask for extreme ultraviolet lithography according to any one of claims 1 to 7, characterized in that the phase shift film contains 70 to 99 at % ruthenium (Ru) and 1 to 30 at % of either nitrogen (N) or oxygen (O).

9. The blank mask for extreme ultraviolet lithography according to any one of claims 1 to 7, characterized in that the phase shift film contains 40 to 98 at % ruthenium (Ru), 1 to 30 at % nitrogen (N), and 1 to 30 at % oxygen (O).

10. The phase shifting film further includes a hard mask film formed on the phase shifting film, 8. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the hard mask film contains tantalum (Ta) and oxygen (O).

11. The hard mask film is a lower layer formed on the phase shift film and containing tantalum (Ta) and nitrogen (N); an upper layer formed on the lower layer and including tantalum (Ta) and oxygen (O); 11. The extreme ultraviolet lithography blank mask of claim 10, comprising:

12. the underlayer comprises 70 to 99 at % tantalum (Ta) and 1 to 30 at % nitrogen (N); 12. The blank mask for extreme ultraviolet lithography according to claim 11, wherein the upper layer contains 70 to 99 at % tantalum (Ta) and 1 to 30 at % oxygen (O).

13. The phase shifting film further includes a hard mask film formed on the phase shifting film, 8. The blank mask for extreme ultraviolet lithography according to claim 1, wherein the hard mask film contains chromium (Cr) and niobium (Nb).

14. 14. The blank mask for extreme ultraviolet lithography according to claim 13, wherein the hard mask film contains chromium (Cr):niobium (Nb)=3:7 to 6:

4.

15. A photomask for extreme ultraviolet lithography manufactured using the blank mask according to claim 1.

Citation Information

Patent Citations

  • Reflective mask blank and reflective mask

    JP2019086802A

  • Mask blank, transfer mask and method for manufacturing semiconductor device

    JP2020042208A

  • Half-tone type phase shift blank mask and manufacturing method of the same

    KR1020060117287A

  • Blankmask for Extreme Ultra-Violet Lithography and Photomask using the same

    KR1020160002332A

  • Reflective photomask and reflective photomask blank

    WO2010113700A1

Cited By

  • Blankmask and photomask for extreme ultraviolet lithography including hard mask film containing chromium and niobium

    JP2026082626A

  • Phase inversion blank masks and photomasks for extreme ultraviolet lithography

    JP2026172787A

  • Hard mask thin film, sputtering target material, and film forming method

    WO2026186604A1